Method for converting high-chromium molten iron to change components of vanadium slag and improve fluidity of vanadium slag
By using iron alumina containing pellets as slag mixing agent and cooling agent in converter vanadium extraction smelting, the problems of vanadium slag viscosity and high iron volume in high chromium vanadium titanium magnetite smelting are solved, and the flow is achieved Improvement of performance and smelting efficiency.
Patent Information
- Application Number
- CN202410922725.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
During the smelting of high chromium vanadium titanium magnetite, the viscosity of vanadium slag and high iron volume lead to high smelting costs and long cycles, and the use of the existing technology slag mixing agent is not effective enough.
In the converter vanadium extraction smelting, iron alumina-containing pellets are added as slag mixing agent and cooling agent. By adding iron alumina-containing pellets in batches, the components of vanadium slag are adjusted, the melting point and viscosity of vanadium slag are reduced, and the flow is improved sex.
It significantly reduces the melting temperature of vanadium slag, improves the fluidity of vanadium extractor converter, shortens the smelting cycle, reduces costs, and meets the national standard requirements for vanadium slag components.
Smart Images

Figure CN118879974A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and particularly relates to a method for blowing high-chromium molten iron to change the composition of vanadium slag and improve the fluidity of the vanadium slag. Background Art
[0002] The converter vanadium extraction process is a molten iron pretreatment process that oxidizes the vanadium in the molten iron into vanadium slag before it enters the steelmaking process. It is also called pyrometallurgy or semi-steel smelting. During the blowing process, oxygen is blown into the molten iron to oxidize the vanadium in the molten iron. The generated V 2 O 3 Vanadium slag can be obtained by entering the slag phase together with the oxides of other easily oxidizable elements such as Si, Ti, Mn, Cr in the molten iron.
[0003] For chromium-containing vanadium-titanium magnetite with high chromium oxide content, Cr 2 O 3 The mass percentage of [Cr] is about 0.5%. The molten iron obtained by smelting this vanadium-titanium magnetite also has a relatively high chromium content, with the mass percentage of [Cr] in the molten iron exceeding 0.25%. Due to the inherent metallic properties of Cr, during the converter vanadium extraction process, most of the [Cr] in the molten iron will be oxidized together with [V] and enter the vanadium slag, thus making the (Cr) in the vanadium slag 2 O 3 ) mass percentage reaches more than 5%, which increases the melting point and viscosity of the vanadium slag, easily leading to the vanadium slag drying out, resulting in a relatively high content of metallic iron in the vanadium slag, which is generally about 25% of the mass of the vanadium slag.
[0004] In view of the semi-steel smelting of high-chromium vanadium-titanium hot metal, Chinese patent CN116121481A proposes "adding slag conditioning agent to the converter, the slag conditioning agent includes iron oxide balls and river sand", "the river sand includes 61-65% SiO 2 ", iron oxide balls contain 16.5-19% SiO 2 , that is, by increasing the SiO 2 The melting point of vanadium slag is reduced by reducing the content of phase, thereby greatly reducing the viscosity of the slag, and then reducing the content of iron in the slag. However, the technical effect of this patent is limited. Although it has been reduced, the iron content is still almost more than 20% of the mass percentage of vanadium slag.
[0005] Chinese patent CN104694698A adds slag adjusting agent in the process of extracting vanadium and chromium from high-chromium vanadium-chromium molten iron. The amount of slag adjusting agent added is positively correlated with the [V]+[Cr] content in the molten iron. The maximum amount added is 6kg / tFe. The main components of the slag adjusting agent include Al 2 O 3 , MgO and FeO, among which Al 2 O3 0%~30%, MgO5~35%, Al 2 O 3 The total content of vanadium and chromium is controlled between 35% and 60%, and the embodiment of the patent controls the iron content of vanadium-chromium slag to less than 10%. However, the amount of coolant added per ton of iron in the patent is large, the oxygen blowing time is long, and the oxygen supply per ton of iron is large, which not only has a high semi-steel smelting cost, but also a long smelting cycle, which is not conducive to continuous operation. Summary of the invention
[0006] In view of the above technical problems, the present invention provides a method for blowing high-chromium molten iron to change the vanadium slag composition and improve the fluidity of the vanadium slag, which can at least solve one of the technical problems of the vanadium slag from the converter vanadium extraction and smelting of vanadium-containing high-chromium molten iron being thick, poor in fluidity, and large amount of iron, as well as the high cost and long cycle of semi-steel smelting.
