Galvanizing process for compressor crankshaft surface treatment
By galvanizing the compressor crankshaft, the zinc layer is formed, which solves the problem of poor corrosion resistance and extends the service life.
Patent Information
- Application Number
- CN202410946821.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing compressor crankshaft has poor corrosion resistance when used and cannot adapt to harsh environments, resulting in a short service life.
Using a compressor crankshaft surface treatment galvanizing process, including cleaning, degreasing, pickling, water washing, assisted plating, preheating, galvanizing and passivation treatment, by soaking the crankshaft in zinc liquid in a hot-dip galvanizing tank , the zinc liquid temperature is 450-460°C and the zinc immersion time is 1-2 minutes to form a complete zinc layer.
It significantly improves the corrosion resistance of the compressor crankshaft and extends its service life.
Smart Images

Figure CN118880210A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of compressor crankshafts, in particular to a galvanizing process for surface treatment of compressor crankshafts. Background Art
[0002] The crankshaft is the most important part of the engine. It bears the force from the connecting rod and converts it into torque, which is output through the crankshaft and drives other accessories on the engine. The crankshaft is subjected to the combined effects of the centrifugal force of the rotating mass, the periodically changing gas inertia force and the reciprocating inertia force, which makes the crankshaft subject to bending and torsion loads. Therefore, the crankshaft is required to have sufficient strength and rigidity, and the journal surface must be wear-resistant, work evenly and have good balance.
[0003] The Chinese patent with publication number CN107876780A discloses a method for manufacturing a compressor crankshaft, which involves the field of powder metallurgy. The preparation method is as follows: iron powder, aluminum powder, copper powder, tin powder, niobium powder, vanadium powder, manganese, chromium, and nano titanium dioxide powder are mixed and stirred at 80-100°C for 60-80 minutes, then heated to 180-200°C, and then boron, silicon nitride, cuprous thiocyanate, antimony trisulfide powder, and carbon powder are added, cooled to 100-120°C, loaded into a mold, pressed into a blank, and then naturally Cool to room temperature, the pressing pressure is 100-200MPa; the obtained compact is placed in a closed sintering furnace for sintering, the sintering temperature rises from room temperature to 900°C at a rate of 14°C / min, and is kept at 900°C for 30 minutes; its tensile strength, yield resistance and wear resistance are very good, and the properties of the original material will not be changed due to processing, avoiding the increased processing complexity caused by other treatments of the processed material to meet performance requirements; however, the patent has the following defects:
[0004] The existing compressor crankshaft has poor anti-corrosion performance when in use and cannot adapt well to harsh environments, resulting in a short service life of the compressor crankshaft. Summary of the invention
[0005] The purpose of the present invention is to provide a galvanizing process for the surface treatment of a compressor crankshaft, which can improve the corrosion resistance of the compressor crankshaft, extend the service life of the compressor crankshaft, and solve the problems raised in the above-mentioned background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A compressor crankshaft surface treatment galvanizing process comprises the following steps:
[0008] S1. Crankshaft cleaning: put the crankshaft into an ultrasonic cleaning machine and use the ultrasonic cleaning machine to clean the impurities on the crankshaft surface;
[0009] S2, degreasing treatment: put the crankshaft into the degreasing tank, immerse the crankshaft completely in the degreasing liquid in the degreasing tank, and use the degreasing liquid to remove grease on the crankshaft surface;
[0010] S3, pickling treatment: put the crankshaft into the pickling tank, immerse the crankshaft completely in the pickling liquid in the pickling tank, and use the pickling liquid to remove the oxide on the crankshaft surface;
[0011] S4, water washing treatment: put the crankshaft into a water washing tank, immerse the crankshaft completely in the clean water in the water washing tank, use clean water to remove the pickling liquid on the surface of the crankshaft, and spray the surface of the crankshaft with water;
[0012] S5, plating treatment: put the crankshaft into the plating tank, make the crankshaft completely immersed in the plating solution in the plating tank, vibrate the crankshaft with a vibrator to shake off the excess plating solution on the crankshaft surface, and make the plating solution on the crankshaft surface evenly covered, and the vibration time is 2-5s;
[0013] S6. Preheating treatment: Place the crankshaft on a drying table, use hot air to dry the crankshaft surface, remove water stains on the crankshaft surface, and preheat the crankshaft surface at the same time;
[0014] S7, galvanizing treatment: put the crankshaft into the hot-dip galvanizing tank, and immerse the crankshaft completely in the zinc liquid in the hot-dip galvanizing tank. The zinc liquid temperature is 450-460℃, and the zinc immersion time is 1-2min. The zinc liquid is completely coated on the surface of the crankshaft, and then cooled after galvanizing;
[0015] S8, passivation treatment: spray the passivation liquid on the surface of the galvanized crankshaft to form a passivation film on the crankshaft surface, and rinse the passivated crankshaft surface at a rinsing temperature of 30-45°C and a rinsing time of 1-2 minutes;
[0016] S9. Inspection and processing: Check whether there is any missing plating, zinc nodules, zinc thorns, or color difference on the crankshaft surface. Grind the zinc nodules and zinc thorns on the crankshaft surface, test the thickness of the zinc layer on the crankshaft surface, and pack and store the qualified crankshafts as required.
