Method for heat treatment of copper-aluminum plug-in composite material
By performing heat treatment under a strong magnetic field condition of 0.5-3T, the growth of intermetallic compounds in the copper-aluminum interlocking composite material is suppressed, the problem of poor interfacial bonding strength is solved, and the mechanical and electrical properties of the material are improved.
Patent Information
- Application Number
- CN202411112905.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
AI Technical Summary
The intermetallic compounds formed by existing copper-aluminum interpolation composites during heat treatment lead to poor interfacial bonding strength, affecting mechanical and electrical properties.
Heat treatment is carried out under a strong magnetic field condition of 0.5-3T to inhibit the growth of brittle compounds, affect the state of electron movement through magnetization energy, and control the size of the interface compound, thereby improving the bonding strength of the copper-aluminum interfacing composite material.
It effectively inhibits the growth of intermetallic compounds, improves the mechanical and electrical properties of copper-aluminum interlocking composite materials, while maintaining the integrity of the material and the feasibility of subsequent processing.
Smart Images

Figure CN118880205A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material preparation, and in particular relates to a method for heat treatment of a copper-aluminum plug-in composite material. Background Art
[0002] Copper-aluminum plug-in composite materials (sheets, strips, copper-clad aluminum, etc.) combine the advantages of copper's high electrical conductivity with aluminum's light weight, low price, excellent electrical and thermal conductivity, etc., and have been widely used in aviation, aerospace, machinery, medical, food, civil and other fields. At present, the production of copper-aluminum plug-in composite materials (sheets, strips, copper-clad aluminum, etc.) mainly adopts solid-solid composite method, solid-liquid composite method such as rolling composite method, casting and rolling composite method, etc. The main basic principle is that the metal plate to be composited produces plastic deformation in the entire metal interface under the pressure of the rolling mill, and the atoms between the component layers on the metal surface move with each other to form a mechanical bond. After rolling is completed, heat treatment is carried out. The internal stress formed during the rolling process is eliminated by heat treatment to improve the plasticity and toughness of the material, and promote the diffusion of copper and aluminum atoms to form a metallurgical bond.
[0003] During the heat treatment process, the solid-state reaction of Cu and Al originates from the thermal motion and diffusion behavior of copper and aluminum atoms. The diffusion of atoms under no external field conditions is related to temperature and holding time. As the temperature increases and the holding time increases, the vibration energy of the atoms increases, so the probability of atoms migrating across the potential barrier with the help of energy fluctuations increases; at the same time, when the atomic ratio exceeds the maximum solid solubility, intermetallic compounds such as CuAl2, CuAl, Cu9Al4, etc. will be formed, causing the interface compound to become thicker; due to the large hardness and brittleness of intermetallic compounds, differences in properties with the matrix on both sides, and high resistivity, when the thickness of the bonding layer is too thick, it affects the bonding strength of copper and aluminum, which will seriously affect the mechanical and electrical properties of the copper-aluminum composite plate and strip. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the main purpose of the present invention is to provide a method for heat treatment of copper-aluminum plug composite materials, aiming to solve the problem of poor mechanical and electrical properties caused by poor interface bonding strength of existing copper-aluminum plug composite materials.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] A method for heat treatment of a copper-aluminum plug-in composite material comprises the following steps:
[0007] 1) Wire cutting the cast-rolled copper-aluminum composite sheet to obtain a copper-aluminum composite sheet sample;
[0008] 2) placing the copper-aluminum composite sheet sample in the center of the magnetic field heat treatment furnace, performing heat treatment at the same time, and then air cooling to room temperature to obtain the copper-aluminum composite sheet after heat treatment;
[0009] 3) grinding and polishing the surface of the heat-treated copper-aluminum composite plate, and then cleaning and drying to obtain a copper-aluminum plug-in composite material.
[0010] Preferably, the length, width and height of the copper-aluminum composite sheet sample are 100-200 mm, 50-70 mm, and 3-8 mm, respectively.
[0011] Preferably, the process parameters of the heat treatment in step 2) are: under the condition of a strong magnetic field of 0.5-3T, the heat treatment temperature is 250-400°C and the time is 0.5-1.5h.