[0007] The purpose of the present invention is mainly achieved through the following technical solutions:
[0008] The present invention provides a method for blowing high-chromium molten iron to change the composition of vanadium slag and improve the fluidity of vanadium slag, comprising the following steps:
[0009] Step S1, after desulfurizing and slagging the vanadium-containing high-chromium molten iron, adding alumina-containing iron pellets into the vanadium-containing high-chromium molten iron at a ratio of 0.95-1.05 kg / t molten iron to form pre-molten slag;
[0010] Step S2, adding molten iron with vanadium and high chromium content with slag, or molten iron with vanadium and molten iron with vanadium and high chromium content with slag into a double-blown converter;
[0011] Step S3, after oxygen blowing starts, alumina-containing iron pellets are added in batches at a total charge ratio of 21-40 kg / t, and the addition is completed within 280 seconds after the start of blowing;
[0012] Step S4: After oxygen blowing for 300 to 420 seconds, steel is tapped, and semi-steel smelting is completed.
[0013] Furthermore, in step S1, the aluminum oxide iron pellets have a particle size of 5 to 15 mm, and according to the mass percentage, the aluminum oxide iron pellets have an aluminum oxide content of 5 to 15 mm. 2 O 3 It accounts for 30%, iron oxides account for 70%, and Fe accounts for 75.5% of iron oxides.
[0014] Furthermore, the composition of the pre-melted slag in step S1 is as follows: CaO 30-40%, Al 2 O 3 10.7~16.5%, FeO29.5~34.5%, Fe 2 O 37~10.5%, MgO0.25~1.67%, MnO0.25~1.0%, Na 2 O0.5~2.0%, SiO 2 3.5~6%, TiO 2 1.0~2.67%, V 2 O 3 0.5~2.0%, S2.0~4.33%.
[0015] Furthermore, in step S2, the vanadium-containing pig iron block and the vanadium-containing high-chromium molten iron have the same composition, which is as follows in terms of mass percentage: C 3.9-4.4%, Si 0.14-0.32%, Mn 0.10-0.35%, P 0.10-0.15%, S 0.005-0.030%, Ti 0.05-0.28%, Cr 0.26-0.90%, V 0.30-0.35%, and the remainder is Fe and unavoidable impurities.
[0016] Furthermore, in step S2, the temperature of the charge is controlled within the range of 1205-1305°C.
[0017] Furthermore, in step S3, during the blowing process, from 0 to 180 seconds, the oxygen lance low position is controlled at 0.7 to 0.9 m, and the oxygen flow rate is 1.5 to 2.5 Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.015~0.06Nm 3 / min·t loading amount; at 181~240 seconds, the oxygen lance low position is controlled at 1.2~1.4m, and the oxygen flow rate is 2.5~3.0Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.12~0.3Nm 3 / min·t loading amount; after 241 seconds, the oxygen lance low position is controlled at 0.7-0.8m, and the oxygen flow rate is 2.5-3.0Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.15~0.3Nm 3 / min·t loading amount.
[0018] Furthermore, in step S3, alumina-iron pellets are added in three batches: 3-5 kg / t of alumina-iron pellets are added at 0-120 seconds after the start of blowing, 10-20 kg / t of alumina-iron pellets are added at 121-200 seconds, and 8-15 kg / t of alumina-iron pellets are added at 201-280 seconds.
[0019] Furthermore, in step S4, the semi-steel components are as follows in terms of mass percentage: [C] ≥ 3.2%, [V] < 0.05%, [Cr] 0.05-0.28%, [Mn] 0.02-0.10%, [P] 0.10-0.15%, [S] 0.008-0.030%, the remainder being Fe and unavoidable impurities, and the semi-steel temperature is 1325-1400°C.
[0020] Furthermore, [C] ≥ 3.4%, [V] ≤ 0.030%.
[0021] Furthermore, in step S4, the main components of the vanadium slag at the end of blowing are as follows: FeO18-23%, SiO 2 9~15%, V 2 O 3 9~22%,Al 2 O 3 17~26%, Cr 2 O 3 5.5~23%, MnO3~10%, TiO 2 3~15%, CaO1~5%, CaO / V 2 O 3 ≤0.25, MgO2~6%, Na 2 O<0.3%, S<0.5%; in addition to the main components of vanadium slag, the weight of metallic iron M.Fe carried by vanadium slag is 5~16%.
[0022] Compared with the prior art, the present invention can achieve at least one of the following technical effects:
[0023] (1) The present invention adds alumina-containing iron pellets to the converter vanadium extraction smelting. The alumina-containing iron pellets have a reasonable composition ratio and can serve as both a cooling agent and a slag conditioning agent. One material replaces the currently used iron balls, pellets, ferrosilicon and other materials, which not only makes the process control more concise, but also controls the alumina content of the vanadium slag to be 17-26% at the end of blowing, and the melting temperature of the vanadium slag is 1350° C. on average, with a variation range of 1343-1364° C., so that the melting temperature of the vanadium slag is greatly reduced, and the fluidity of the molten pool of the vanadium extraction converter is increased.
[0024] (2) The alumina-containing iron pellets of the present invention are mainly homemade pellets pressed from waste slag from aluminum production and iron oxide scale from steel rolling mills, which is a waste utilization and has the advantage of low cost.
