Aluminum alloy and preparation method and application thereof

By adjusting the content of Ce, La, Sr, and B, changing the structural morphology of the aluminum alloy, and refining the needle-shaped β-ferrous phase and fibrous eutectic silicon, the problem of insufficient thermal conductivity of the aluminum alloy is solved and the aluminum alloy is improved Mechanical and thermal conductivity, suitable for automotive central control display base parts.

CN118880129APending Publication Date: 2024-11-01CHENGDU HUITENG CHUANGZHI INFORMATION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410973369.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The thermal conductivity of the existing aluminum alloy material ADC12 is insufficient, resulting in the temperature of the electronic components in the automotive central control display base increases, the stability of the electronic components decreases, and the probability of failure increases, affecting the safe use of the automobile.

Method used

By adjusting the combined content of Ce, La, Sr, and B, the metallographic morphology of the structure in the aluminum alloy is changed, and the refined needle-shaped β-ferrous phase and fibrous eutectic silicon are generated, the secondary dendrites are controlled, and the aluminum alloy is enhanced. mechanical properties and thermal conductivity.

Benefits of technology

The thermal conductivity and mechanical properties of aluminum alloy are significantly improved, the tensile strength, yield strength and elongation are improved, and the thermal conductivity reaches 180-210W/m·K, meeting the heat dissipation and strength requirements of the base parts of the automotive central control display screen.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880129A_ABST
    Figure CN118880129A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum alloy as well as a preparation method and application thereof, and the aluminum alloy comprises the following components in percentage by mass: 7.0-9.5% of Si, less than or equal to 0.5% of Ce, less than or equal to 0.2% of B, less than or equal to 0.5% of Mg, 0.6-1.0% of Fe, less than or equal to 0.5% of La and 0.01-0.06% of Sr. The rest elements are impurity elements, the content of a single impurity element is less than 0.03%, and the total amount of the impurity elements is less than 0.15%; and the balance of aluminum. In the aluminum alloy, the length range of the needle-shaped iron phase beta-Al5FeSi is 15-50 microns, and the secondary dendritic crystal spacing range is 10-50 microns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aluminum alloys, and in particular to an aluminum alloy and a preparation method and application thereof. Background Art

[0002] In recent years, the new energy vehicle industry has developed rapidly. As a "large terminal" integrating multiple technologies such as mechanics, electronics, computing, perception, audio-visual, and energy storage, intelligent networked new energy vehicles have become the main direction of the transformation and upgrading of the automobile industry. In new energy vehicle equipment products, the electronic components inside the equipment are usually installed at a high density. The more heat is generated per unit time, the main heat dissipation method of metal is metal conduction heat dissipation, and high thermal conductivity components can better achieve heat transfer; at the same time, it can be considered that under the condition of reasonable arrangement of components, a smooth air flow channel can be formed, and air inlet and outlet holes can be opened in the structure, so that the heat-conducting metal and air convection exchange can be fully utilized to reduce the ambient temperature of equipment components, achieve efficient operation of the equipment, ensure the stability and service life of the equipment, and improve control accuracy.

[0003] In the prior art, the center console display screen base of the car is made of traditional die-cast aluminum alloy material ADC12. According to the JIS H5302 standard indicators: ADC12 mechanical properties: tensile strength 213MPa, yield strength 131MPa, elongation 1.7%; thermal expansion coefficient: 23μm / (m·℃); density 2.70-2.75g / cm 3 ; Used for die-casting parts, the thermal conductivity of this grade of material is 96W / mK. This die-cast aluminum alloy material has disadvantages: due to the increasing requirements of existing technologies for automobile central control systems, the functions of automobile central control systems are also increasing, which leads to increased energy consumption of the central control system, especially the central control display screen. When it is in working state, the working environment temperature of the electronic components in the base of the central control display screen will gradually increase, resulting in decreased stability of the electronic components inside, increased power consumption of the central control system control, increased probability of failure, and shortened life of electronic components, which ultimately leads to excessive heating of the automobile central console, prone to abnormal control, and affects the safe use of the car. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide an aluminum alloy and a preparation method and application thereof, so as to solve the problem of insufficient thermal conductivity of the die-cast aluminum alloy material ADC12 in the prior art.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] An aluminum alloy, calculated by mass percentage, comprises the following components:

[0007] Si is 7.0-9.5%, Ce≤0.5%, B≤0.2%, Mg≤0.5%, Fe is 0.6-1.0%, La≤0.5%, Sr is 0.01-0.06%; the remaining elements are all impurity elements, and the content of a single impurity element is less than 0.03%, and the total amount of the impurity elements is less than 0.15%; the balance is aluminum;

[0008] In the aluminum alloy, the length of the needle-shaped iron phase β-Al5FeSi ranges from 15 to 50 μm, and the distance between secondary dendrites ranges from 10 to 50 μm.

[0009] Preferably, the aluminum alloy comprises the following components calculated by mass percentage:

[0010] Si is 7.7-8.7%, Ce is 0.15-0.4%, B≤0.2%, Mg is 0.15-0.35%, Fe is 0.6-0.8%, La is 0.1-0.3%, Sr is 0.015-0.03%; the remaining elements are all impurity elements, and the content of a single impurity element is less than 0.03%, and the total amount of the impurity elements is less than 0.15%; the balance is aluminum.

[0011] Preferably, the aluminum alloy has a linear expansion coefficient of 22.5 μm / (m·°C) in the range of 0 to 60°C.

