Optical temperature sensing near-infrared phosphor and its preparation method and application

By developing an optical temperature sensing near-infrared phosphor that generates 600-1100 nm emitted light under visible light excitation, the luminous intensity ratio of Cr3+, Yb3+, Nd3+ thermal coupling energy levels is solved by solving the complex and extreme environments of traditional thermometers in complex and extreme environments The problem of insufficient sensitivity under the problem of high sensitivity and wide application of non-contact optical temperature measurement is achieved.

CN118879324BActive Publication Date: 2024-12-06INNER MONGOLIA UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411393194.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-06
Estimated Expiration
2044-10-08

AI Technical Summary

Technical Problem

Traditional contact thermometers have low sensitivity during temperature measurement, making it difficult to adapt to the temperature measurement needs in complex and extreme environments, especially in strong acidic, submicron-level ultra-small areas, regional gradient temperature measurement, strong electromagnetic and flammable and explosive environments. Difficult to apply.

Method used

Develop an optical temperature sensing near-infrared phosphor with the general chemical formula Gd2.4-a-b-cLu0.6Ga4-aAlO12: aCr3+, bNd3+, cYb3+, which generates 600-1100 nm of emitted light under visible light excitation, using pomegranate The stone structure realizes high sensitivity temperature sensing through the luminous intensity ratio of Cr3+, Yb3+, Nd3+ thermal coupling energy levels. The preparation method includes high-temperature calcination and grinding, which is suitable for non-contact optical temperature measurement.

Benefits of technology

It realizes high sensitivity optical temperature sensing in the range of 300 K to 500 K, with a wide range of application and is suitable for large-scale industrial production, suitable for temperature detection in ultra-small areas, flammable and explosive and extreme environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879324B_ABST
    Figure CN118879324B_ABST
Patent Text Reader

Abstract

The present invention is applicable to the technical field of luminescent materials, and is an optical temperature sensing near-infrared phosphor and its preparation method and application, wherein the chemical general formula of the near-infrared phosphor is: Gd 2.4‑a‑b‑ c Lu 0.6 Ga 4‑a AlO 12 :aCr 3+ , bNd 3+ , 3+ The method comprises the following steps: (1) weighing; (2) obtaining a mixture; (3) obtaining a sintered body; and (4) obtaining a phosphor with a particle size of 1-5 μm. Beneficial effect: The phosphor disclosed in the present invention generates emission light with a wavelength of 600-1100 nm under visible light excitation, and is highly sensitive to temperature. 3+ , Yb 3+ , Nd 3+ The ratio of the luminous intensity of the thermal coupling energy level as a function of temperature can obtain a highly sensitive optical temperature sensing material in a wide range of 300 K to 500 K. The phosphor preparation method disclosed in the present invention is simple, has high yield, low production cost, stable properties, is easy to store, has a wide range of applications, and can meet the needs of industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of luminescent materials, and more specifically, to an optical temperature sensing near-infrared phosphor and a preparation method and application thereof. Background Art

[0002] As an important basic physical parameter, temperature sensing has a wide range of applications in industry and science. Traditional contact thermometers mainly include liquid thermometers and thermocouples. These thermometers need to have physical contact with the object to be measured during the temperature measurement process, and have low detection sensitivity, which makes it difficult to meet the increasingly complex actual measurement needs, especially for special conditions (such as strong acidity, submicron-level ultra-small area temperature measurement, regional gradient temperature measurement, strong electromagnetic and flammable and explosive extreme environments). In order to meet these new challenges, the development of new non-contact optical temperature measurement technology is imminent.

[0003] Near-infrared materials are one of the current research hotspots, especially they have been widely used in security monitoring, food testing and medical imaging. For example, the patent for a broadband short-wave infrared phosphor and its preparation method and a light-emitting device disclosed in application number CN202211319646.7 is particularly suitable for near-infrared LED (light-emitting diode) applications, and can be used in micro-spectroscopy technology, biomedicine and other fields; the patent for a near-infrared fluorescent material and its preparation method and application disclosed in application number CN202311578874.0 is mainly used in near-infrared LED light sources.

