Smelting method for increasing metal yield of low-carbon steel converter

By using a combination of low lance position and high bottom blowing flow rate at the end of converter smelting, and adding SiO2-containing substances to promote carbon-oxygen reaction, the problem of controlling the total iron content in slag during low-carbon steel smelting was solved, and the metal yield was improved.

CN118879973APending Publication Date: 2024-11-01ZENITH STEEL GROUP CORP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410913671.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively control the total iron content of converter slag below 12% at the end of low-carbon steel smelting, especially when the carbon content at the end is ≤0.05%, resulting in significant iron loss.

Method used

In the final stage of converter smelting, a combination of low lance position and large bottom blowing flow rate is adopted to improve the dynamic conditions of the molten pool. In the later stage of smelting, SiO2-containing substances are added to increase the FeO activity of the slag and promote the carbon-oxygen reaction. By controlling the slag composition and charging system, the total iron content of the slag is reduced.

Benefits of technology

It has achieved stable control of the total iron content in the converter slag at the end point in low-carbon steel smelting, which is below 12%, and improved the metal yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004934441690000011
    Figure HDA0004934441690000011
  • Figure HDA0004934441690000012
    Figure HDA0004934441690000012
Patent Text Reader

Abstract

The invention relates to a low-carbon steel smelting process, and belongs to a smelting method for improving the metal yield of a low-carbon steel converter, the low-carbon steel smelting process adopts a single slag method for smelting, the steel scrap ratio of the converter is controlled to be 10-20%, the oxygen supply flow is controlled to be 5.0-6.0 Nm < 3 > / (min.t), and the bottom blowing flow is controlled to be 0.02-0.08 Nm < 3 > / (min.t); in the smelting process, through cooperation of the gun position and feeding, the slagging effect is improved; the method comprises the following steps: blowing 70-80% of oxygen, adding silica, controlling the SiO2 content of the slag to be 18-22% so as to improve the activity of FeO in the slag, stably controlling the total iron content of the slag to be within 10% under the condition that the endpoint carbon content of the converter is less than or equal to 0.05%, and improving the metal yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of converter steelmaking, in particular to a smelting method for improving metal recovery rate in a low-carbon steel converter, and belongs to the technical field of metallurgy. Background Art

[0002] Converter steelmaking is an oxidative process to remove impurities. Oxygen is blown from the top of an oxygen lance to oxidize elements such as C, Si, Mn, and P in the molten steel, forming gases or oxides that enter the slag for removal. Along with the removal of impurity elements, a large amount of iron in the molten pool is oxidized and enters the slag, resulting in iron loss. This is especially true when smelting low-carbon steel. Since the carbon content of the molten steel at the end of smelting is lower, the molten steel is more oxidizable and the iron loss is greater. The general practice of reducing the total iron content of the converter slag at the end is mainly to tap high-carbon steel, reduce the iron oxide content of the slag, and reduce iron loss. This article focuses on low-carbon steel smelting, and the steel type with a converter carbon content requirement of ≤0.05% is difficult to reduce the slag oxidizability by tapping high-carbon steel.

[0003] After searching, a patent for a converter slag making method with high efficiency of dephosphorization (CN 110042189A) adopts single slag smelting method, a certain amount of lime and magnesite are added according to the silicon content of molten iron in the early stage of smelting, ferrosilicon and magnesite are added in the middle and late stages of the converter to generate more 2CaO·SiO2 in the slag, and the basicity of the converter slag at the end point is controlled at 3.0-3.5, thereby improving the dephosphorization capacity of the converter slag in the late stage of smelting. The main function of adding ferrosilicon in the middle and late stages of converter smelting is to generate more 2CaO·SiO2 phase and promote the dephosphorization reaction.