[0012] Preferably, the density of the aluminum alloy is 2.65-2.75 g / cm 3 .

[0013] Preferably, the thermal conductivity of the aluminum alloy at 25° C. is at least 180 W / m·K; the tensile strength of the aluminum alloy is at least 220 MPa, the yield strength is at least 140 MPa, and the elongation is at least 3%.

[0014] Preferably, the thermal conductivity of the aluminum alloy at 25° C. is 180-210 W / m·K; the tensile strength of the aluminum alloy is 220-290 MPa, the yield strength is 140-220 MPa, and the elongation is 3-12%.

[0015] The present invention provides a method for preparing an aluminum alloy. The specific steps of preparing the aluminum alloy are as follows:

[0016] Step 1: preparing materials so that the proportion of each component meets the requirements of the above-mentioned aluminum alloy; wherein the raw materials include aluminum ingots, industrial silicon, aluminum-cerium alloy, aluminum-boron alloy, magnesium ingots, iron additives, aluminum-lanthanum alloy, and aluminum-strontium alloy;

[0017] Step 2: Place the aluminum ingot in a melting furnace and heat it up to melt to obtain aluminum liquid. The aluminum liquid temperature is controlled at 750-800°C, and then industrial silicon and iron additives are added. After all are melted, the temperature is lowered to 720-750°C, and a refining agent is added to refine the aluminum liquid;

[0018] Step 3: Add aluminum-cerium alloy, aluminum-lanthanum alloy, and magnesium ingot to the aluminum liquid obtained in step 2, and control the temperature at 690-720°C after all are melted, add aluminum-boron alloy and aluminum-strontium alloy, and test their components after all are melted. After the test is qualified, degas the aluminum liquid with high-purity nitrogen or argon, and keep the temperature of the aluminum liquid at 680-710°C;

[0019] Step 4: The aluminum obtained in step 3 is hydraulically pressed into a mold for die casting, and the obtained casting is subjected to aging treatment to obtain the aluminum alloy.

[0020] Preferably, in step 4, before die-casting, the die-casting mold is kept at a temperature of 240-280° C. in advance; and the die-casting is performed at a pressure of 35-65 MPa.

[0021] Preferably, in step 4, the aluminum alloy aging process is: aging temperature 180-360° C., aging time: 2-6 hours.

[0022] The present invention provides an application of an aluminum alloy. The aluminum alloy or the aluminum alloy prepared by the above preparation method is used to prepare a base part of a central control display screen of an automobile.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention changes the microstructure of the high-fluidity aluminum alloy from different directions by adjusting the combined content of Ce, La, Sr, and B; especially in the aluminum alloy system with a high content of Fe, the generation of needle-shaped β-iron phase (β-Al5FeSi) has a very obvious harmful effect on the mechanical properties of the alloy, and the generation of hard and brittle needle-shaped β-iron phase (β-Al5FeSi) will greatly reduce the mechanical properties and thermal conductivity of the present invention; the present invention unexpectedly found that under the combined action of Ce, La, Sr, and B, the microstructure of the high-fluidity aluminum alloy is changed from different directions; especially in the aluminum alloy system with a high content of Fe, the generation of needle-shaped β-iron phase (β-Al5FeSi) has a very obvious harmful effect on the mechanical properties of the alloy, and the generation of hard and brittle needle-shaped β-iron phase (β-Al5FeSi) will greatly reduce the mechanical properties and thermal conductivity of the present invention. The state of the alloy structure phase, combined with alloy elements, causes the coarse needle-shaped β-iron phase (β-Al5FeSi) to branch and break into smaller fragments; reduces the possibility of independent generation of the needle-shaped iron phase; and can be adsorbed on the surface of the needle-shaped iron phase to inhibit its growth, thereby refining the needle-shaped iron phase and shortening the length of the needle-shaped iron phase, and controlling the length of the needle-shaped β-iron phase (β-Al5FeSi) to 15-50μm; reduces the distortion of the alloy structure and the scattering of electrons, thereby enhancing the mechanical properties and thermal conductivity of the alloy.

[0025] 2. The present invention also found that under the action of Ce, La, Sr, and B, the eutectic silicon in the alloy material can be transformed into fibers, and the α-Al can be transformed from dendrites into equiaxed dendrites, and the grain size is significantly reduced. At the same time, the secondary dendrite spacing range of the aluminum alloy material is controlled within 10-50μm, thereby improving the mechanical properties of the alloy material. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is an electron microscope image (100 times) of the aluminum alloy prepared in Example 1. DETAILED DESCRIPTION

[0027] The present invention will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the present invention belong to the scope of protection of the present invention.

[0028] Unless otherwise indicated in specific cases in the present invention, the numerical ranges listed herein include the upper and lower limits, and all integers and fractions within the range, and are not limited to the specific values ​​listed when defining the range.

[0029] 1. Aluminum alloy

[0030] Calculated by mass percentage, the aluminum alloy includes the following components:

[0031] Si is 7.0-9.5%, Ce≤0.5%, B≤0.2%, Mg≤0.5%, Fe is 0.6-1.0%, La≤0.5%, Sr is 0.01-0.06%; the remaining elements are all impurity elements, and the content of a single impurity element is less than 0.03%, and the total amount of the impurity elements is less than 0.15%; the balance is aluminum. In the aluminum alloy, the length of the needle-shaped iron phase β-Al5FeSi ranges from 15 to 50 μm, and the secondary dendrite spacing ranges from 10 to 50 μm.