[0004] However, there are no reports on the application of visible light-excited near-infrared emitting phosphors in non-contact optical temperature measurement technology. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an optical temperature sensing near-infrared phosphor and a preparation method and application thereof. The optical temperature sensing near-infrared phosphor provided by the present invention generates emission light with a wavelength of 600-1100 nm under visible light excitation, and is highly sensitive to temperature; the preparation method is simple, the yield is high, the production cost is low, the property is stable and it is easy to store, the application range is wide, and it can meet the needs of industrial large-scale production. It is expected to be used for temperature measurement in ultra-small areas, and temperature detection in harsh and extreme environments such as flammable and explosive environments and acid-base corrosion environments.

[0006] To achieve the above object, the present invention provides the following technical solution: an optical temperature sensing near-infrared phosphor, the chemical formula of which is: Gd 2.4-a-b-c Lu 0.6 Ga 4-a AlO 12 :aCr3+ , bNd 3+ , cYb 3+ , where 0 < a ≤ 2.00, 0 ≤ b ≤ 2.00, 0 ≤ c ≤ 2.00, 0 < b + c, and its crystal structure is garnet structure. The general chemical formula of the garnet structure is A3B5O 12 , The general chemical formula of the near-infrared phosphor of the present invention is the same as it. Therefore, the crystal structure of the near-infrared phosphor disclosed in the present invention is garnet structure.

[0007] Further, the excitation light wavelength range of the near-infrared phosphor is 350 - 1000 nm.

[0008] Further, the emission light wavelength range of the near-infrared phosphor is 600 - 1100 nm.

[0009] On the other hand, the present invention provides the following technical solution: A preparation method of an optical temperature sensing type near-infrared phosphor, which includes the following steps:

[0010] (1) Accurately weigh Gd source compound, Lu source compound, Ga source compound, Al source compound, Cr source compound, Yb source compound and Nd source compound according to the element molar ratio of 2.4 - a - b - c: 0.6: 4 - a: 1: a: b: c, where 0 < a ≤ 2.00, 0 ≤ b ≤ 2.00, 0 ≤ c ≤ 2.00, 0 < b + c;

[0011] (2) Mix and grind the raw materials weighed in step (1) with absolute ethanol充分 to obtain a mixture;

[0012] (3) Place the mixture in step (2) in a high-temperature environment of 1200 - 1600 °C and calcine for 3 - 8 h. The mixture is calcined in a reducing atmosphere to obtain a sintered body;

[0013] (4) Naturally cool the sintered body in step (3), and then grind it充分 with a mortar to obtain a phosphor with a particle size of 1 - 5 um.

[0014] Further, the Gd source compound, Lu source compound, Ga source compound, Al source compound, Cr source compound, Yb source compound and Nd source compound in step (1) are one of their corresponding oxides, halides, nitrates.

[0015] Further, the amount of the absolute ethanol in step (2) is 0% - 100% of the total weight of the raw materials.

[0016] Further, the heating rate in step (3) is 3 °C / min.

[0017] Furthermore, the reducing atmosphere in step (3) is a mixture of hydrogen and nitrogen, and the volume ratio of hydrogen to nitrogen is 5-10:95-90; the flow rate of the reducing atmosphere is 10-100 mL / min.

[0018] Another aspect of the present invention provides the following technical solution: an application of an optical temperature sensing near-infrared phosphor, which is applied to temperature indication in the optical field.

[0019] Furthermore, the temperature indication ranges from 300K to 500K.

[0020] The advantages of the present invention are:

[0021] 1. The phosphor disclosed in the present invention generates emission light with a wavelength of 600-1100 nm under visible light excitation, and is highly sensitive to temperature. 3+ , Yb 3+ , Nd 3+ The luminescence intensity ratio of the thermally coupled energy levels as a function of temperature can obtain a highly sensitive optical temperature sensing material in a wide range of 300 K to 500 K.

[0022] 2. The phosphor preparation method disclosed in the present invention is simple, has high yield, low production cost, stable properties and is easy to store. It has a wide range of applications and can meet the needs of industrial large-scale production. It is expected to be used for temperature measurement in ultra-small areas, and temperature detection in harsh and extreme environments such as flammable and explosive environments and acid-base corrosion environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the near infrared spectrum of the phosphor of Example 1 of the present invention.

[0024] Figure 2 This is the near infrared spectrum of the phosphor of Example 8 of the present invention.