[0017] Preferably, in S1, the cleaning time is 20-25 min, the cleaning frequency is 20-30 kHz, and the sound wave intensity is 0.5-0.8 W / cm 2 .
[0018] Preferably, in S2, the degreasing liquid is an aqueous solution containing 4-7% sodium hydroxide, the temperature of the degreasing liquid is 60° C.-80° C., and the immersion time of the degreasing liquid is 8-15 min.
[0019] Preferably, in S3, the pickling solution is a hydrochloric acid solution with a mass concentration of 13-15%, and the soaking time of the pickling solution is 8-16 minutes.
[0020] Preferably, in S4, a multi-angle synchronous spraying method is used to spray and wash the crankshaft surface in all directions to clean the crankshaft surface, and the washing time is 20-30 minutes.
[0021] Preferably, in S5, the plating-assisting solution comprises the following raw materials in parts by weight: 7-10 parts of ammonium chloride, 12-15 parts of zinc chloride, 18-22 parts of citric acid and 160-180 parts of water.
[0022] Preferably, in S6, the hot air temperature is 80-120°C, so that the crankshaft is preheated to 120-180°C.
[0023] Preferably, in S7, the cooling water temperature is 35-50°C, and during cooling, the crankshaft is completely immersed in the cooling water, and the cooling water is kept flowing.
[0024] Preferably, in S8, the passivation solution is a chromium-free passivation solution.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention performs cleaning, degreasing, pickling, water washing, plating assistance, preheating, galvanizing, passivation and inspection on the surface of the compressor crankshaft, and can pack qualified crankshafts into storage as required. During the galvanizing treatment, the crankshaft is placed in a hot-dip galvanizing tank, and the crankshaft is completely immersed in the zinc liquid in the hot-dip galvanizing tank, the zinc liquid temperature is 450-460°C, the zinc immersion time is 1-2min, the zinc liquid is completely coated on the surface of the crankshaft, and cooling is performed after galvanizing, so that the corrosion resistance of the compressor crankshaft is improved and the service life of the compressor crankshaft is extended. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The present invention is a flow chart of the compressor crankshaft surface treatment galvanizing process. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In order to solve the problem that the existing compressor crankshaft has poor anti-corrosion performance during use and cannot adapt well to harsh environments, resulting in a short service life of the compressor crankshaft, please refer to Figure 1 , this embodiment provides the following technical solutions:
[0030] Embodiment 1
[0031] A compressor crankshaft surface treatment galvanizing process comprises the following steps:
[0032] S1. Crankshaft cleaning: Place the crankshaft into an ultrasonic cleaning machine and use the ultrasonic cleaning machine to clean the impurities on the crankshaft surface. The cleaning time is 20-25 minutes, the cleaning frequency is 20-30kHz, and the sound wave intensity is 0.5-0.8W / cm 2 ;
[0033] It should be noted that the ultrasonic cleaning machine emits a high-frequency oscillation signal from an ultrasonic generator, which is converted into a high-frequency mechanical oscillation by a transducer and propagated into the cleaning solvent. The ultrasonic wave radiates forward in the cleaning liquid in a sparse and dense manner, causing the liquid to flow and generate tens of thousands of tiny bubbles with a diameter of 50-500μm. The tiny bubbles in the liquid vibrate under the action of the sound field. These bubbles are formed and grow in the negative pressure area of the longitudinal propagation of the ultrasonic wave. In the positive pressure area, when the sound pressure reaches a certain value, the bubbles increase rapidly and then suddenly close; and when the bubbles close, shock waves are generated, and thousands of atmospheres of pressure are generated around them, destroying insoluble dirt and dispersing them in the cleaning liquid. When the group particles are wrapped in oil and adhere to the surface of the cleaning part, the oil is emulsified and the solid particles are separated, thereby achieving the purpose of crankshaft purification.