[0032] The present invention is based on the shortcomings of the traditional die-casting aluminum alloy material ADC12 in the prior art, and conducts in-depth research on aluminum alloy materials. However, improving the mechanical strength and thermal conductivity of aluminum alloys are generally considered to be contradictory goals, because enhancing the strength of the alloy often requires the addition of alloying elements, which may reduce thermal conductivity. Therefore, the present invention considers adjusting the metallographic phase to achieve a smooth improvement of both as much as possible. The present invention finds that during the preparation process of aluminum alloy, the Fe element will inevitably enter the aluminum alloy system, and the Fe element also needs to be added to the aluminum alloy system to improve the mold sticking phenomenon, but the metallographic phase formed by the Fe element has an adverse effect on the mechanical properties and thermal conductivity of the aluminum alloy material. However, if the metallographic morphology formed by the Fe element can be improved, the mechanical properties and thermal conductivity of the aluminum alloy material can be improved simultaneously. The present invention unexpectedly discovered that by adjusting the combined content of Ce, La, Sr, and B, the microstructure morphology of the high-fluidity aluminum alloy is changed from different directions; especially in the aluminum alloy system with a high content of Fe, the needle-shaped β-iron phase (β-Al5FeSi) originally generated in a needle-shaped form has a very obvious harmful effect on the mechanical properties of the alloy, and the formation of a hard and brittle needle-shaped β-iron phase (β-Al5FeSi) will greatly reduce the mechanical properties and thermal conductivity of the aluminum alloy material of the present invention; and the present invention unexpectedly discovered that under the combined action of Ce, La, Sr, and B, the microstructure morphology of the high-fluidity aluminum alloy is changed from different directions; especially in the aluminum alloy system with a high content of Fe, the harmful effect of the needle-shaped β-iron phase (β-Al5FeSi) originally generated in a needle-shaped form on the mechanical properties of the alloy is very obvious, and the formation of a hard and brittle needle-shaped β-iron phase (β-Al5FeSi) will greatly reduce the mechanical properties and thermal conductivity of the aluminum alloy material of the present invention. The state of the alloy structure phase and the combination of alloy elements cause the coarse needle-shaped β-iron phase (β-Al5FeSi) to branch and break into smaller fragments; reducing the possibility of independent generation of the needle-shaped iron phase; and these elements can be adsorbed on the surface of the needle-shaped iron phase to inhibit its growth, thereby refining the needle-shaped iron phase and shortening the length of the needle-shaped iron phase. The length of the needle-shaped β-iron phase (β-Al5FeSi) is controlled within the range of 15-50μm, which can effectively reduce the distortion of the alloy structure and the scattering of electrons, thereby enhancing the mechanical properties and thermal conductivity of the alloy. In the aluminum alloy of the present invention, the length of the needle-shaped iron phase β-Al5FeSi is the length of a single needle-shaped iron phase β-Al5FeSi, and its length range is controlled between 15-50 μm, which can be 15 μm, 20 μm, 25 μm, 35 μm, 45 μm, 48 μm, 49 μm, 50 μm, etc., and all ranges and sub-ranges between the above values; the secondary dendrite spacing is an average value obtained after multiple measurements, and the secondary dendrite spacing range is controlled between 10 and 50 μm, which can be 10 μm, 15 μm, 26 μm, 31 μm, 35 μm, 45 μm, 50 μm, etc., and all ranges and sub-ranges between the above values. It should be understood that in the implementation scheme, any of the above ranges can be combined with any other ranges.

[0033] In some embodiments, the present invention controls the amount of Si element, and controls it between 7.0-9.5%; because although the element Si can improve the fluidity of die-cast aluminum alloy and enhance the strength of the alloy, and reduce the thermal conductivity of the alloy material; but when the Si content is too high, because the solid solubility of Si in the aluminum matrix is ​​as high as 1.65%, the solid solution atoms of Si are strong scattering sources, destroying the periodic potential field of the lattice and hindering the movement of electrons and phonons; in addition, excessive Si elements will form a coarse lath-shaped eutectic Si phase, cut off the transportation channel of electrons and phonons, and reduce the thermal conductivity of the aluminum alloy material; however, when the Si content is too low, the fluidity of the aluminum alloy material is reduced, and the aluminum alloy die-casting is difficult, resulting in the aluminum alloy material not meeting the production requirements. Therefore, the amount of Si element is further preferably 7.7-8.7%, which can be 7.0%, 7.5%, 7.7%, 8.0%, 8.1%, 8.6%, 8.7%, 9.0%, 9.5%, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.