[0025] (3) The oxygen supply time of the converter vanadium smelting method of the present invention does not exceed 7 minutes, the oxygen blowing time is short, the smelting cycle is short, and continuous operation is facilitated.
[0026] (4) In the final semi-steel of the converter vanadium extraction and smelting method of the present invention, [C]≥3.0%, [V]<0.05%, thus achieving the purpose of vanadium extraction and carbon preservation.
[0027] (5) The converter vanadium smelting method of the present invention, V in vanadium slag 2 O 3 9~22%、SiO 2 <24%、CaO / V 2 O 3 ≤0.25, M.Fe<19%, phosphorus-free, meeting the requirements of national standard YB / T008-2006 on vanadium slag composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference numerals refer to like components throughout the drawings.
[0029] Figure 1 Contains 18% Al 2 O 3 Thermal analysis diagram of vanadium slag;
[0030] Figure 2 Contains 23% Al 2 O 3 Thermal analysis diagram of vanadium slag;
[0031] Figure 3 Contains 6.7% Al 2 O 3 Thermal analysis diagram of vanadium slag;
[0032] Figure 4 Contains 4.5% Al 2 O 3 Thermal analysis diagram of vanadium slag. DETAILED DESCRIPTION
[0033] A method for changing the composition of vanadium slag and improving the fluidity of vanadium slag by blowing high-chromium molten iron is further described in detail below in conjunction with specific examples. These examples are only used for comparison and explanation purposes, and the present invention is not limited to these examples.
[0034] A method for changing the composition of vanadium slag and improving the fluidity of vanadium slag by blowing high-chromium molten iron comprises the following steps:
[0035] Step S1, after desulfurizing and slagging the vanadium-containing high-chromium molten iron, adding alumina-containing iron pellets into the vanadium-containing high-chromium molten iron at a ratio of 0.95-1.05 kg / t molten iron to form pre-molten slag;
[0036] Step S2, adding molten iron with vanadium and high chromium content with slag, or molten iron with vanadium and molten iron with vanadium and high chromium content with slag into a double-blown converter;
[0037] Step S3, after oxygen blowing starts, alumina-containing iron pellets are added in batches at a total charge ratio of 21-40 kg / t, and the addition is completed within 280 seconds after the start of blowing;
[0038] Step S4: After oxygen blowing for 300 to 420 seconds, steel is tapped, and semi-steel smelting is completed.
[0039] Specifically, in step S1, the composition of the vanadium-containing high-chromium molten iron is as follows in terms of mass percentage: C 3.9-4.4%, Si 0.14-0.32%, Mn 0.10-0.35%, P 0.10-0.15%, S 0.005-0.030%, Ti 0.05-0.28%, Cr 0.26-0.90%, V 0.30-0.35%, and the remainder is Fe and unavoidable impurities.
[0040] Alumina-containing iron pellets are homemade pellets, mainly made from waste slag from aluminum production and iron oxide scale from steel rolling mills. The particle size is 5 to 15 mm. According to the mass percentage, the Al content in the alumina-containing iron pellets is 2 O 3 The proportion of aluminum oxide is about 30%, the proportion of iron oxide is about 70%, and the proportion of Fe in iron oxide is about 75.5%. The aluminum oxide iron pellets are used as cooling agents and slag regulators in the vanadium smelting process to replace the currently used iron balls, pellets and ferrosilicon. Specifically, the aluminum oxide iron pellets contain aluminum oxide. 2 O 3 While cooling, the slag is adjusted mainly by changing the composition of the slag, while the iron oxide in the alumina-containing iron pellets mainly plays a role in cooling while adjusting the slag by changing the composition of the slag.
[0041] It should be noted that after desulfurization and slagging of vanadium-containing high-chromium hot metal, the hot metal contains a small amount of hot metal slag, the weight of which is about 1-2 kg / t hot metal. In terms of mass percentage, the main components are CaO55-65%, Al 2 O 3 1.0~3.0%, FeO10~20%, MgO0.5~2.5%, MnO0.5~1.5%, Na 2 O1.0~3.0%, SiO 2 7.0~9.0%,TiO 2 2.0~4.0%, V 2 O 3 According to the ratio of 0.95-1.05kg / t molten iron, for example, 1.0kg / t molten iron, add alumina iron pellets to vanadium-containing high-chromium molten iron to form pre-melted slag, the composition of the pre-melted slag is as follows: CaO 30-40%, Al 2 O 310.7~16.5%, FeO29.5~34.5%, Fe 2 O 3 7~10.5%, MgO0.25~1.67%, MnO0.25~1.0%, Na 2 O0.5~2.0%, SiO 2 3.5~6%, TiO 2 1.0~2.67%,V 2 O 3 The function of pre-melted slag is to protect the composition and temperature of molten iron, avoid excessive oxidation and large heat loss of molten iron before adding it into converter, and lay a good material foundation for the next step of converter vanadium extraction with suitable slag system, so that vanadium extraction slag can be slaged early and well.