[0034] S2. Degreasing treatment: put the crankshaft into the degreasing tank, immerse the crankshaft completely in the degreasing liquid in the degreasing tank, and use the degreasing liquid to remove the grease on the surface of the crankshaft. The temperature of the degreasing liquid is 60℃-80℃, and the degreasing liquid immersion time is 8-15min;
[0035] Wherein, the degreasing liquid is an aqueous solution containing 4-7% sodium hydroxide;
[0036] S3, pickling treatment: put the crankshaft into the pickling tank, immerse the crankshaft completely in the pickling liquid in the pickling tank, use the pickling liquid to remove the oxide on the crankshaft surface, and the pickling liquid immersion time is 8-16 minutes;
[0037] Wherein, the pickling liquid is a hydrochloric acid solution with a mass concentration of 13-15%;
[0038] S4, water washing treatment: put the crankshaft into a water washing tank, immerse the crankshaft completely in the clean water in the water washing tank, use clean water to remove the pickling liquid on the surface of the crankshaft, and spray the surface of the crankshaft with water;
[0039] Among them, a multi-angle synchronous spraying method is used to spray and wash the crankshaft surface in all directions to make the crankshaft surface clean. The washing time is 20-30 minutes;
[0040] S5, plating treatment: put the crankshaft into the plating tank, make the crankshaft completely immersed in the plating solution in the plating tank, vibrate the crankshaft with a vibrator to shake off the excess plating solution on the crankshaft surface, and make the plating solution on the crankshaft surface evenly covered, and the vibration time is 2-5s;
[0041] The plating solution includes the following raw materials in parts by weight: 7-10 parts of ammonium chloride, 12-15 parts of zinc chloride, 18-22 parts of citric acid and 160-180 parts of water;
[0042] S6. Preheating treatment: Place the crankshaft on a drying table, use hot air to dry the crankshaft surface, remove water stains on the crankshaft surface, and preheat the crankshaft surface at a hot air temperature of 80-120°C to preheat the crankshaft to 120-180°C;
[0043] S7, galvanizing treatment: put the crankshaft into the hot-dip galvanizing tank, and immerse the crankshaft completely in the zinc liquid in the hot-dip galvanizing tank. The zinc liquid temperature is 450℃, and the galvanizing time is 1min. The zinc liquid is completely coated on the surface of the crankshaft. After galvanizing, cool it. The cooling water temperature is 35-50℃. During cooling, immerse the crankshaft completely in the cooling water and keep the cooling water flowing;
[0044] It should be noted that during galvanizing, the temperature of the zinc solution and the galvanizing time must be controlled;
[0045] The temperature is too low, the fluidity of the zinc liquid is poor, the coating is thick and uneven, it is easy to sag, and the appearance quality is poor;
[0046] The temperature is high, the fluidity of zinc liquid is good, the zinc liquid is easy to separate from the workpiece, reducing the occurrence of sagging and wrinkling, strong adhesion, thin coating, good appearance and high production efficiency;
[0047] However, if the temperature is too high, the crankshaft and hot-dip galvanizing tank will suffer serious damage, which will easily produce a large amount of zinc slag, affecting the quality of the zinc-dip layer, causing high zinc consumption and even making it impossible to galvanize.
[0048] S8, passivation treatment: spray the passivation liquid on the surface of the galvanized crankshaft to form a passivation film on the crankshaft surface, and rinse the passivated crankshaft surface at a rinsing temperature of 30-45°C and a rinsing time of 1-2 minutes;
[0049] Wherein, the passivation solution is a chromium-free passivation solution.
[0050] S9. Inspection and processing: Check whether there is any missing plating, zinc nodules, zinc thorns, or color difference on the crankshaft surface. Grind the zinc nodules and zinc thorns on the crankshaft surface, test the thickness of the zinc layer on the crankshaft surface, and pack and store the qualified crankshafts as required.