[0004] In the later stage of converter smelting, the main reaction in the molten pool is the carbon-oxygen reaction, and its reaction equation is: (FeO) + [C] = [Fe] + CO↑. In order to reduce the total iron content of the slag, it is necessary to promote the decarburization reaction to proceed in the forward direction. Improving the mass transfer of carbon and increasing the activity of slag FeO can promote the reaction to proceed in the forward direction and reduce the FeO content of the slag. CN202310782147.X A smelting method for reducing the consumption of converter steel materials adopts the combination of oxygen supply and feeding. The silicon content of molten iron is calculated and a calcium ferrite dephosphorization agent and a calcium ferrite slag agent containing CaO·SiO2 are added to improve the slag effect, enhance the dephosphorization ability of the slag, and realize converter low-slag smelting. At the same time, the basicity of the converter final slag is controlled at 2.2-2.8, and the terminal carbon is greater than 0.05%, so as to achieve the purpose of increasing the metal recovery rate. It mainly realizes low-slag smelting by improving the dephosphorization ability. At the same time, the high-carbon steelmaking at the end reduces the total iron of the slag, and finally achieves the purpose of increasing the metal recovery rate. Compared with the above, the present invention mainly adds SiO2 during the smelting process to increase the activity of FeO in the slag and promote the carbon-oxygen reaction, thereby reducing the total iron in the slag and achieving a steel carbon content of less than 0.05%, while the total iron in the final slag is difficult to be further controlled below 12% in the prior art.

[0005] For steel grades with a converter final carbon content requirement of ≤0.05%, how to stably control the total iron content of the slag within 12% is a technical problem to be solved by the present invention. Summary of the invention

[0006] The present invention is directed to the present invention in the background technology. The present invention provides a smelting method for improving the metal yield of a low-carbon steel converter. The main technical means of the present invention are: (1) adopting low-lance smelting and increasing bottom blowing flow at the end of converter smelting to improve the kinetic conditions of the molten pool and the mass transfer rate of carbon, thereby promoting the carbon-oxygen reaction; (2) adding silica in the later stage of smelting to increase the SiO2 content of the slag, increase the activity of FeO in the slag, further promote the carbon-oxygen reaction, and finally control the total iron content of the converter final slag of low-carbon steel with C≤0.05% to below 12%.

[0007] The specific method steps and control method parameters are as follows:

[0008] A smelting method for improving the metal recovery rate of a low-carbon steel converter, using a single slag method for smelting, controlling the converter scrap ratio at 10-20%, and controlling the top blowing oxygen flow rate at 5.0-6.0 Nm 3 / (min·t), the bottom blowing argon gas flow rate is controlled at 0.02~0.08Nm 3 / (min·t); The slag reduction effect is improved by the coordination of the gun position and the feeding in the smelting process, specifically:

[0009] When the oxygen supply reaches 15-20% of the total amount, add 60-70% of the total amount of lime at one time, add all the lightly burned dolomite, and add 8-15kg / t of ore to help slag formation; when the oxygen supply reaches 50-70% of the total amount, add the remaining lime in small batches, and add an appropriate amount of ore according to the slag formation effect. When the oxygen supply reaches 70-80% of the total amount, add a certain amount of silica, and then supply oxygen until the end without adding any slag-making materials. The SiO2 content in the final slag of the converter smelting is controlled at 18-22%. According to this method, the total iron content of the converter final slag can be controlled below 12%.

[0010] Further, when the oxygen supply reaches 70-80% of the total amount, a certain amount of silica is added, specifically: when the silicon content of the molten iron is ≤0.2%, 400-500kg of silica is added; when the silicon content of the molten iron is 0.2-0.5%, 300-400kg of silica is added; when the silicon content of the molten iron is greater than 0.5%, the amount of silica added is 200-300kg. The specifications of silica are: SiO2: 90-98.0%, Al2O3: 1.0-3.0%, Fe2O3: 1.0-4.0%, and some inevitable impurities, and the particle size is 20-60mm.

[0011] Furthermore, the oxygen supply system is as follows: from the start of oxygen blowing to 85% of oxygen blowing, the oxygen lance position is controlled at 1.5-2.0m; from 85% of oxygen blowing to the end of blowing, the oxygen lance position is controlled at 1.3-1.5m.