[0012] Preferably, the grinding and polishing in step 3) is specifically: grinding with SiC sandpaper from 400# to 2000#, and then electrolytic polishing.
[0013] Furthermore, the electrolyte used in the electrolytic polishing is 60% methanol + 35% n-butanol + 5% perchloric acid, the voltage is 35V, the time is 15s-30s, and the electrolyte temperature is ≤10°C.
[0014] Preferably, the copper in the copper-aluminum composite plate is T2 copper, and the aluminum is 1060 aluminum.
[0015] Compared with the prior art, the present invention has at least the following advantages:
[0016] The heat treatment method of the copper-aluminum plug composite material provided by the present invention adopts the method of introducing a steady magnetic field for heat treatment, suppresses the growth of brittle compounds during the heat treatment of the copper-aluminum plug composite material, uses the magnetic field to apply additional magnetization energy and driving force, affects the motion state of electrons in the material to cause a phase change, thereby making the size of the compounds at the interface of the copper-aluminum plug composite material smaller, improving the bonding strength between the interfaces, and thus improving the mechanical and electrical properties of the copper-aluminum plug composite material; at the same time, the method has a simple process and strong replicability, can ensure that the copper-aluminum plug composite material does not crack, and does not affect subsequent processing steps. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.
[0018] Figure 1 This is an electron microscope (TEM) image of the copper-aluminum plug-in composite material of Example 1 of the present invention;
[0019] Figure 2Electron microscope (TEM) image of the copper-aluminum plug composite material of Comparative Example 1 of the present invention;
[0020] Figure 3 Electron microscope (TEM) image of the copper-aluminum plug-in composite material of Example 2 of the present invention;
[0021] Figure 4 Electron microscope (TEM) image of the copper-aluminum plug composite material of Comparative Example 2 of the present invention;
[0022] Figure 5 Electron microscope (TEM) image of the copper-aluminum plug composite material of Comparative Example 3 of the present invention;
[0023] Figure 6 Electron microscope (TEM) image of the copper-aluminum plug composite material of Example 4 of the present invention;
[0024] Figure 7 Electron microscope (TEM) image of the copper-aluminum plug-in composite material of Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0025] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0026] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values listed herein include the endpoints of the range, and all integers and fractions within the range.
[0027] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.
[0028] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.
[0029] Example 1
[0030] A method for heat treatment of a copper-aluminum composite material provided in this embodiment includes the following steps:
[0031] 1) Cut the cast-rolled copper-aluminum composite sheet into copper-aluminum composite sheet samples with a size of 150 mm × 60 mm × 5 mm by wire cutting, wherein the copper is T2 copper and the aluminum is 1060 aluminum;
[0032] 2) Setting the magnetic field strength to 0.5T, after the magnetic field strength reaches the set value, placing the copper-aluminum composite plate sample in step 1) in the center of the magnetic field heat treatment furnace, and performing heat treatment at the same time to ensure that the copper-aluminum composite plate sample is heated evenly and the surrounding gradient magnetic field is minimized;
[0033] The heat treatment temperature was set at 285°C, the heating rate was set at 40°C / min, the temperature was raised from room temperature to the set temperature, the temperature was kept for 60 minutes, and then air-cooled to room temperature to obtain the heat-treated copper-aluminum composite plate;
[0034] 3) The surface of the copper-aluminum composite plate after heat treatment is first polished with SiC sandpaper from 400# to 2000#, and then electrolytically polished, wherein the electrolyte is 60% methanol + 35% n-butanol + 5% perchloric acid, the voltage is 35V, the time is 20s, the electrolyte temperature is ≤10°C, and after polishing, it is placed in an ultrasonic wave and washed with alcohol and dried to obtain a copper-aluminum plug-in composite material.