[0042] Specifically, in step S2, the composition of the vanadium-containing pig iron block is the same as that of the above-mentioned vanadium-containing high-chromium molten iron, and the mass percentage is: C3.86-4.36%, Si0.15-0.30%, Mn0.12-0.30%, P0.10-0.13%, S0.006-0.026%, Ti0.04-0.25%, Cr0.25-0.85%, V0.31-0.36%, and the balance is Fe and unavoidable impurities; the temperature of the charge is controlled within the range of 1205-1305°C by the ratio of the vanadium-containing pig iron block and the vanadium-containing high-chromium molten iron.
[0043] Specifically, in step S3, alumina-containing iron pellets are added in batches at a ratio of a total amount of 21-40 kg / t, the loading amount being the total weight of the vanadium-containing pig iron block and the vanadium-containing high-chromium molten iron. The alumina-containing iron pellets are added in three batches. 3-5 kg / t of alumina-containing iron pellets are added at 0-120 seconds after the start of blowing, 10-20 kg / t of alumina-containing iron pellets are added at 121-200 seconds, and 8-15 kg / t of alumina-containing iron pellets are added at 201-280 seconds. Alumina-containing iron pellets are used as cooling agents and slag regulators in the vanadium extraction smelting process. They are added in batches to steadily control the reaction process of slag and molten iron according to the furnace conditions, so that the vanadium extraction reaction proceeds steadily, orderly and efficiently. At the same time, the furnace temperature is controlled to rise slowly so that the semi-steel temperature at the end of blowing is within the range of 1325-1400°C. Therefore, the batch addition of alumina-containing iron pellets is the result of comprehensive consideration of the thermodynamics and kinetics of the slag-iron reaction.
[0044] During the blowing process, from 0 to 180 seconds, the oxygen lance low position is controlled at 0.7 to 0.9 m, and the oxygen flow rate is 1.5 to 2.5 Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.015~0.06Nm 3 / min·t loading amount; at 181~240 seconds, the oxygen lance low position is controlled at 1.2~1.4m, and the oxygen flow rate is 2.5~3.0Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.12~0.3Nm 3 / min·t loading amount; after 241 seconds, the oxygen lance low position is controlled at 0.7-0.8m, and the oxygen flow rate is 2.5-3.0Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.15~0.3Nm 3 / min·t loading amount.
[0045] It should be noted that the existing converter vanadium extraction principle shows that due to the absolute advantage of Fe atomic concentration in molten iron, the main reaction mode is that oxygen first reacts with Fe atoms in molten iron to form FeO, and then FeO reacts with other elements in molten iron, such as Ti, Si, Mn, V, Cr, and C to form the corresponding oxidation product TiO 2 、SiO 2 、MnO、V 2 O 3 Cr 2 O 3 , CO. Thermodynamic data show that different elements have different affinities with oxygen. There is a sequence of element oxidation at the same temperature. Metal oxidation is carried out in the order of Ti, Si, V, Mn, and Cr. The oxygen potential line of C and the oxygen potential line of other metal elements have opposite directions. The two must have an intersection. The temperature corresponding to the intersection is the exchange temperature of the metal and carbon oxidation sequence, that is, the conversion temperature of selective oxidation. Therefore, for the purpose of vanadium extraction and carbon preservation, the temperature of the molten iron in the vanadium extraction reaction process needs to be controlled as much as possible below the carbon-vanadium conversion temperature. The oxidation of Fe, Ti, Si, V, Mn, Cr, and C releases a lot of heat, so it is necessary to add a cooling agent, such as iron pellets containing aluminum oxide, to control the rise in the temperature of the molten iron. The existing converter vanadium extraction process shows that it is appropriate to control the semi-steel smelting temperature below 1400°C.
[0046] In addition, the oxygen element in the alumina-containing iron pellets added as a cooling agent also provides a part of the oxygen source for the oxidation of metal and carbon in the molten iron. This part of oxygen and the converter top-blown oxygen together constitute the amount of oxygen required for the oxidation reaction.
[0047] Specifically, in step S4, the semi-steel composition is as follows according to the mass percentage: [C] ≥ 3.2%, [V] < 0.05%, [Cr] 0.05-0.28%, [Mn] 0.02-0.10%, [P] 0.10-0.15%, [S] 0.008-0.030%, the remainder is Fe and unavoidable impurities, and the semi-steel temperature is 1325-1400° C. In the semi-steel composition of the present invention, [C] ≥ 3.2%, preferably [C] ≥ 3.4%; [V] < 0.05%, preferably [V] ≤ 0.030%, which well achieves the purpose of extracting vanadium and retaining carbon.