[0012] Furthermore, the bottom blowing system is from the start of oxygen blowing to 85% oxygen blowing, and the bottom blowing flow rate is 0.02-0.05Nm 3 / (min·t); Blow oxygen 85% to lift the gun, bottom blowing flow 0.05~0.08Nm 3 / (min·t).

[0013] Furthermore, the slag composition at the end of converter smelting is CaO: 40-55%, SiO2: 18-22%, MnO: 2-6%, MgO: 6-10%, P2O5: 2-5%, Al2O3: 2-6%, total iron: 5-12%, and some inevitable impurities.

[0014] Furthermore, the carbon content of low carbon steel produced from the converter is ≤0.05%.

[0015] Technical advantages: The main technical advantages of the present invention are that the problem of strong oxidizing property of slag at the end of smelting of low-carbon steel (such as QD08, ZCH6A, etc.) is addressed by improving the kinetic conditions by adopting low-gun position and large bottom blowing flow stirring in the later stage of converter smelting, and at the same time adding SiO2-containing substances to increase the SiO2 content in the slag and the activity of FeO in the slag, thereby promoting the carbon-oxygen reaction and reducing the total iron content in the slag. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The effect of SiO2 content in slag on FeO activity in slag was studied for the present invention.

[0017] Figure 2 This is the relationship between the SiO2 content in the slag and the total iron content in the slag in the study of the present invention. DETAILED DESCRIPTION

[0018] Example 1

[0019] The 120t converter is used to smelt low carbon steel. The raw materials are: 117t molten iron, 1310℃ molten iron temperature, 0.1% silicon in molten iron, and 13t scrap steel.

[0020] The smelting process adopts constant flow operation, and the oxygen supply flow rate is 36000Nm 3 / h. Top blowing oxygen supply system: oxygen supply 0-85%, smelting gun position 1.5-2.0m; oxygen supply 85% to lifting gun, smelting gun position 1.3m. Bottom blowing argon system: oxygen supply 0-85%, bottom blowing flow rate 144Nm 3 / h; oxygen supply 85% ~ lifting gun, bottom blowing flow 360Nm 3 / h.

[0021] Feeding system: 15-20% oxygen supply, 2200kg lime, 1800kg light-burned dolomite, 1000kg ore; 50-70% oxygen supply, lime and ore, specifically: 200kg lime, 55% and 60% oxygen supply, 200kg ore and 300kg ore respectively; 75% oxygen supply, 500kg silica; after blowing 75% oxygen, no slag-making materials are added. The slag composition at the end of converter smelting: CaO: 46%, SiO2: 20.3%, MnO: 4.7%, MgO: 7.5%, P2O5: 3.2%, Al2O3: 2.6%, total iron: 6.5%, and some inevitable impurities.

[0022] Smelting by the above method, the final converter temperature is: 1618℃, the final carbon is: 0.03%, the SiO2 content of the slag is: 20.3%, and the final slag total iron is: 6.5%.

[0023] Example 2

[0024] The 120t converter is used to smelt low carbon steel. The raw materials are: 104t molten iron, 1380℃ molten iron temperature, 0.51% silicon in molten iron, and 26t scrap steel.

[0025] The smelting process adopts constant flow operation, and the oxygen supply flow rate is 42000Nm 3 / h. Oxygen supply system: oxygen supply 0-85%, smelting gun position 1.5-2.0m; oxygen supply 85%-lift gun, smelting gun position 1.4m. Bottom blowing system: oxygen supply 0-85%, bottom blowing flow 320Nm 3 / h; oxygen supply 85% ~ lifting gun, bottom blowing flow 560Nm 3 / h.

[0026] Feeding system: 15-20% oxygen supply, 4000kg lime, 2200kg light-burned dolomite, 1800kg ore; 50-70% oxygen supply, 600kg lime is added at 50%, 55% and 60% oxygen supply, 300kg ore and 500kg ore are added at 55% and 60% oxygen supply; 75% oxygen supply, 280kg silica is added, the composition of silica is SiO2: 95.2%, Al2O3: 2.2%, Fe2O3: 2.3%, particle size: 20-60mm. After blowing 75% oxygen, no slag-making materials are added. The composition of the final slag of converter smelting is: CaO: 51.1%, SiO2: 19.2%, MnO: 3.7%, MgO: 7.8%, P2O5: 2.9%, Al2O3: 2.8%, total iron: 7.2%, and some inevitable impurities.