[0035] Comparative Example 1
[0036] The comparative example provides a method for heat treatment of a copper-aluminum plug-in composite material, which is basically the same as that of Example 1, except that a steady magnetic field is not used in step 2), specifically:
[0037] 1) Cut the cast-rolled copper-aluminum composite sheet into copper-aluminum composite sheet samples with a size of 150 mm × 60 mm × 5 mm by wire cutting, wherein the copper is T2 copper and the aluminum is 1060 aluminum;
[0038] 2) heat treating the copper-aluminum composite plate sample in step 1), wherein the heat treatment temperature is set to 285° C., the heating rate is set to 40° C. / min, the temperature is raised from room temperature to the set temperature, kept at this temperature for 60 minutes, and then air-cooled to room temperature to obtain the heat-treated copper-aluminum composite plate;
[0039] 3) The surface of the copper-aluminum composite plate after heat treatment is first polished with SiC sandpaper from 400# to 2000#, and then electrolytically polished, wherein the electrolyte is 60% methanol + 35% n-butanol + 5% perchloric acid, the voltage is 35V, the time is 20s, the electrolyte temperature is ≤10°C, and after polishing, it is placed in an ultrasonic wave and washed with alcohol and dried to obtain a copper-aluminum plug-in composite material.
[0040] The present application conducted electron microscope scanning on the copper-aluminum plug composite material prepared in Example 1 and Comparative Example 1. The results are as follows: Figure 1 and Figure 2As shown in the figure, it can be seen that the copper-aluminum plug-in composite material that was heat treated at 285℃ / 60min under 0.5T strong magnetic field conditions, compared with the copper-aluminum plug-in composite material that was directly heat treated at 285℃ / 60min, the compound size of the bonding interface of the copper-aluminum plug-in composite material changed from 16.11um to 8.74um, indicating that the magnetic field combined with heat treatment can effectively inhibit the growth size of intermetallic compounds, thereby improving the strength between the copper-aluminum bonding interface.
[0041] Example 2
[0042] A method for heat treatment of a copper-aluminum composite material provided in this embodiment includes the following steps:
[0043] 1) Cut the cast-rolled copper-aluminum composite sheet into copper-aluminum composite sheet samples with a size of 150 mm × 60 mm × 5 mm by wire cutting, wherein the copper is T2 copper and the aluminum is 1060 aluminum;
[0044] 2) Setting the magnetic field strength to 0.5T, after the magnetic field strength reaches the set value, placing the copper-aluminum composite plate sample in step 1) in the center of the magnetic field heat treatment furnace, and performing heat treatment at the same time to ensure that the copper-aluminum composite plate sample is heated evenly and the surrounding gradient magnetic field is minimized;
[0045] The heat treatment temperature was set at 315°C, the heating rate was set at 40°C / min, the temperature was raised from room temperature to the set temperature, the temperature was kept for 60 minutes, and then air-cooled to room temperature to obtain the copper-aluminum composite plate after heat treatment;
[0046] 3) The surface of the copper-aluminum composite plate after heat treatment is first polished with SiC sandpaper from 400# to 2000#, and then electrolytically polished, wherein the electrolyte is 60% methanol + 35% n-butanol + 5% perchloric acid, the voltage is 35V, the time is 20s, the electrolyte temperature is ≤10°C, and after polishing, it is placed in an ultrasonic wave and washed with alcohol and dried to obtain a copper-aluminum plug-in composite material.
[0047] Comparative Example 2
[0048] The comparative example provides a method for heat treatment of a copper-aluminum plug-in composite material, which is basically the same as that of Example 1, except that a steady magnetic field is not used in step 2), specifically:
[0049] 1) Cut the cast-rolled copper-aluminum composite sheet into copper-aluminum composite sheet samples with a size of 150 mm × 60 mm × 5 mm by wire cutting, wherein the copper is T2 copper and the aluminum is 1060 aluminum;
[0050] 2) heat treating the copper-aluminum composite plate sample in step 1), wherein the heat treatment temperature is set to 315° C., the heating rate is set to 40° C. / min, the temperature is raised from room temperature to the set temperature, kept at this temperature for 60 min, and then air-cooled to room temperature to obtain the heat-treated copper-aluminum composite plate;
[0051] 3) The surface of the copper-aluminum composite plate after heat treatment is first polished with SiC sandpaper from 400# to 2000#, and then electrolytically polished, wherein the electrolyte is 60% methanol + 35% n-butanol + 5% perchloric acid, the voltage is 35V, the time is 20s, the electrolyte temperature is ≤10°C, and after polishing, it is placed in an ultrasonic wave and washed with alcohol and dried to obtain a copper-aluminum plug-in composite material.