[0034] In some embodiments, the aluminum alloy of the present invention contains Ce element, which can be preferentially adsorbed at the twin concave angle groove of Si phase, "poisoning" the preferred position of Si phase growth, causing its growth rate in certain directions to change, which is mainly reflected in two aspects: on the one hand, it reduces the density of growing twins, inhibiting the rapid growth of twin concave angle groove; on the other hand, it causes a sharp increase in twin density, causing Si to produce twins in more directions. Both results lead to an isotropic growth structure, changing the eutectic Si from coarse needle-like to fine point-like. The α-Al precipitated by the Al-Ce eutectic reaction provides a crystallization core for the nucleation of primary α-Al. The dendrite growth loses spatial conditions due to the dense dendrites, and the coarse dendrites are inhibited, which effectively refines the α-Al grains. The solid solubility of rare earth elements in α-Al is extremely small, so during the solidification process, the Ce element will gather at the front of the solid / liquid interface to cause supercooling of the composition, reduce the secondary dendrite spacing of the alloy, and enhance the mechanical properties of the material; the addition of Ce has an inhibitory effect on the needle-shaped β-Al5FeSi iron phase in the alloy, thereby reducing its splitting of the alloy matrix and improving the mechanical properties. Therefore, the amount of Ce element is preferably 0.14-0.5%, more preferably 0.15-0.4%, which can be 0.14%, 0.15%, 0.25%, 0.35%, 0.4%, 0.45%, 0.46%, 0.50%, etc., as well as all ranges and sub-ranges between the above values. It should be understood that in the implementation scheme, any of the above ranges can be combined with any other ranges.

[0035] In some embodiments, the B element in the aluminum alloy of the present invention. The B element reacts with other impurity elements (Mn, Ti, V, Zr, etc., which will sharply reduce the thermal conductivity of the aluminum alloy material) in the aluminum alloy of the present invention to form a precipitate, which can play a role in precipitation strengthening and impurity removal; at the same time, after adding the B element, compared with the aluminum alloy system without adding the B element, the grains of the aluminum alloy of the present invention become smaller, and the grain boundaries become finer and cleaner, thereby enhancing the mechanical properties of the material. However, when the B content is too high, after the B element content reaches saturation, it will become an impurity, thereby reducing the thermal conductivity and mechanical properties of the material. However, if the amount of B element added is too low, less than 0.03%, it will not be able to play the role of removing impurities, causing the B element to become an impurity element, which has an adverse effect on the thermal conductivity of the aluminum alloy. Therefore, the amount of B element is further preferably 0.03-0.20%, which can be 0.03%, 0.05%, 0.09%, 0.12%, 0.15%, 0.16%, 0.19%, 0.20%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0036] In some embodiments, the aluminum alloy of the present invention contains Mg element, and the room temperature solid solubility of Mg in the aluminum alloy is 0.34%, and the limit solid solubility is 14.9%. Therefore, the Mg element can not only form a Mg2Si precipitation strengthening phase with Si, but also further improve the strength of the alloy through solid solution strengthening. Mg will form a coarse Mg2Si phase during the solidification process of the aluminum alloy, and then completely or partially dissolve into the aluminum matrix during the solid solution treatment of the alloy to form a supersaturated solid solution, and then precipitate a Mg2Si strengthening phase during artificial aging. Since the Fe element will inevitably be brought into the alloy with the smelting tool during the smelting process of the alloy to combine with Si and Al to form a brittle needle-shaped iron-containing phase, which seriously affects the mechanical properties of the alloy. The addition of the Mg element can inhibit the harmful effects of the Fe element. The Mg element can form a skeleton-like π phase (Al8Si6Mg3Fe) with the Fe element, reduce the influence of the needle-shaped β-Fe phase on the performance of the aluminum alloy, and improve the strength of the aluminum alloy. However, the increase in the amount of Mg added will cause the aluminum alloy to oxidize and absorb air. The chemical affinity of magnesium to oxygen is greater than that of aluminum to oxygen. The density of magnesium is less than that of aluminum. It is surface active in aluminum liquid and is enriched on the surface of aluminum liquid. Therefore, excessive Mg will cause it to be preferentially oxidized, resulting in the oxide film on the surface of aluminum liquid being composed entirely of MgO. The vapor pressure of MgO is high and the structure is loose. The oxide film mainly formed by MgO cannot protect the aluminum liquid, which leads to an increase in the tendency of aluminum liquid to absorb air, causing serious slag inclusion in die-cast aluminum alloy materials, and adversely affecting the thermal conductivity and mechanical strength of aluminum alloy materials. Therefore, the amount of Mg element is preferably 0.15-0.5%, more preferably 0.15-0.35%, and can be 0.15%, 0.21%, 0.25%, 0.32%, 0.35%, 0.43%, 0.45%, 0.49%, 0.50%, etc., as well as all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.