[0048] The main components of the vanadium slag at the end of blowing are as follows: FeO18-23%, SiO 2 9~15%, V 2 O 3 9~22%,Al 2 O 3 17~26%, Cr 2 O 3 5.5~23%, MnO3~10%, TiO 2 3~15%, CaO1~5%, CaO / V 2 O 3 ≤0.25, MgO2~6%, Na 2 O<0.3%, S<0.5%; in addition, the weight of metallic iron carried by the vanadium slag besides the main components of the vanadium slag is 4~15% of the total weight of the vanadium slag, that is, M.Fe5~16%.
[0049] It should be noted that research shows that after vanadium extraction, C and V meet the requirements of the above-mentioned semi-steel composition, that is, when the oxidation rate of C is about 20% and the oxidation rate of V is about 90%, the remaining Ti and Si in the semi-steel are traces, that is, the oxidation rates of Ti and Si are close to 100%, the oxidation rate of Mn is about 75%, and the oxidation rate of Cr is about 70%. The oxidation products of these metals TiO 2 、SiO 2 、MnO、V 2 O 3 Cr 2 O 3 and FeO, as well as A1 added during slag adjustment 2 O 3 , and iron oxides together constitute the main components of vanadium slag after vanadium extraction.
[0050] According to the results of industrial tests, after adding alumina-containing iron pellets, the Al content in vanadium slag can be controlled. 2 O 3 When the content of vanadium slag is 17-26%, the melting temperature of vanadium slag is 1350℃ on average, ranging from 1343℃ to 1364℃. 2 O3 The melting temperature of vanadium slag with low vanadium content is 1494℃ on average, ranging from 1431℃ to 1516℃, which indicates that the fluidity of vanadium slag increases after adding alumina. Figure 1 Contains 18% Al 2 O 3 Thermoanalysis diagram of vanadium slag shows that the melting temperature of vanadium slag is 1351℃; Figure 2 Contains 23% Al 2 O 3 The thermal analysis diagram of vanadium slag shows that the melting temperature of vanadium slag is 1345℃; Figure 3 Contains 6.7% Al 2 O 3 The thermal analysis diagram of vanadium slag shows that the melting temperature of vanadium slag is 1500℃; Figure 4 Contains 4.5% Al 2 Thermal analysis diagram of O3 vanadium slag, the melting temperature of vanadium slag is 1512℃.
[0051] The existing silica slag-adjusting process shows that although it can also play a role in reducing the melting temperature and improving fluidity, the effect is limited. At the same time, it also increases the silica content in the vanadium slag, such as more than 25%. The national standard has an upper limit on the silica content in vanadium slag, which cannot exceed 24%. Therefore, the silica slag-adjusting agent cannot meet the national standard requirements for vanadium slag. The amount of existing alumina slag-adjusting agents added is limited, such as adding a maximum of 1.8kg / t of molten iron, which makes the alumina content in the final vanadium slag less than 16.1%, and the melting temperature of the vanadium slag is limited to drop, such as not lower than 1400℃, and there will be no good vanadium extraction effect.
[0052] The present invention reduces the high Cr content by adding alumina-containing iron pellets in the converter vanadium extraction smelting. 2 O 3 The melting temperature of vanadium slag improves the fluidity of vanadium slag. After oxygen blowing smelting for no more than 7 minutes, the semi-steel composition achieves the purpose of extracting vanadium and retaining carbon. Not only is the smelting efficiency high, but also the V in vanadium slag is 2 O 3 9~22%、SiO 2 <24%、CaO / V 2 O 3 ≤0.25, M.Fe<19%, phosphorus-free, meeting the requirements of national standard YB / T008-2006 on vanadium slag composition.
[0053] Example 1
[0054] A method for changing the composition of vanadium slag and improving the fluidity of vanadium slag by blowing high-chromium molten iron:
[0055] Step S1, after desulfurizing and slagging the vanadium-containing high-chromium molten iron, adding alumina-containing iron pellets into the vanadium-containing high-chromium molten iron at a ratio of 1.0 kg / t molten iron to form pre-molten slag;
[0056] The composition of vanadium-containing high-chromium molten iron is as follows by mass percentage: C3.9%, Si0.14%, Mn0.10%, P0.10%, S0.005%, Ti0.05%, Cr0.26%, V0.30%, and the balance is Fe and unavoidable impurities;
[0057] After desulfurization and slagging of vanadium-containing high-chromium hot metal, the hot metal contains a small amount of hot metal slag, the weight of which is about 1kg / t hot metal. In terms of mass percentage, the main components are CaO63%, Al 2 O 3 1.0%, FeO20%, MgO0.5%, MnO0.5%, Na 2 O1.0%, SiO 2 7.0%, TiO 2 2.0%, V 2 O 3 1.0%, S4.0%.