[0052] The present application conducted electron microscope scanning on the copper-aluminum plug composite material prepared in Example 2 and Comparative Example 2. The results are as follows: Figure 3 and Figure 4 As shown in the figure, it can be seen that the copper-aluminum plug-in composite material that was heat treated at 315℃ / 60min under 0.5T strong magnetic field conditions, compared with the copper-aluminum plug-in composite material that was directly heat treated at 315℃ / 60min, the compound size of the bonding interface of the copper-aluminum plug-in composite material changed from 17.42um to 6.06um, indicating that the magnetic field combined with heat treatment can effectively inhibit the growth size of intermetallic compounds, thereby improving the strength between the copper-aluminum bonding interface.
[0053] Example 3
[0054] The present embodiment provides a method for heat treatment of a copper-aluminum plug composite material, which is basically the same as that of Embodiment 2, except that the magnetic field strength is set to 1.5 T in step 2); specifically, the method comprises the following steps:
[0055] 1) Cut the cast-rolled copper-aluminum composite sheet into copper-aluminum composite sheet samples with a size of 150 mm × 60 mm × 5 mm by wire cutting, wherein the copper is T2 copper and the aluminum is 1060 aluminum;
[0056] 2) Setting the magnetic field strength to 1.5 T, after the magnetic field strength reaches the set value, placing the copper-aluminum composite plate sample in step 1) in the center of the magnetic field heat treatment furnace, and performing heat treatment at the same time to ensure that the copper-aluminum composite plate sample is heated evenly and the surrounding gradient magnetic field is minimized;
[0057] The heat treatment temperature was set at 315°C, the heating rate was set at 40°C / min, the temperature was raised from room temperature to the set temperature, the temperature was kept for 60 minutes, and then air-cooled to room temperature to obtain the copper-aluminum composite plate after heat treatment;
[0058] 3) The surface of the copper-aluminum composite plate after heat treatment is first polished with SiC sandpaper from 400# to 2000#, and then electrolytically polished, wherein the electrolyte is 60% methanol + 35% n-butanol + 5% perchloric acid, the voltage is 35V, the time is 20s, the electrolyte temperature is ≤10°C, and after polishing, it is placed in an ultrasonic wave and washed with alcohol and dried to obtain a copper-aluminum plug-in composite material.
[0059] The present application conducted electron microscope scanning on the copper-aluminum plug composite material prepared in Example 3. The results are as follows: Figure 5 As shown in the figure, it can be seen that the copper-aluminum plug-in composite material that was heat treated at 315℃ / 60min under 1.5T strong magnetic field conditions, compared with the copper-aluminum plug-in composite material that was directly heat treated at 315℃ / 60min, the compound size of the bonding interface of the copper-aluminum plug-in composite material changed from 17.42um to 3.13um, indicating that the magnetic field combined with heat treatment can effectively inhibit the growth size of intermetallic compounds, thereby improving the strength between the copper-aluminum bonding interface.
[0060] Example 4
[0061] A method for heat treatment of a copper-aluminum composite material provided in this embodiment includes the following steps:
[0062] 1) Cut the cast-rolled copper-aluminum composite sheet into copper-aluminum composite sheet samples with a size of 150 mm × 60 mm × 5 mm by wire cutting, wherein the copper is T2 copper and the aluminum is 1060 aluminum;
[0063] 2) Setting the magnetic field strength to 3T, after the magnetic field strength reaches the set value, placing the copper-aluminum composite plate sample in step 1) in the center of the magnetic field heat treatment furnace, and performing heat treatment at the same time, to ensure that the copper-aluminum composite plate sample is heated evenly and the surrounding gradient magnetic field is minimized;
[0064] The heat treatment temperature was set at 400°C, the heating rate was set at 40°C / min, the temperature was raised from room temperature to the set temperature, the temperature was kept for 90 minutes, and then air-cooled to room temperature to obtain the heat-treated copper-aluminum composite plate;
[0065] 3) The surface of the copper-aluminum composite plate after heat treatment is first polished with SiC sandpaper from 400# to 2000#, and then electrolytically polished, wherein the electrolyte is 60% methanol + 35% n-butanol + 5% perchloric acid, the voltage is 35V, the time is 20s, the electrolyte temperature is ≤10°C, and after polishing, it is placed in an ultrasonic wave and washed with alcohol and dried to obtain a copper-aluminum plug-in composite material.