[0037] In some embodiments, the aluminum alloy of the present invention is added with Fe element, and Fe is an inevitable element in cast aluminum alloy. Since most of the tools and equipment used in the smelting and casting process are made of iron, Fe is easily brought into the aluminum liquid. Moreover, the Fe content in the alloy will increase every time the recycled materials are remelted. After repeated reuse, the Fe content in the aluminum alloy will gradually increase, and the increase in the Fe element content in metal mold casting and pressure casting will be particularly prominent. In the aluminum alloy of the present invention, the iron phase mainly includes α-iron phase (α-Al8Fe2Si) and needle-shaped β-iron phase (β-Al5FeSi). The α-iron phase structure morphology is mostly Chinese characters or skeletons, etc., and the β-iron phase (β-Al5FeSi) is needle-shaped (three-dimensionally sheet-shaped), wherein the β-iron phase has a very prominent effect on the performance of the aluminum alloy material. When excessive needle-shaped β-iron phase (β-Al5FeSi) is formed in the aluminum alloy, the surface oxide film will lose continuity, thereby improving the die-casting sticking phenomenon. However, this also means that the Fe content in the aluminum alloy is too high. The needle-shaped β-iron phase (β-Al5FeSi) is brittle and hard, which will seriously split the aluminum alloy matrix, causing stress concentration, destroying the connection strength of the aluminum alloy matrix, and greatly reducing the mechanical properties and thermal conductivity of the aluminum alloy material. However, when the needle-shaped β-iron phase (β-Al5FeSi) formed in the aluminum alloy is insufficient, sticking will occur. In order to meet the requirements of the reusable and recyclable use of the aluminum alloy of the present invention and to prevent the die-casting sticking phenomenon, the amount of Fe element is adjusted, and the amount of Fe element is preferably 0.6-0.8%, which can be 0.6%, 0.65%, 0.71%, 0.73%, 0.82%, 0.88%, 0.91%, 0.95%, 0.98%, 1.0%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0038] In some embodiments, La is added to the aluminum alloy of the present invention. La can inhibit the generation of needle-shaped β-iron phase (β-Al5FeSi) in the aluminum alloy, mainly because La is easily adsorbed on the surface of the needle-shaped β-iron phase (β-Al5FeSi), hindering its growth, and has a more obvious inhibitory effect on the needle-shaped β-iron phase (β-Al5FeSi) in the high-iron aluminum-silicon alloy: it can make the coarse needle-shaped β-iron phase (β-Al5FeSi) become fine; it can make the eutectic silicon in the alloy aluminum-silicon alloy have a better metamorphic effect, so that it changes from coarse flakes to fine short needles, and the refinement effect of eutectic silicon is the best; at the same time, it can also refine the α-Al grains in the high-iron aluminum-silicon alloy and reduce its secondary dendrite spacing. However, the amount of La added should not be too much. Too much will form a large number of needle-shaped and plate-shaped LaAlSi intermetallic compounds in the aluminum alloy system of the present invention, thereby causing over-metamorphism, affecting the mechanical properties and thermal conductivity of the aluminum alloy, and reducing the corrosion resistance of the aluminum alloy. Therefore, the amount of La element is preferably 0.1-0.5%, more preferably 0.1-0.3%, and can be 0.1%, 0.15%, 0.16%, 0.21%, 0.24%, 0.30%, 0.33%, 0.35%, 0.46%, 0.50%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0039] In some embodiments, the aluminum alloy of the present invention further adds the Sr element. For the needle-shaped iron phase in the high-iron aluminum-silicon alloy of the present invention, in addition to Ce and La being able to change its length, Sr, as a surface active element, is also easily adsorbed on the growth substrate of the needle-shaped β-iron phase (β-Al5FeSi). When a certain concentration is reached, the growth of the inherent steps on the substrate is prevented. The addition of the Sr element "poisons" the activity of the substrate and destroys the symbiotic nucleation conditions, thereby inhibiting the growth of the needle-shaped β-iron phase (β-Al5FeSi), causing the coarse needle-shaped β-iron phase (β-Al5FeSi) to branch and break into smaller fragments. From a thermodynamic point of view, the formation of phases always tends to the lowest energy state. The needle-shaped β-iron phase (β-Al5FeSi) has a large specific surface area, so its energy state is relatively high. Therefore, as long as the kinetic conditions are met, it will break and transform to a lower energy state. The addition of Sr can reduce the twin boundary energy, thereby increasing the probability of twinning, making the occurrence of twinning behavior easier, and the needle-shaped β-iron phase (β-Al5FeSi) grows in more directions, causing the Fe phase to bend and decompose, and finally the needle-shaped iron phase is continuously refined. In the present invention, the composite modification of Ce, La, and Sr has a synergistic effect on the modification of the needle-shaped iron phase, and the combined effect makes the length of the needle-shaped iron phase shorter, thereby enhancing the electrical conductivity and mechanical properties of the material. In addition, Sr is also an excellent eutectic silicon modifier. The Sr modifier is adsorbed on the growth step of silicon, hindering silicon from growing into a sheet by a step growth mechanism; and the atoms of the modifier are adsorbed on the surface of the silicon phase, causing the stacking order of silicon atoms to change, thereby causing a large number of twins to be generated in the silicon crystal, so the eutectic silicon phase grows by a twin valley mechanism instead. At the same time, the addition of Sr also improves the chemical potential of the a-Al phase in the alloy, and enhances the nucleation and growth ability of the phase during eutectic solidification. Since the growth of eutectic silicon phase is suppressed and the nucleation and growth ability of a-Al phase during eutectic solidification are enhanced, the leading phase of eutectic growth is transformed from the silicon phase before modification to the aluminum phase after modification. After modification, the surrounding eutectic a-Al phase crystals limit the growth of eutectic silicon, so that it can only grow along the axial direction, and finally lead to the production of fibrous silicon. If the Sr content is too little, the modification will be insufficient, and the mechanical properties and thermal conductivity will be reduced; if the Sr content is too much, the hydrogen absorption rate of aluminum liquid will be increased, and the strength and thermal conductivity of the alloy will be reduced. Therefore, the Sr dosage is further preferably 0.015-0.03%, which can be 0.010%, 0.015%, 0.021%, 0.025%, 0.033%, 0.035%, 0.042%, 0.045%, 0.058%, 0.060%, etc., as well as all ranges and sub-ranges between the above values. It should be understood that in the implementation scheme, any of the above ranges can be combined with any other ranges.

[0040] In some embodiments, the aluminum alloy has a linear expansion coefficient of 22.5 μm / (m·°C) in the range of 0 to 60°C.