[0027] Smelting by the above method, the final converter temperature is: 1622℃, the final carbon is: 0.028%, the SiO2 content of the slag is: 19.2%, and the final slag total iron is: 7.2%.

[0028] Comparative Example 1

[0029] 120t converter smelts low carbon steel, raw materials: molten iron 117t, molten iron temperature 1308℃, molten iron silicon 0.12%, scrap steel 13t. The smelting process adopts constant flow operation, and the oxygen flow rate is 36000Nm 3 / h.

[0030] Oxygen supply system: oxygen supply 0-85%, smelting gun position 1.5-2.0m; oxygen supply 85%-lift gun, smelting gun position 1.3m. Bottom blowing system: oxygen supply 0-85%, bottom blowing flow 144Nm 3 / h; oxygen supply 85% ~ lifting gun, bottom blowing flow 360Nm 3 / h.

[0031] Feeding system: supply oxygen 15-20%, add 2200kg lime, add 1800kg light-burned dolomite, add 1000kg ore; supply oxygen 50-70%, add 200kg lime at 50%, 55% and 60% respectively, add 200kg ore and 300kg ore at 55% and 60% respectively; supply oxygen 70% until the gun is lifted, without adding any slag-making materials. The slag composition at the end of converter smelting is CaO: 34.3%, SiO2: 9.8%, MnO: 5.9%, MgO: 8.7%, P2O5: 2.1%, Al2O3: 3.5%, total iron: 22.3%, and some inevitable impurities.

[0032] Smelting by the above method, the final converter temperature is: 1616℃, the final carbon is: 0.031%, the SiO2 content of the slag is: 9.8%, and the final slag total iron is: 22.3%.

[0033] Comparative Example 2

[0034] 120t converter smelts low carbon steel, raw materials: molten iron volume 117.2t, molten iron temperature 1312℃, molten iron silicon 0.12%, scrap steel volume 12.9t. The smelting process adopts constant flow operation, and the oxygen flow rate is 36000Nm 3 / h.

[0035] Oxygen supply system: oxygen supply 0-85%, smelting gun position 1.5-2.0m; oxygen supply 85%-lift gun, smelting gun position 1.3m. Bottom blowing system: oxygen supply 0-85%, bottom blowing flow 144Nm 3 / h; oxygen supply 85% ~ lifting gun, bottom blowing flow 360Nm 3 / h.

[0036] Feeding system: oxygen supply 15-20%, add 2200kg lime, add 1810kg light-burned dolomite, add 1000kg ore; oxygen supply 50-70%, add 200kg lime at 50%, 55% and 60% respectively, add 200kg ore and 300kg ore at 55% and 60% respectively; oxygen supply 75%, add 200kg silica, the composition of silica is SiO2: 95.2%, Al2O3: 1.7%, Fe2O3: 2.6%, particle size: 20-60mm. After blowing 75% oxygen, no slag-making materials are added. The final slag composition of the converter is: CaO: 45.6%, SiO2: 15.3%, MnO: 5.1%, MgO: 8.2%, P2O5: 2.3%, Al2O3: 4.7%, total iron: 13.6%, and some inevitable impurities.

[0037] Smelting by the above method, the final converter temperature is: 1621℃, the final carbon is: 0.033%, the SiO2 content of the slag is: 15.3%, and the final slag total iron is: 13.6%.

[0038] Comparative Example 3

[0039] The 120t converter is used to smelt low carbon steel. The raw materials are: 116.8t of molten iron, 1309℃ of molten iron temperature, 0.15% silicon in molten iron, and 13.3t of scrap steel.

[0040] The smelting process adopts constant flow operation, and the oxygen supply flow rate is 36000Nm 3 / h. Oxygen supply system: oxygen supply 0-85%, smelting gun position 1.5-2.0m; oxygen supply 85%-lift gun, smelting gun position 1.3m. Bottom blowing system: oxygen supply 0-85%, bottom blowing flow 144Nm 3 / h; oxygen supply 85% ~ lifting gun, bottom blowing flow 360Nm 3 / h.

