Fast-spheroidizing high-spheroidizing-rate high-carbon steel and preparation method thereof
By adding Al to high-carbon steel and performing heat treatment under a strong magnetic field, the problems of low spheroidization rate and long spheroidization time of high-carbon steel are solved, the high spheroidization rate and uniform carbide distribution are achieved, and the high-carbon steel is improved. Performance.
Patent Information
- Application Number
- CN202410932752.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-01
AI Technical Summary
The spheroidization rate of existing high-carbon steels is not high, the carbide particles in the tissue are large and unevenly distributed, and the spheroidization period is long, which affects energy consumption and final use performance.
Add 1.15% to 1.61% of Al to high-carbon steel and place it under a steady-state strong magnetic field of 6 to 10T for heat treatment, including austenitization and isothermal treatment, shortening the spheroidization time and improving the spheroidization rate.
The high spheroidization rate (>85%) and fine and uniform carbide distribution of high-carbon steel are achieved, which shortens the spheroidization time and reduces energy consumption.
Smart Images

Figure CN118880174A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel material preparation, and relates to a fast spheroidizing high spheroidizing rate high carbon steel and a preparation method thereof. Background Art
[0002] High carbon steel has the advantages of high strength and hardness, good wear resistance and fatigue resistance, and is widely used in machinery manufacturing, transportation, energy security and other fields. In the preparation process of the above products, the original structure of high carbon steel is generally lamellar pearlite, which has high hardness, high brittleness, easy cracking, and is not convenient for subsequent cutting and processing. It often needs to be spheroidized before use. After spheroidization, a structure with carbide particles distributed on the ferrite matrix can be obtained. The finer, more uniform and more rounded the carbide particles are, the more conducive to the subsequent cutting and processing of high carbon steel. However, the spheroidization rate of ordinary high carbon steel is often not high after spheroidization treatment, the carbide particles in the structure are large, unevenly distributed, and the spheroidization cycle is also long, which has an adverse effect on energy consumption and the final use performance of high carbon steel. Therefore, selecting suitable chemical composition and designing a reasonable spheroidization heat treatment process are key issues that need to be solved in the field of high carbon steel spheroidizing annealing to obtain ideal spheroidized structure, shorten spheroidization treatment time, and improve the use performance of high carbon steel.
[0003] The existing patent technologies for improving the spheroidization rate and improving the structure of high carbon steel mainly focus on optimizing the spheroidizing annealing process or adding chemical components, while there are few patents that have both. For example, Chinese invention patent CN114855076B, a high carbon steel with high spheroidization rate and its preparation method, discloses a preparation method for improving the spheroidization rate of high carbon steel. The method can further improve the spheroidization rate under the existing spheroidization process by adding 0.01-0.10% Nb by weight on the basis of the high carbon steel composition. However, in order to facilitate the precipitation strengthening of Nb and promote the nucleation of pearlite, obtain fine lamellar pearlite, and thus facilitate the high spheroidization rate, the patent requires 4-6 rough rolling and 6-12 finishing rolling. At the same time, it has high requirements on the rolling inlet and outlet temperature, the cooling rate after rolling, etc., and the rolling process is complex and the energy consumption is high. Chinese invention patent application CN113957209A, a high carbon chromium bearing steel strong magnetic field rapid spheroidizing annealing process, discloses a high carbon steel rapid spheroidizing annealing method, which places the high carbon steel in a strong magnetic field heat treatment device with a strength of 8-12T. The strong magnetic field can reduce the pro-eutectoid cementite content, accelerate the divorced eutectoid phase transformation, and shorten the spheroidizing annealing time. However, the formation of carbides in this patent mainly occurs in the slow cooling process, making the particle size uneven. Summary of the invention
[0004] The first object of the present invention is to provide a high carbon steel with a high spheroidization rate and a fast spheroidization rate in view of the above-mentioned problems existing in the prior art. The technical problem to be solved by the present invention is to improve the spheroidization rate of high carbon steel and shorten the required spheroidization time.
[0005] The object of the present invention can be achieved by the following technical scheme: a fast spheroidizing high-spheroidizing rate high-carbon steel, characterized in that, in terms of weight percentage, the chemical composition of the high-carbon steel is: 0.60% to 0.85% C, 1.35% to 1.80% Si, 1.75% to 2.20% Mn, 0.75% to 1.25% Cr, 0.15% to 0.35% Mo, 1.15% to 1.61% Al, no more than 0.012% P, no more than 0.005% S, the balance is Fe and unavoidable impurities, the microstructure of the high-carbon steel includes ferrite and dispersed spheroidal carbides, and the spheroidizing rate of the high-carbon steel is greater than 85%.
[0006] On the basis of high carbon steel composition, 1.15% to 1.61% Al by mass is added. Al precipitates after solid solution, which promotes the formation of fine lamellar pearlite, and can further improve the spheroidization rate under the existing spheroidizing process.
[0007] The second object of the present invention is to provide a method for preparing the above-mentioned high carbon steel, aiming to shorten the spheroidization time, reduce energy consumption and improve the spheroidization effect.