[0041] In some embodiments, the density of the aluminum alloy is 2.65-2.75 g / cm 3 .

[0042] In some embodiments, the thermal conductivity of the aluminum alloy at 25° C. is 180-210 W / m·K; the tensile strength of the aluminum alloy is 220-290 MPa, the yield strength is 140-220 MPa, and the elongation is 3-12%.

[0043] 2. A method for preparing aluminum alloy

[0044] Step 1: preparing materials so that the proportion of each component meets the requirements of the above-mentioned aluminum alloy; wherein the raw materials include aluminum ingots, industrial silicon, aluminum-cerium alloy, aluminum-boron alloy, magnesium ingots, iron additives, aluminum-lanthanum alloy, and aluminum-strontium alloy;

[0045] Step 2: Place the aluminum ingot in a melting furnace and heat it up to melt to obtain aluminum liquid. The aluminum liquid temperature is controlled at 750-800°C, and then industrial silicon and iron additives are added. After all are melted, the temperature is lowered to 720-750°C, and a refining agent is added to refine the aluminum liquid;

[0046] Step 3: Add aluminum-cerium alloy, aluminum-lanthanum alloy, and magnesium ingot to the aluminum liquid obtained in step 2, and control the temperature at 690-720°C after all are melted, add aluminum-boron alloy and aluminum-strontium alloy, and test their components after all are melted. After the test is qualified, degas the aluminum liquid with high-purity nitrogen or argon, and keep the temperature of the aluminum liquid at 680-710°C;

[0047] Step 4: The aluminum obtained in step 3 is hydraulically pressed into a mold for die casting, and the obtained casting is subjected to aging treatment to obtain the aluminum alloy.

[0048] In some embodiments, in step 4, before die-casting, the die-casting mold is kept at a temperature of 240-280° C. in advance; and the die-casting is performed at a pressure of 35-65 MPa.

[0049] In some embodiments, in step 4, the aluminum alloy aging process is: aging temperature 180-360° C., aging time: 2-6 hours.

[0050] The present invention provides an application of an aluminum alloy. The aluminum alloy or the aluminum alloy prepared by the above preparation method is used to prepare a base part of a central control display screen of an automobile.

[0051] 3. Application of Aluminum Alloy

[0052] The aluminum alloy material of the present invention or the aluminum alloy material prepared by the method of the present invention can be used to prepare the base parts of the central control display screen of an automobile.

[0053] 4. Examples and Comparative Examples

[0054] Table 1 (Unit: wt%)

[0055]

[0056] Example 1

[0057] Step 1: Weigh the raw materials according to the proportion of each element in Table 1. The raw materials include aluminum ingots, industrial silicon, aluminum-cerium alloy, aluminum-boron alloy, magnesium ingot, iron additive, aluminum-lanthanum alloy, and aluminum-strontium alloy;

[0058] Step 2: Place the aluminum ingot in a melting furnace and heat it up to melt to obtain aluminum liquid. The aluminum liquid temperature is controlled at 750-800°C, and then industrial silicon and iron additives are added. After all are melted, the temperature is lowered to 720-750°C, and a refining agent is added to refine the aluminum liquid;

[0059] Step 3: Add aluminum-cerium alloy, aluminum-lanthanum alloy, and magnesium ingot to the aluminum liquid obtained in step 2, and control the temperature at 690-720°C after all are melted, add aluminum-boron alloy and aluminum-strontium alloy, and test their components after all are melted, and degas the aluminum liquid after passing the test, and keep the aluminum liquid temperature at 680-710°C;

[0060] Step 4: hydraulically press the aluminum obtained in step 3 into a mold for die casting, and perform aging treatment on the die-cast parts of the central control screen display base of the new energy vehicle to obtain the aluminum alloy; in step 4, before die casting, the die casting mold is pre-maintained at a temperature of 240-280° C.; during die casting, the aluminum liquid is cast at a pressure of 30-65 MPa;

[0061] Step 5: The aging treatment process of the parts is: aging temperature: 180-360℃; aging insulation time: 2-6 hours.

[0062] The embodiments and comparative examples adopt the component ratios in Table 1, and both adopt the preparation method of Example 1 to prepare the central control display base parts of new energy vehicles, and sample the part bodies, perform tensile tests and thermal conductivity tests, metallographic preparation and metallographic tests.

[0063] Determine the mechanical properties according to GB / T 228.1 Metallic materials tensile test Part 1: Room temperature test method;

[0064] Thermal conductivity was tested according to ASTM-E1461 Standard Test Method for Determination of Fixed Thermal Conductivity by Flash Method;

[0065] According to GB / T 13298 metal microstructure inspection method, the length of needle-shaped β-Al5FeSi was measured;

[0066] The secondary dendrite spacing of the alloy was determined according to the GB / T 14999.7 high-temperature alloy casting grain size, primary dendrite spacing and microporosity determination method.

[0067] The test mechanical properties parameters, thermal conductivity and metallographic data are shown in Table 2.