[0025] Figure 3 The X-ray diffraction patterns of the phosphors of Examples 1-14 and Comparative Example 2 of the present invention are shown.

[0026] Figure 4 1 and 2 are the excitation spectra of the phosphors of Examples 1 and 8 and Comparative Examples 1 and 2 of the present invention.

[0027] Figure 5 The luminescence spectrum of the phosphor prepared in Example 1 of the present invention when the temperature is uniformly increased from 300K to 500K under 450nm visible light excitation.

[0028] Figure 6 This is the luminescence spectrum of the phosphor prepared in Example 8 of the present invention when the temperature is uniformly increased from 300K to 500K under 450nm visible light excitation.

[0029] Figure 7 The absolute sensitivity and relative sensitivity of the phosphors prepared in Examples 1-7 are respectively related to temperature.

[0030] Figure 8 The absolute sensitivity and relative sensitivity of the phosphors prepared in Examples 8-13 are respectively related to temperature.

[0031] Fig. 9 This is a luminous model captured by the visible light camera and near infrared camera of the present invention. DETAILED DESCRIPTION

[0032] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0033] It should be noted that, unless otherwise specified, all technical and scientific terms used in this application have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs.

[0034] In the present invention, unless otherwise specified, the directions used, such as "up" and "down", usually refer to the directions shown in the drawings, or to the vertical, perpendicular or gravity directions; similarly, for ease of understanding and description, "left" and "right" usually refer to the left and right shown in the drawings; "inside" and "outside" refer to the inside and outside relative to the outline of each component itself, but the above-mentioned directions are not used to limit the present invention.

[0035] Example 1: 0.8700 g of gadolinium oxide (99.999%), 0.1790 g of lutetium oxide (99.999%), 0.7498 g of gallium oxide (99.999%), 0.1020 g of aluminum oxide (99.99%), 0.0395 g of chromium oxide (99.999%) and 0.0591 g of ytterbium oxide (99.99%) were placed in an agate mortar, 5 ml of anhydrous ethanol was added, and the mixture was mixed and ground for 30 minutes. The ground mixture is then transferred to an alumina crucible, which is then placed in a tube furnace, and a reducing atmosphere (5% H2+95% N2) is introduced at a flow rate of 10-100 mL / min. The tube furnace then begins to heat from room temperature to 1200-1600°C at a rate of 3°C / min, and the mixture is sintered at this temperature for 3-8 hours. The heating is then stopped and the mixture is naturally cooled to room temperature. Finally, the sintered body is fully ground in an agate mortar into a phosphor powder with a particle size of 1-5 um. The chemical formula of the phosphor is: Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ , 15% Yb 3 +The optical properties of the phosphor prepared in this example were tested, and the obtained near-infrared spectrum was as follows: Figure 1 As shown, the material of this example has broadband emission in the range of 650-1050 nm under the excitation of 450 nm visible light.

[0036] Example 2: The overall content is the same as Example 1, except that 0.8700 g of gadolinium oxide (99.999%), 0.1591 g of lutetium oxide (99.999%), 0.7498 g of gallium oxide (99.999%), 0.1020 g of aluminum oxide (99.99%), 0.0395 g of chromium oxide (99.999%) and 0.0788 g of ytterbium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 20%Yb 3+ .

[0037] Example 3: The overall content is the same as Example 1, except that 0.8700g of gadolinium oxide (99.999%), 0.1990g of lutetium oxide (99.999%), 0.7498g of gallium oxide (99.999%), 0.1020g of aluminum oxide (99.99%), 0.0395g of chromium oxide (99.999%) and 0.0394g of ytterbium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 10%Yb 3+ .

[0038] Example 4: The overall content is the same as Example 1, except that 0.8700g of gadolinium oxide (99.999%), 0.2109g of lutetium oxide (99.999%), 0.7498g of gallium oxide (99.999%), 0.1020g of aluminum oxide (99.99%), 0.0395g of chromium oxide (99.999%) and 0.0276g of ytterbium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 7%Yb 3+ .

[0039] Example 5: The overall content is the same as Example 1, except that 0.8700g of gadolinium oxide (99.999%), 0.2189g of lutetium oxide (99.999%), 0.7498g of gallium oxide (99.999%), 0.1020g of aluminum oxide (99.99%), 0.0395g of chromium oxide (99.999%) and 0.0197g of ytterbium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 5%Yb 3+ .