[0058] The particle size of the alumina iron pellets is 5 to 15 mm. According to the mass percentage, the Al content in the alumina iron pellets is 2 O 3 It accounts for 30%, iron oxides account for 70%, and Fe accounts for about 75.5% of iron oxides.
[0059] Add alumina-containing iron pellets to form pre-melted slag, the composition of the pre-melted slag is as follows: CaO40%, Al 2 O 3 10.7%,FeO34.3%,Fe 2 O 3 7%, MgO0.25%, MnO0.25%, Na 2 O0.5%, SiO 2 3.5%, TiO 2 1.0%, V 2 O 3 0.5%, S2.0%.
[0060] Step S2, adding 85 tons of molten iron with slag and vanadium and high chromium into a double-blown converter with a nominal capacity of 80 tons, and the temperature of the molten iron entering the furnace is 1205°C.
[0061] Step S3, after the oxygen supply and blowing start, the alumina-containing iron pellets are added in three batches according to the total amount of 21kg / t charge amount, 255kg is added at 0-120 seconds after the blowing starts, 850kg is added at 121-200s, and 680kg is added at 201-280s; during the blowing process, the oxygen lance low position is controlled at 0.7m at 0-180s, and the oxygen flow rate is 1.5Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.015Nm 3 / min·t loading amount; at 181-240 seconds, the oxygen lance low position is controlled at 1.2m, and the oxygen flow rate is 2.5Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.12Nm 3 / min·t loading amount; after 241 seconds, the oxygen lance low position is controlled at 0.7m, and the oxygen flow rate is 2.5Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.15Nm 3 / min·t loading amount.
[0062] Step S4: After oxygen blowing for 300 seconds, steel is tapped, and semi-steel smelting is completed.
[0063] The semi-steel composition is as follows: [C] 3.2%, [V] 0.02%, [Cr] 0.05%, [Mn] 0.02%, [P] 0.10%, [S] 0.008%, the remainder is Fe and unavoidable impurities, and the semi-steel temperature is 1325°C; the main components of the vanadium slag are as follows: FeO 23%, SiO 2 10%, V 2 O 3 22%, Al 2 O 3 17%, Cr 2 O 3 5.5%, MnO6%, TiO 2 7%, CaO5%, CaO / V 2 O 3 =0.23, MgO4%, Na 2 O0.2%, S0.3%; in addition, the weight of metallic iron carried by the vanadium slag besides the main components of the vanadium slag is 15% of the total weight of the vanadium slag, that is, M.Fe16%.
[0064] Example 2
[0065] A method for changing the composition of vanadium slag and improving the fluidity of vanadium slag by blowing high-chromium molten iron:
[0066] Step S1, after desulfurizing and slagging the vanadium-containing high-chromium molten iron, adding alumina-containing iron pellets into the vanadium-containing high-chromium molten iron at a ratio of 1.0 kg / t molten iron to form pre-molten slag;
[0067] The composition of vanadium-containing high-chromium molten iron is as follows according to mass percentage: C4.4%, Si0.32%, Mn0.35%, P0.15%, S0.030%, Ti0.28%, Cr0.90%, V0.35%, and the balance is Fe and unavoidable impurities;
[0068] After desulfurization and slagging of vanadium-containing high-chromium hot metal, the hot metal contains a small amount of hot metal slag, the weight of which is about 2kg / t hot metal. In terms of mass percentage, the main components are CaO55%, Al 2 O 3 3.0%, FeO12.5%, MgO2.5%, MnO1.5%, Na 2 O3.0%, SiO 2 9.0%, TiO 2 4.0%, V 2 O 3 3.0%, S6.5%.
[0069] The particle size of the alumina iron pellets is 5 to 15 mm. According to the mass percentage, the Al content in the alumina iron pellets is 2 O 3 It accounts for 30%, iron oxides account for 70%, and Fe accounts for about 75.5% of iron oxides.
[0070] Add alumina-containing iron pellets to form pre-melted slag, the composition of the pre-melted slag is as follows: CaO 30%, Al 2 O 3 14.83%, FeO29.5%, Fe 2 O 3 8%, MgO1.67%, MnO1.0%, Na 2 O2.0%, SiO 2 4%, TiO 2 2.67%, V 2 O 3 2.0%, S4.33%.
[0071] Step S2, adding 80 tons of vanadium-containing high-chromium molten iron with slag and 10 tons of vanadium-containing pig iron blocks into a double-blown converter with a nominal capacity of 80t; the components of the vanadium-containing pig iron blocks are as follows in terms of mass percentage: C4.36%, Si0.30%, Mn0.30%, P0.13%, S0.026%, Ti0.25%, Cr0.85%, V0.36%, and the remainder is Fe and unavoidable impurities; the charging temperature is 1305°C.