[0068] Table 2

[0069]

[0070] Combining Table 1 and Table 2, we can see that:

[0071] (1) The results show that the die-cast aluminum alloy prepared by the element content and composition of the present invention has excellent mechanical properties and thermal conductivity. By adjusting the amount of each element, the embodiment can ensure that the length of the needle-shaped β-iron phase (β-Al5FeSi) in the obtained aluminum alloy is controlled between 15-50μm, and the secondary dendrite spacing range is controlled between 10-50μm. The aluminum alloy with the above metallographic phase not only maintains excellent mechanical properties, but also has significantly improved thermal conductivity, with tensile strength reaching 220-290MPa, yield strength reaching 140-220MPa, and elongation reaching 3-12%; the thermal conductivity is increased to 180-210W / m·K. Compared with the traditional aluminum alloy material ADC12 material, not only the tensile strength, yield strength and elongation are improved, but also the thermal conductivity is greatly improved. It can well replace the traditional aluminum alloy material and be used for the preparation of the base parts of the automobile central control display screen, and can well meet the requirements of the base parts of the automobile central control display screen for strength and heat dissipation. In the comparative example, since the amount of each component element was not adjusted, the length of the needle-shaped β-iron phase (β-Al5FeSi) and the secondary dendrite spacing in the obtained aluminum alloy were not effectively controlled, which made it difficult to simultaneously improve the mechanical properties and thermal conductivity of the aluminum alloy obtained in the comparative example.

[0072] (2) Compared with Example 1, in Comparative Example 1, the Si element exceeds the required range of the element, and the amount of Si element increases, which increases the consumption of the metamorphic and refining elements Sr, Ce, La, and B, thereby causing the eutectic silicon and primary silicon structures to become coarser, and further causing the secondary dendrite spacing to become larger, the β-iron phase needle length to become longer, and ultimately the plastic toughness of the aluminum alloy material to decrease, the brittleness to increase, and the thermal conductivity of the alloy to decrease.

[0073] (3) Compared with Example 2, in Comparative Example 2, the Ce element exceeds the set range of the element, and the Ce element is increased. After the excessive Ce is added, the size of the needle-shaped β-iron phase (β-Al5FeSi) increases instead, and a large number of needle-shaped, short-sheet and plate-shaped (AlSiCe) intermetallic compounds appear in the α-Al matrix. The reason for the increase in the size of the needle-shaped iron phase is that the excessive Ce forms needle-shaped compounds with Al, Si, and Fe, resulting in over-deformation and reducing the mechanical properties of the material. These (AlSiCe) intermetallic compounds can cause lattice distortion and grain boundary defects, and reduce the thermal conductivity of the aluminum alloy.

[0074] (4) Compared with Example 3, in Comparative Example 3, the B element exceeds the set range of the element, the B element content is too high, the excess B element and the metamorphic element Sr are poisoned, and Sr further poisons each other with B, consuming a certain amount of Sr and B, reducing the effective Sr and B in the melt, resulting in a decrease in the amount of effective Sr in the melt, a decrease in the supercooling of the eutectic, and an increase in the twin interface energy, which reduces the probability of inducing twins, resulting in thickening of the silicon fibers; thereby reducing the mechanical properties and thermal conductivity of the material; and increasing the grain size of the alloy.

[0075] (5) Compared with Example 4, in Comparative Example 4, the Mg element exceeds the set range of the element, and the Mg element content is too high. According to the free electron thermal conductivity mechanism of the metal, the thermal conductivity of the aluminum alloy is related to factors such as the degree of lattice distortion, defects, impurities, phase composition and distribution in the structure. Excessive Mg element increases the solid solubility, the number of intercrystalline second phases increases, and the degree of lattice distortion increases; at the same time, it can be seen from metallographic observation that the grains are refined, the grain boundaries increase, and the grain boundaries, as a surface defect, have a strong hindering effect on the movement of free electrons, which will reduce the energy transmission efficiency and thermal conductivity. The increase in Mg content makes aluminum alloys prone to oxidation and air absorption. The chemical affinity of magnesium to oxygen is greater than that of aluminum to oxygen, the density of magnesium is less than that of aluminum, and it is surface active in the aluminum liquid, enriched on the surface of the aluminum liquid, and preferentially oxidized. The Mg content in the aluminum liquid is too high, and the oxide film on the aluminum liquid surface is composed entirely of MgO. MgO has a high vapor pressure and a loose structure, and has no protective effect on the aluminum liquid. Therefore, with the increase of Mg content, the air absorption tendency of the aluminum liquid increases, and at the same time, it causes serious slag inclusion in the die-cast aluminum alloy material, reducing the thermal conductivity and strength of the alloy.

[0076] (6) Compared with Example 4, in Comparative Example 5, the Fe content exceeds the standard, and the solid solubility of Fe in the Al matrix at room temperature is only 0.05%. Therefore, most of the Fe elements exist in the form of precipitated phases. As the Fe content exceeds the standard, the average size and number of the Fe-containing phases also increase significantly, and a large number of long needle-shaped β-A15FeSi phases are rapidly formed. This coarse precipitated needle-shaped β-A15FeSi phase will seriously hinder the movement of free electrons, thereby causing a significant increase in the probability of electron scattering and a decrease in the thermal conductivity of the alloy. In addition, as the Fe content increases, the α-Al matrix grain structure is refined, the number of grain boundaries increases, and there is a strong inhibitory effect on the movement of free electrons, which will also reduce the energy transmission efficiency and thermal conductivity; the mechanical properties of the aluminum alloy will decrease sharply. It is mainly harmful to the tensile strength and toughness of the aluminum alloy. At the same time, this phase is a very active pore nucleation substrate, and tiny pores rely on this phase to nucleate, resulting in micro-shrinkage in the interdendritic region. Therefore, the tensile strength and elongation of the alloy will be reduced.