[0066] Comparative Example 4
[0067] The comparative example provides a method for heat treatment of a copper-aluminum plug-in composite material, which is basically the same as that of Example 1, except that a steady magnetic field is not used in step 2), specifically:
[0068] 1) Cut the cast-rolled copper-aluminum composite sheet into copper-aluminum composite sheet samples with a size of 150 mm × 60 mm × 5 mm by wire cutting, wherein the copper is T2 copper and the aluminum is 1060 aluminum;
[0069] 2) heat treating the copper-aluminum composite plate sample in step 1), wherein the heat treatment temperature is set to 400° C., the heating rate is set to 90° C. / min, the temperature is raised from room temperature to the set temperature, kept at this temperature for 60 min, and then air-cooled to room temperature to obtain the heat-treated copper-aluminum composite plate;
[0070] 3) The surface of the copper-aluminum composite plate after heat treatment is first polished with SiC sandpaper from 400# to 2000#, and then electrolytically polished, wherein the electrolyte is 60% methanol + 35% n-butanol + 5% perchloric acid, the voltage is 35V, the time is 20s, the electrolyte temperature is ≤10°C, and after polishing, it is placed in an ultrasonic wave and washed with alcohol and dried to obtain a copper-aluminum plug-in composite material.
[0071] The present application conducted electron microscope scanning on the copper-aluminum plug composite material prepared in Example 4 and Comparative Example 4. The results are as follows: Figure 6 and Figure 7 As shown in the figure, it can be seen that the copper-aluminum plug-in composite material that was heat treated at 400℃ / 90min under a 3.0T strong magnetic field, compared with the copper-aluminum plug-in composite material that was directly heat treated at 400℃ / 90min, the compound size of the bonding interface of the copper-aluminum plug-in composite material changed from 25.59um to 10.05um, indicating that the magnetic field combined with heat treatment can effectively inhibit the growth size of intermetallic compounds, thereby improving the strength between the copper-aluminum bonding interface.
[0072] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A method for heat treatment of copper-aluminum plug-in composite materials, It is characterized in that The steps include: 1) Wire cutting the cast-rolled copper-aluminum composite sheet to obtain a copper-aluminum composite sheet sample; 2) placing the copper-aluminum composite sheet sample in the center of the magnetic field heat treatment furnace, performing heat treatment at the same time, and then air cooling to room temperature to obtain the copper-aluminum composite sheet after heat treatment; 3) grinding and polishing the surface of the heat-treated copper-aluminum composite plate, and then cleaning and drying to obtain a copper-aluminum plug-in composite material.
2. The method for heat treatment of the copper-aluminum composite material according to claim 1, It is characterized in that The length, width and height of the copper-aluminum composite plate sample are 100-200 mm, 50-70 mm, and 3-8 mm respectively.
3. The method for heat treatment of the copper-aluminum composite material according to claim 1, It is characterized in that The process parameters of the heat treatment in step 2) are: under the condition of a strong magnetic field of 0.5-3T, the heat treatment temperature is 250-400°C and the time is 0.5-1.5h.
4. The method for heat treatment of the copper-aluminum composite material according to claim 1, It is characterized in that The grinding and polishing in step 3) is specifically: grinding with SiC sandpaper from 400# to 2000#, and then electrolytic polishing.
5. The method for heat treatment of the copper-aluminum plug composite material according to claim 4, It is characterized in that The electrolyte used in the electrolytic polishing is 60% methanol + 35% n-butanol + 5% perchloric acid, the voltage is 35V, the time is 15s-30s, and the electrolyte temperature is ≤10°C.