[0040] Example 6: The overall content is the same as Example 1, except that 0.8700g of gadolinium oxide (99.999%), 0.2268g of lutetium oxide (99.999%), 0.7498g of gallium oxide (99.999%), 0.1020g of aluminum oxide (99.99%), 0.0395g of chromium oxide (99.999%) and 0.01182g of ytterbium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 3%Yb 3+ .

[0041] Example 7: The overall content is the same as Example 1, except that 0.8700g of gadolinium oxide (99.999%), 0.2348g of lutetium oxide (99.999%), 0.7498g of gallium oxide (99.999%), 0.1020g of aluminum oxide (99.99%), 0.0395g of chromium oxide (99.999%) and 0.0039g of ytterbium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 1%Yb 3+ .

[0042] Example 8: The overall content is the same as Example 1, except that 0.8700 g of gadolinium oxide (99.999%), 0.2268 g of lutetium oxide (99.999%), 0.7498 g of gallium oxide (99.999%), 0.1020 g of aluminum oxide (99.99%), 0.0395 g of chromium oxide (99.999%) and 0.0101 g of neodymium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 3%Nd 3+ The optical properties of the phosphor prepared in this embodiment were tested, and the near-infrared spectrum obtained was as follows: Figure 2 As shown, the material of this example has broadband emission in the range of 650-950 nm under the excitation of 450 nm visible light.

[0043] Example 9: The overall content is the same as Example 1, except that 0.8700 g of gadolinium oxide (99.999%), 0.2348 g of lutetium oxide (99.999%), 0.7498 g of gallium oxide (99.999%), 0.1020 g of aluminum oxide (99.99%), 0.0395 g of chromium oxide (99.999%) and 0.0034 g of neodymium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 1%Nd 3+ .

[0044] Example 10: The overall content is the same as Example 1, except that 0.8700g of gadolinium oxide (99.999%), 0.2308g of lutetium oxide (99.999%), 0.7498g of gallium oxide (99.999%), 0.1020g of aluminum oxide (99.99%), 0.0395g of chromium oxide (99.999%) and 0.0067g of neodymium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 2%Nd 3+ .

[0045] Example 11: The overall content is the same as Example 1, except that 0.8700g of gadolinium oxide (99.999%), 0.2228g of lutetium oxide (99.999%), 0.7498g of gallium oxide (99.999%), 0.1020g of aluminum oxide (99.99%), 0.0395g of chromium oxide (99.999%) and 0.0135g of neodymium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 4%Nd 3+.

[0046] Example 12: The overall content is the same as Example 1, except that 0.8700g of gadolinium oxide (99.999%), 0.2189g of lutetium oxide (99.999%), 0.7498g of gallium oxide (99.999%), 0.1020g of aluminum oxide (99.99%), 0.0395g of chromium oxide (99.999%) and 0.0168g of neodymium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 5%Nd 3+ .

[0047] Example 13: The overall content is the same as Example 1, except that 0.8700g of gadolinium oxide (99.999%), 0.2149g of lutetium oxide (99.999%), 0.7498g of gallium oxide (99.999%), 0.1020g of aluminum oxide (99.99%), 0.0395g of chromium oxide (99.999%) and 0.0202g of neodymium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 6%Nd 3+ .

[0048] Example 14: The overall content is the same as Example 1, except that 0.8700 g of gadolinium oxide (99.999%), 0.2109 g of lutetium oxide (99.999%), 0.7498 g of gallium oxide (99.999%), 0.1020 g of aluminum oxide (99.99%), 0.0395 g of chromium oxide (99.999%) and 0.0236 g of neodymium oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ , 7%Nd 3+ .

[0049] Comparative Example 1: The overall content is the same as Example 1, except that 0.8700g of gadolinium oxide (99.999%), 0.2388g of lutetium oxide (99.999%), 0.7498g of gallium oxide (99.999%) and 0.1020g of aluminum oxide (99.99%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4Lu 0.6 Ga4AlO 12 .