[0041] Charging system: oxygen supply 15-20%, add 2200kg lime, add 1800kg light-burned dolomite, add 1000kg ore; oxygen supply 50-70%, add 200kg lime at 50%, 55% and 60% respectively, add 200kg ore and 300kg ore at 55% and 60% respectively; oxygen supply 75%, add 1500kg calcium silicate, the composition of calcium silicate is SiO2: 45%, CaO: 50%, particle size: 20-60mm, and some inevitable impurities. After blowing 75% oxygen, no slag-making materials are added. The composition of the final converter slag is CaO: 48.3%, SiO2: 20.6%, MnO: 3.9%, MgO: 7.3%, P2O5: 2.1%, Al2O3: 2.1%, total iron: 12.7%, and some inevitable impurities.

[0042] Smelting by the above method, the final converter temperature is: 1620℃, the final carbon is: 0.029%, the SiO2 content of the slag is: 20.6%, and the final slag total iron is: 12.7%.

Claims

1. A smelting method for improving metal yield in a low-carbon steel converter, characterized in that: The single slag method is used for smelting, the scrap ratio of the converter is controlled at 10-20%, and the top blowing oxygen flow rate is controlled at 5.0-6.0Nm 3 / (min·t), the bottom blowing argon gas flow rate is controlled at 0.02~0.08Nm 3 / (min·t); the slag-forming effect is improved by coordinating the gun position and the feeding in the smelting process; silica is added when the oxygen blowing rate is 70-80%, the SiO2 content of the converter slag at the end of smelting is controlled at 18-22%, and the total iron content of the converter final slag is controlled below 12%.

2. The smelting method for improving metal yield in a low carbon steel converter according to claim 1, characterized in that: The smelting process is specifically coordinated through the gun position and the addition of materials as follows: when the oxygen supply reaches 15% to 20% of the total amount, 60% to 70% of the total amount of lime is added at one time, all the lightly burned dolomite is added, and 8 to 15 kg / t of ore is added to help slag; when the oxygen supply reaches 50% to 70% of the total amount, the remaining lime is added in multiple batches; when the oxygen blowing reaches 70% to 80% of the total amount, silica is added; The slag composition at the end of converter smelting is CaO: 40-55%, SiO2: 18-22%, MnO: 2-6%, MgO: 6-10%, P2O5: 2-5%, Al2O3: 2-6%, total iron: 5-12%, and some inevitable impurities.

3. The smelting method for improving metal yield in a low carbon steel converter according to claim 1, characterized in that: The oxygen supply system is that from the start of oxygen blowing to 85% of oxygen blowing, the oxygen lance position is controlled at 1.5-2.0m; from 85% of oxygen blowing to the end of blowing, the oxygen lance position is controlled at 1.3-1.5m.

4. The smelting method for improving metal yield in a low-carbon steel converter according to claim 1, characterized in that: The bottom blowing system is from the start of oxygen blowing to 85% oxygen blowing, and the bottom blowing argon flow rate is 0.02~0.05Nm 3 / (min·t); Blow oxygen 85% to lift the gun, bottom blowing argon flow rate 0.05~0.08Nm 3 / (min·t).

5. The smelting method for improving metal yield in a low-carbon steel converter according to claim 1, characterized in that: The conditions for adding silica are: when the silicon content of molten iron is ≤0.2%, add 400-500kg of silica; when the silicon content of molten iron is 0.2-0.5%, add 300-400kg of silica; when the silicon content of molten iron is >0.5%, add 200-300kg of silica; the mass percentage specifications of silica components are: SiO2: 90-98.0%, Al2O3: 1.0-3.0%, Fe2O3: 1.0-4.0%, and some inevitable impurities.

6. The smelting method for improving metal yield in a low carbon steel converter according to claim 1, characterized in that: The carbon content of low carbon steel out of converter is ≤0.05%.