[0072] Step S3, after the oxygen supply blowing starts, the alumina-containing iron pellets are added in three batches according to the ratio of the total amount of 40 kg / t of the charging amount, 450 kg is added at 0 to 120 seconds after the blowing starts, 1800 kg is added at 121 to 200 seconds, and 1350 kg is added at 201 to 280 seconds;
[0073] During the blowing process, from 0 to 180 seconds, the oxygen lance low position is controlled at 0.9m, and the oxygen flow rate is 2.5Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.06Nm 3 / min·t loading amount; at 181-240 seconds, the oxygen lance low position is controlled at 1.4m, and the oxygen flow rate is 3.0Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.3Nm 3 / min·t loading amount; after 241 seconds, the oxygen lance low position is controlled at 0.8m, and the oxygen flow rate is 3.0Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.3Nm 3 / min·t loading amount.
[0074] Step S4: After 420s of oxygen blowing, steel is tapped, and semi-steel smelting is completed.
[0075] The semi-steel composition is as follows: [C] 3.9%, [V] 0.030%, [Cr] 0.28%, [Mn] 0.08%, [P] 0.15%, [S] 0.030%, the remainder is Fe and unavoidable impurities, and the semi-steel temperature is 1400°C; the main components of the vanadium slag are as follows: FeO 18%, SiO 2 15%, V 2 O 3 9%,Al 2 O 3 26%,Cr 2 O 3 23%, MnO3%, TiO 2 3%, CaO1%, CaO / V 2 O 3 =0.11, MgO2%; in addition, the weight of metallic iron carried by the vanadium slag in addition to the main components of the vanadium slag is 4% of the total weight of the vanadium slag, that is, M.Fe5%.
[0076] Example 3
[0077] A method for changing the composition of vanadium slag and improving the fluidity of vanadium slag by blowing high-chromium molten iron:
[0078] Step S1, after desulfurizing and slagging the vanadium-containing high-chromium molten iron, adding alumina-containing iron pellets into the vanadium-containing high-chromium molten iron at a ratio of 1.0 kg / t molten iron to form pre-molten slag;
[0079] The composition of vanadium-containing high-chromium molten iron is as follows by mass percentage: C4.2%, Si0.23%, Mn0.25%, P0.125%, S0.016%, Ti0.165%, Cr0.55%, V0.325%, and the balance is Fe and unavoidable impurities;
[0080] After desulfurization and slagging of vanadium-containing high-chromium hot metal, the hot metal contains a small amount of hot metal slag, the weight of which is about 1.5 kg / t hot metal. In terms of mass percentage, the main components are CaO 60%, Al 2 O 3 2.0%, FeO15%, MgO1.5%, MnO1.0%, Na 2 O2.0%, SiO 2 8.0%, TiO 2 3.0%, V 2 O 3 2.0%, S5.5%.
[0081] The particle size of the alumina iron pellets is 5 to 15 mm. According to the mass percentage, the Al content in the alumina iron pellets is 2 O 3 It accounts for 30%, iron oxides account for 70%, and Fe accounts for about 75.5% of iron oxides.
[0082] Add alumina-containing iron pellets to form a pre-melted slag, the composition of the pre-melted slag is as follows: CaO 33.7%, Al 2 O 3 13%, FeO32%, Fe 2 O 3 8.5%, MgO1.0%, MnO0.6%, Na 2 O1.2%, SiO 2 4%, TiO 2 1.8%, V 2 O 3 1.2%, S3.0%.
[0083] Step S2, adding 130 tons of molten iron with slag, vanadium and high chromium into a double-blown converter with a nominal capacity of 120 tons, and the temperature of the molten iron entering the furnace is 1250°C.
[0084] Step S3, after the oxygen supply and blowing start, the alumina-containing iron pellets are added in three batches according to the total amount of 30kg / t, 520kg is added at 0-120 seconds after the blowing starts, 1950kg is added at 121-200 seconds, and 1430kg is added at 201-280 seconds; during the blowing process, the oxygen lance low position is controlled at 0.8m at 0-180 seconds, and the oxygen flow rate is 2.0Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.038Nm3 / min·t loading amount; at 181-240 seconds, the oxygen lance low position is controlled at 1.3m, and the oxygen flow rate is 2.8Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.21Nm 3 / min·t loading amount; after 241 seconds, the oxygen lance low position is controlled at 0.75m, and the oxygen flow rate is 2.8Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.23Nm 3 / min·t loading amount.
[0085] Step S4: After oxygen blowing for 360 seconds, steel is tapped and semi-steel smelting is completed.