[0008] The object of the present invention can be achieved by the following technical scheme: A method for preparing high-carbon steel with rapid spheroidization and high spheroidization rate, characterized in that it comprises the following steps: smelting and continuously casting molten steel to obtain a steel billet; heating the steel billet to obtain a hot steel billet; rolling the hot steel billet and then cooling it to obtain high-carbon steel; during the smelting, the chemical component Al of the steel is added at the end of the smelting;
[0009] The high carbon steel is placed in a steady-state strong magnetic field heat treatment device with a strength of 6 to 10 T. The high carbon steel is heated to A under this magnetic field. c1 +(30~60)℃ temperature for austenitization, where A c1 It is the temperature at which pearlite starts to transform into austenite during heating, and the heating and holding time is 30 to 50 minutes. The magnetic field is reduced and the temperature is lowered until the magnetic field reaches zero, which is room temperature. The high carbon steel is then placed in a steady strong magnetic field with an intensity of 6 to 10T at a temperature of 700-750℃ for isothermal treatment, and the isothermal time is 120 to 240 minutes. The magnetic field is reduced and the temperature is lowered until the magnetic field reaches zero, which is room temperature.
[0010] Furthermore, the strong magnetic field applied during the heat treatment is generated by a superconducting magnet, and the heat treatment device is a tantalum wire heating tubular furnace under a controllable temperature magnetic field.
[0011] Furthermore, the heating tube furnace is placed in the horizontal through hole of the superconducting magnet with a cross-aperture.
[0012] By applying a strong magnetic field, the phase change is accelerated, the spheroidization time is shortened, the energy consumption is reduced, and the spheroidization effect is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is the metallographic (OM) organization diagram of the spheroidizing treatment of the present invention;
[0014] Figure 2 It is a scanning electron microscope (SEM) organization diagram of the spheroidization treatment of the present invention. DETAILED DESCRIPTION
[0015] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.
[0016] Example 1
[0017] In this embodiment, 1.46% Al by mass is added to high carbon steel, and the high carbon steel is placed in a steady strong magnetic field heat treatment device with a strength of 10T. The high carbon steel is heated to 950°C under the magnetic field for austenitization, and the austenitization time is 30 minutes. The magnetic field is reduced and the temperature is lowered until the magnetic field is zero and the temperature is room temperature. The high carbon steel is then placed in a steady strong magnetic field with a strength of 10T at 710°C for isothermal treatment, and the isothermal time is 200 minutes. The magnetic field is reduced and the temperature is lowered until the magnetic field is zero and the temperature is room temperature.
[0018] The microstructure of the high carbon steel after treatment in this embodiment is fine, uniform, and dispersed spheroidal carbides embedded in a ferrite matrix, the spheroidization rate is >85%, and the microhardness of the spheroidized microstructure is 276HV1.
[0019] Example 2
[0020] In this embodiment, 1.37% Al by mass is added to high carbon steel, and the high carbon steel is placed in a steady strong magnetic field heat treatment device with a strength of 10T. The high carbon steel is heated to 910°C for austenitization under the magnetic field for 40 minutes, and the magnetic field is reduced and the temperature is lowered until the magnetic field is zero and the temperature is room temperature; the high carbon steel is then placed in a steady strong magnetic field with a strength of 10T at 710°C for isothermal treatment, and the isothermal time is 240 minutes, and the magnetic field is reduced and the temperature is lowered until the magnetic field is zero and the temperature is room temperature.
[0021] like Figure 1 and Figure 2 As shown, in the high carbon steel structure treated by the method described in this embodiment, the carbides are fine, uniform, and dispersedly distributed on the ferrite matrix, the spheroidization rate is >85%, and the microhardness of the spheroidized structure is 263HV1.
[0022] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. A fast spheroidizing high carbon steel with high spheroidizing rate, characterized in that: The chemical composition of the high carbon steel is, by weight percentage, 0.60% to 0.85% C, 1.35% to 1.80% Si, 1.75% to 2.20% Mn, 0.75% to 1.25% Cr, 0.15% to 0.35% Mo, 1.15% to 1.61% Al, no more than 0.012% P, no more than 0.005% S, and the balance is Fe and unavoidable impurities. The microstructure of the high carbon steel includes ferrite and dispersed spheroidal carbides, and the spheroidization rate of the high carbon steel is >85%.
2. A method for preparing high carbon steel by rapid spheroidization, characterized in that: The method comprises the following steps: A. based on the chemical composition of the high carbon steel as claimed in claim 1, smelting molten steel obtained by melting materials other than the chemical component Al, adding the chemical component Al at the end of smelting, and obtaining a steel billet by continuous casting; The steel billet is heated to obtain a hot steel billet; the hot steel billet is rolled and then cooled to obtain high carbon steel; B. Place the high carbon steel obtained in step A in a steady-state strong magnetic field heat treatment device with a strength of 6 to 10 T, and heat the high carbon steel to A under the magnetic field. c1 +(30~60)℃ temperature for austenitization, where A c1 It is the temperature at which pearlite starts to transform into austenite during heating, and the heating and holding time is 30 to 50 minutes. The magnetic field is reduced and the temperature is lowered until the magnetic field reaches zero, which is room temperature. The high carbon steel is then placed in a steady strong magnetic field with an intensity of 6 to 10T at a temperature of 700-750℃ for isothermal treatment, and the isothermal time is 120 to 240 minutes. The magnetic field is reduced and the temperature is lowered until the magnetic field reaches zero, which is room temperature.
3. The method for preparing a high carbon steel with rapid spheroidization and high spheroidization rate according to claim 2, characterized in that: The strong magnetic field applied during the heat treatment in step B is generated by a superconducting magnet, and the heat treatment device is a tantalum wire heating tubular furnace under a controllable temperature magnetic field.
4. The method for preparing high carbon steel with rapid spheroidization and high spheroidization rate according to claim 3, characterized in that: The heating tube furnace is placed in the horizontal through hole of the superconducting magnet with a cross-intersecting aperture.
Citation Information
Patent Citations
High-carbon chromium bearing steel high-intensity magnetic field rapid spheroidizing annealing process
CN113957209A
A high-sphericity high-carbon steel and its preparation method