[0050] Comparative Example 2: The overall content is the same as Example 1, except that 0.8700 g of gadolinium oxide (99.999%), 0.3979 g of lutetium oxide (99.999%), 0.7498 g of gallium oxide (99.999%), 0.1020 g of aluminum oxide (99.99%) and 0.0395 g of chromium oxide (99.999%) are put into an agate mortar; the chemical formula of the phosphor finally obtained is: Gd 2.4 Lu 0.6 Ga4AlO 12 : 1%Cr 3+ .

[0051] Experiment 1:

[0052] The optical temperature sensing near-infrared phosphor materials prepared in Examples 1-14 and Comparative Example 2 were analyzed using an X-ray diffractometer. The results are as follows: Figure 3 As shown in the figure, when Nd 3+ The concentration of Yb varies in the range of 0.00-0.07. 3+ When the concentration of is varied in the range of 0.00-0.20, all diffraction peaks of the samples in the examples can be well indexed to the standard card, and no other impurity peaks are observed, indicating that the samples in Examples 1-14 are successfully synthesized and are pure phases; in addition, the standard cards 071-0701 correspond to Gd3Ga5O 12 The diffraction peaks of Examples 1-14 of the present invention are consistent with the garnet structure, indicating that the crystal structure of the phosphor prepared by Examples 1-14 of the present invention is the garnet structure.

[0053] Experiment 2:

[0054] At a detection wavelength of 750 nm, the excitation spectra of the optical temperature sensing near-infrared phosphor materials prepared in Example 1, Example 8 and Comparative Examples 1-2 of the present invention were tested, and the results were as follows: Figure 4 ,As can be seen from the figure, the excitation band of this material is in the violet light region, and it can be ,well excited around 400nm-450nm.

[0055] Experiment 3:

[0056] The optical temperature sensing near-infrared phosphor materials prepared in Example 1 and Example 8 were placed on a heating table under 450nm visible light excitation, and the temperature was uniformly increased from 300K to 500K. The spectra were collected at several temperature nodes to obtain Figure 5 and Figure 6 ,from Figure 5It can be seen from the figure that the optical temperature sensing near-infrared phosphor material prepared in Example 1 changes its fluorescence intensity with the change of temperature under the excitation of 450nm visible light, which reflects its temperature sensing ability. Figure 6 It can be seen that the optical temperature sensing near-infrared phosphor material prepared in Example 8 can also change its fluorescence intensity as the temperature changes under 450nm visible light excitation, reflecting its temperature sensing ability.

[0057] Experiment 4:

[0058] Example 1-7 Using Cr 3+ and Yb 3+ The emission intensity ratio of the ions is used as a temperature measurement parameter, and the calculation formula is as follows:

[0059]

[0060] The absolute sensitivity (Sa) and relative sensitivity (Sr) are calculated as follows:

[0061]

[0062]

[0063] The results are detailed in Figure 7 , in the range of 303-483K, the S of all synthetic phosphors a When Yb doping is 0.20, the maximum value of Sr is 0.5% / K at 423K.

[0064] Example 8-13: Cr 3+ and Nd 3+ The emission intensity ratio of ions is used as a temperature measurement parameter

[0065]

[0066] The absolute sensitivity (Sa) and relative sensitivity (Sr) are calculated as follows:

[0067]

[0068]

[0069] like Figure 8 As shown, S r increases with increasing temperature, and at 483 K Gd 2.4 Lu 0.6 Ga4AlO 12 : Cr 3+ ,0.03Nd 3+ The maximum value (S r= 0.2% / K). It is worth noting that LIR has high sensitivity in the high temperature range and can achieve high-precision temperature readout.

[0070] Experiment 5:

[0071] 15g of the optical temperature sensing near-infrared phosphor material and Ba2SiO4 material prepared in Example 1 and Example 8 were mixed with 480ml of epoxy resin glue, and an equal amount of pure epoxy resin glue was taken and poured into molds respectively. They were dried at room temperature for 12 hours and then dried at 180°C for 2 hours to obtain 4 bear models (a: pure epoxy resin glue; b: mixture of Ba2SiO4 and epoxy resin glue; c: mixture of phosphor in Example 1 and epoxy resin glue; d: mixture of phosphor in Example 8 and epoxy resin glue). The four models were photographed under different light sources (such as Fig. 9 ): I is a visible light photo under natural light; II is a near-infrared photo under natural light; III is a near-infrared photo under natural light + 450nm laser; IV is a near-infrared photo under light excitation in the dark; V is a near-infrared photo under 450nm laser excitation in the dark; VI is a near-infrared photo under 450nm laser + light excitation in the dark.