[0086] The semi-steel composition is as follows: [C] 3.45%, [V] 0.025%, [Cr] 0.16%, [Mn] 0.06%, [P] 0.125%, [S] 0.018%, the remainder is Fe and unavoidable impurities, and the semi-steel temperature is 1359°C; the main components of the vanadium slag are as follows: FeO 20%, SiO 2 12%, V 2 O 3 15%, Al 2 O 3 22%, Cr 2 O 3 14%, MnO4%, TiO 2 8%, CaO2%, CaO / V 2 O 3 =0.13, MgO3%; in addition, the weight of metallic iron carried by the vanadium slag in addition to the main components of the vanadium slag is 10% of the total weight of the vanadium slag, that is, M.Fe10%.
[0087] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for changing the composition of vanadium slag and improving the fluidity of vanadium slag by blowing high chromium hot metal. It is characterized in that The method comprises the following steps: Step S1, after desulfurizing and slagging the vanadium-containing high-chromium molten iron, adding alumina-containing iron pellets into the vanadium-containing high-chromium molten iron at a ratio of 0.95-1.05 kg / t molten iron to form pre-molten slag; Step S2, adding molten iron with vanadium and high chromium content with slag, or molten iron with vanadium and molten iron with vanadium and high chromium content with slag into a double-blown converter; Step S3, after the oxygen blowing starts, the alumina-containing iron pellets are added in batches according to the total amount of 21-40 kg / t, and the addition is completed within 280 seconds after the blowing starts; Step S4: After oxygen blowing for 300 to 420 seconds, steel is tapped and semi-steel smelting is completed.
2. The method according to claim 1, It is characterized in that In step S1, the alumina-containing iron pellets have a particle size of 5 to 15 mm. According to the mass percentage, the Al content in the alumina-containing iron pellets is 2 O 3 It accounts for 30%, iron oxides account for 70%, and Fe accounts for 75.5% of iron oxides.
3. The method according to claim 1 or 2, It is characterized in that The composition of the pre-melted slag in step S1 is as follows: CaO 30-40%, Al 2 O 3 10.7~16.5%, FeO29.5~34.5%, Fe 2 O 3 7~10.5%, MgO0.25~1.67%, MnO0.25~1.0%, Na 2 O0.5~2.0%, SiO 2 3.5~6%, TiO 2 1.0~2.67%,V 2 O 3 0.5~2.0%, S2.0~4.33%.
4. The method according to claim 1, It is characterized in that In the step S2, the vanadium-containing pig iron block and the vanadium-containing high-chromium molten iron have the same composition, which is as follows in terms of mass percentage: C 3.9-4.4%, Si 0.14-0.32%, Mn 0.10-0.35%, P 0.10-0.15%, S 0.005-0.030%, Ti 0.05-0.28%, Cr 0.26-0.90%, V 0.30-0.35%, and the remainder is Fe and unavoidable impurities.
5. The method according to claim 1, It is characterized in that In step S2, the temperature of the charge is controlled within the range of 1205-1305°C.
6. The method according to claim 1, It is characterized in that In step S3, during the blowing process, the oxygen lance low position is controlled at 0.7-0.9 m and the oxygen flow rate is 1.5-2.5 Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.015~0.06Nm 3 / min·t loading amount; at 181~240 seconds, the oxygen lance low position is controlled at 1.2~1.4m, and the oxygen flow rate is 2.5~3.0Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.12~0.3Nm 3 / min·t loading amount; after 241 seconds, the oxygen lance low position is controlled at 0.7-0.8m, and the oxygen flow rate is 2.5-3.0Nm 3 / min·t loading amount, bottom blowing nitrogen flow rate 0.15~0.3Nm 3 / min·t loading amount.
7. The method according to claim 1, It is characterized in that In the step S3, the alumina-iron pellets are added in three batches. 3-5 kg / t of the alumina-iron pellets are added at 0-120 seconds after the start of blowing, 10-20 kg / t of the alumina-iron pellets are added at 121-200 seconds, and 8-15 kg / t of the alumina-iron pellets are added at 201-280 seconds.
8. The method according to claim 1, It is characterized in that In step S4, the semi-steel components are as follows in terms of mass percentage: [C] ≥ 3.2%, [V] < 0.05%, [Cr] 0.05-0.28%, [Mn] 0.02-0.10%, [P] 0.10-0.15%, [S] 0.008-0.030%, and the remainder is Fe and unavoidable impurities. The semi-steel temperature is 1325-1400°C.
9. The method according to claim 8, It is characterized in that The [C]≥3.4%, and the [V]≤0.030%.
10. The method according to claim 1, It is characterized in that In step S4, the main components of the vanadium slag at the end of blowing are as follows: FeO 18-23%, SiO 2 9~15%, V 2 O 3 9~22%,Al 2 O 3 17~26%, Cr 2 O 3 5.5~23%, MnO3~10%, TiO 2 3~15%, CaO1~5%, CaO / V 2 O 3 ≤0.25, MgO2~6%, Na 2 O<0.3%, S<0.5%; in addition to the main components of vanadium slag, the weight of metallic iron M.Fe carried by vanadium slag is 5~16%.