[0077] (7) Compared with Example 5, in Comparative Example 6, the La element exceeds the range. After excessive La is added, a large number of needle-shaped and plate-shaped LaAlSi intermetallic compounds are easily formed in the aluminum alloy, resulting in over-metamorphism, which affects the mechanical properties of the alloy; at the same time, excessive La reduces the corrosion resistance of the alloy.

[0078] (8) Compared with Example 5, in Comparative Example 7, excessive Sr elements cause excessive qualitative changes in the aluminum alloy material. The agglomeration and coarsening of the eutectic Si phase weaken the modification effect, resulting in the appearance of Al2Si2Sr compounds. At the same time, the dendrite spacing increases, reducing the mechanical properties. There is also a serious hydrogen absorption phenomenon, the gas content of the organization increases, and the mechanical properties and thermal conductivity of the material are reduced.

[0079] (9) Compared with Example 3, in Comparative Example 8, no Sr, Ce, La, or B elements were added for alloying. The eutectic silicon in the structure grew into flake and block silicon, the α-Al grains in the alloy were coarse, and the secondary dendrite spacing size reached 129 μm; the β-iron phase size was coarse, reaching 187 μm, which seriously split the structure, hindered the movement of electrons and phonons, and reduced the mechanical properties and thermal conductivity of the material.

[0080] The aluminum alloy material of the present invention can replace the traditional aluminum alloy material ADC12 and be applied to the central control screen display base shell parts of new energy vehicles. At the same time, the material of the present invention can also be used in industries with strength and thermal conductivity requirements such as photovoltaics, energy storage, communications, and rail transportation, as well as in scenarios where high thermal conductivity parts are used and replaced.

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.

Claims

1. An aluminum alloy, characterized in that: Calculated by mass percentage, the aluminum alloy includes the following components: Si is 7.0-9.5%, Ce≤0.5%, B≤0.2%, Mg≤0.5%, Fe is 0.6-1.0%, La≤0.5%, Sr is 0.01-0.06%; the remaining elements are all impurity elements, and the content of a single impurity element is less than 0.03%, and the total amount of the impurity elements is less than 0.15%; the balance is aluminum; In the aluminum alloy, the length of the needle-shaped iron phase β-Al5FeSi ranges from 15 to 50 μm, and the distance between secondary dendrites ranges from 10 to 50 μm.

2. The aluminum alloy according to claim 1, characterized in that: Calculated by mass percentage, the aluminum alloy includes the following components: Si is 7.7-8.7%, Ce is 0.15-0.4%, B≤0.2%, Mg is 0.15-0.35%, Fe is 0.6-0.8%, La is 0.1-0.3%, Sr is 0.015-0.03%; the remaining elements are all impurity elements, and the content of a single impurity element is less than 0.03%, and the total amount of the impurity elements is less than 0.15%; the balance is aluminum.

3. The aluminum alloy according to claim 1, characterized in that: The aluminum alloy has a linear expansion coefficient of 22.5 μm / (m·°C) in the range of 0 to 60°C.

4. The aluminum alloy according to claim 1, characterized in that: The density of the aluminum alloy is 2.65-2.75 g / cm 3 .

5. The aluminum alloy according to claim 1, characterized in that: The thermal conductivity of the aluminum alloy at 25° C. is at least 180 W / m·K; the tensile strength of the aluminum alloy is at least 220 MPa, the yield strength is at least 140 MPa, and the elongation is at least 3%.

6. A method for preparing an aluminum alloy, characterized in that: The aluminum alloy according to any one of claims 1 to 5 is prepared by the following specific steps: Step 1: preparing materials, so that the proportion of each component satisfies the aluminum alloy described in any of claims 1 to 5; wherein the raw materials include aluminum ingots, industrial silicon, aluminum-cerium alloy, aluminum-boron alloy, magnesium ingots, iron additives, aluminum-lanthanum alloy, and aluminum-strontium alloy; Step 2: Place the aluminum ingot in a melting furnace and heat it up to melt to obtain aluminum liquid. The aluminum liquid temperature is controlled at 750-800°C, and then industrial silicon and iron additives are added. After all are melted, the temperature is lowered to 720-750°C, and a refining agent is added to refine the aluminum liquid; Step 3: Add aluminum-cerium alloy, aluminum-lanthanum alloy, and magnesium ingot to the aluminum liquid obtained in step 2, and control the temperature at 690-720°C after all are melted, add aluminum-boron alloy and aluminum-strontium alloy, and test their components after all are melted. After the test is qualified, degas the aluminum liquid with high-purity nitrogen or argon, and keep the temperature of the aluminum liquid at 680-710°C; Step 4: The aluminum obtained in step 3 is hydraulically pressed into a mold for die casting, and the obtained casting is subjected to aging treatment to obtain the aluminum alloy.

7. The preparation method according to claim 6, characterized in that: In step 4, before die-casting, the die-casting mold is kept at a temperature of 240-280° C.; and die-casting is performed at a pressure of 35-65 MPa.

8. The preparation method according to claim 6, characterized in that: In step 4, the aluminum alloy aging process is: aging temperature 180-360° C., aging time: 2-6 hours.

9. An application of aluminum alloy, characterized in that: The aluminum alloy described in any one of claims 1 to 5 or the aluminum alloy prepared by the preparation method described in any one of claims 6 to 8 is used to prepare the base parts of the automobile central control display screen.