[0072] from Fig. 9 It can be seen from II, III, IV, V and VI that the bear models prepared in Examples 1 and 8 emit strong or weak light under the irradiation of a near-infrared camera, natural light, light and 450nm laser excitation, indicating that the samples can also be excited under natural light.

[0073] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. An optical temperature sensing near-infrared phosphor, characterized in that: The chemical formula of the near-infrared phosphor is: Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ , 15% Yb 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,20%Yb 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,10% Yb 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,7%Yb 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1% Cr 3+ ,5%Yb 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,3%Yb 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,1%Yb 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,3%Nd 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,1%Nd 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,2%Nd 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,4%Nd 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,5%Nd 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,6%Nd 3+ ; or Gd 2.4 Lu 0.6 Ga4AlO 12 :1%Cr 3+ ,7%Nd 3+ ; Its crystal structure is garnet structure.

2. The optical temperature sensing near-infrared phosphor according to claim 1, characterized in that: The excitation light wavelength range of the near-infrared phosphor is 350-1000nm.

3. The optical temperature sensing near-infrared phosphor according to claim 1, characterized in that: The emission wavelength of the near-infrared phosphor is in the range of 600-1100 nm.

4. A method for preparing the optical temperature sensing near-infrared phosphor according to any one of claims 1 to 3, characterized in that: It includes the following steps: Solution 1: Put 0.8700g of 99.999% pure gadolinium oxide, 0.1790g of 99.999% pure lutetium oxide, 0.7498g of 99.999% pure gallium oxide, 0.1020g of 99.99% pure aluminum oxide, 0.0395g of 99.999% pure chromium oxide and 0.0591g of 99.99% pure ytterbium oxide into an agate mortar, add 5ml of anhydrous ethanol and grind for 30 minutes; then grind the mixture into a mortar and grind for 30 minutes. The mixture is transferred into an alumina crucible, and then the alumina crucible is placed into a tube furnace, and then a reducing atmosphere of 5% H2+95% N2 is continuously introduced at a flow rate of 10-100 mL / min, and then the tube furnace starts heating from room temperature to 1200-1600°C at a rate of 3°C / min, and the mixture is sintered at this temperature for 3-8 hours, and then the heating is stopped and naturally cooled to room temperature, and finally the obtained sintered body is fully ground into a phosphor powder with a particle size of 1-5 um in an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.1591 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0788 g of ytterbium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.1990 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0394 g of ytterbium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2109 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0276 g of ytterbium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2189 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0197 g of ytterbium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2268 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.01182 g of ytterbium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2348 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0039 g of ytterbium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2268 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0101 g of neodymium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2348 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0034 g of neodymium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2308 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0067 g of neodymium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2228 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0135 g of neodymium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2189 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0168 g of neodymium oxide with a purity of 99.99% are put into an agate mortar; or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2149 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0202 g of neodymium oxide with a purity of 99.99% are put into an agate mortar; Or the overall content is the same as Scheme 1, except that 0.8700 g of gadolinium oxide with a purity of 99.999%, 0.2109 g of lutetium oxide with a purity of 99.999%, 0.7498 g of gallium oxide with a purity of 99.999%, 0.1020 g of aluminum oxide with a purity of 99.99%, 0.0395 g of chromium oxide with a purity of 99.999% and 0.0236 g of neodymium oxide with a purity of 99.99% are put into an agate mortar.

5. An application of the optical temperature sensing near-infrared phosphor according to any one of claims 1 to 3, characterized in that: It is applied to temperature indication in the optical field.

6. The use of an optical temperature sensing near-infrared phosphor according to claim 5, characterized in that: The temperature indication ranges from 300K to 500K.

Citation Information

Patent Citations

  • Broadband short-wave infrared fluorescent powder, preparation method thereof and luminescent device

    CN115558491A

  • Near-infrared fluorescent material as well as preparation method and application thereof

    CN117701280A

  • Near-infrared fluorescent powder, preparation method thereof and light-emitting device for supplementing light to pitaya

    CN113355095A

  • Laser material