[0051] Embodiment 2
[0052] Compared with the first embodiment, the difference is that during the galvanizing treatment, the zinc liquid temperature and the zinc immersion time are different;
[0053] Among them, the zinc liquid temperature is 460℃ and the zinc immersion time is 1min.
[0054] Embodiment 3
[0055] Compared with the first embodiment, the difference is that during the galvanizing treatment, the zinc liquid temperature and the zinc immersion time are different;
[0056] Among them, the zinc liquid temperature is 450℃ and the zinc immersion time is 2min.
[0057] Comparative Example
[0058] A Chinese patent with publication number CN107876780A discloses a method for manufacturing a compressor crankshaft. The compressor crankshaft is manufactured according to the above-mentioned method for manufacturing a compressor crankshaft, wherein the compressor crankshaft is not subjected to galvanizing treatment.
[0059] The surface of the compressor crankshaft was galvanized according to the galvanizing process in Examples 1-3, and the performance of the compressor crankshaft after galvanizing was tested, wherein the performance test results of the compressor crankshaft are shown in Table 1:
[0060] Table 1: Compressor crankshaft performance test results
[0061] Embodiment 1 Embodiment 2 Embodiment 3 Comparative Example Galvanizing have have have none Zinc liquid temperature 450℃ 460℃ 450℃ none Galvanizing time 1min 1min 2min none Zinc layer thickness 66um 69um 74um none Anti-corrosion properties 97.34% 97.85% 98.27% 76.14%
[0062] It can be seen from the above table that the galvanizing process for the surface treatment of the compressor crankshaft in Examples 1 to 3 can improve the anti-corrosion performance of the compressor crankshaft and extend the service life of the compressor crankshaft.
[0063] Among them, compared with Example 1, Example 2 has improved anti-corrosion performance, which indicates that increasing the temperature of zinc liquid can improve the anti-corrosion performance of the compressor crankshaft and extend the service life of the compressor crankshaft;
[0064] Among them, compared with Example 1, Example 3 has improved anti-corrosion performance, which indicates that increasing the zinc immersion time can improve the anti-corrosion performance of the compressor crankshaft and extend the service life of the compressor crankshaft;
[0065] Among them, compared with Example 1, the anti-corrosion performance of the comparative example is reduced. Since the surface of the compressor crankshaft in the comparative example is not galvanized, the anti-corrosion performance is reduced, which indicates that galvanizing can improve the anti-corrosion performance of the compressor crankshaft and extend the service life of the compressor crankshaft.
[0066] Therefore, by cleaning, degreasing, pickling, washing, plating, preheating, galvanizing, passivation and inspecting the surface of the compressor crankshaft, the qualified crankshafts can be packaged and stored as required. During the galvanizing treatment, the crankshaft is placed in a hot-dip galvanizing tank, and the crankshaft is completely immersed in the zinc liquid in the hot-dip galvanizing tank. The zinc liquid temperature is 450-460℃, the galvanizing time is 1-2min, and the zinc liquid is completely coated on the crankshaft surface. Cooling after galvanizing can improve the corrosion resistance of the compressor crankshaft and extend the service life of the compressor crankshaft.
[0067] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0068] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A compressor crankshaft surface treatment galvanizing process, characterized in that: The steps include: S1. Crankshaft cleaning: put the crankshaft into an ultrasonic cleaning machine and use the ultrasonic cleaning machine to clean the impurities on the crankshaft surface; S2, degreasing treatment: put the crankshaft into the degreasing tank, immerse the crankshaft completely in the degreasing liquid in the degreasing tank, and use the degreasing liquid to remove grease on the crankshaft surface; S3, pickling treatment: put the crankshaft into the pickling tank, immerse the crankshaft completely in the pickling liquid in the pickling tank, and use the pickling liquid to remove the oxide on the crankshaft surface; S4, water washing treatment: put the crankshaft into a water washing tank, immerse the crankshaft completely in the clean water in the water washing tank, use clean water to remove the pickling liquid on the surface of the crankshaft, and spray the surface of the crankshaft with water; S5, plating treatment: put the crankshaft into the plating tank, make the crankshaft completely immersed in the plating solution in the plating tank, vibrate the crankshaft with a vibrator to shake off the excess plating solution on the crankshaft surface, and make the plating solution on the crankshaft surface evenly covered, and the vibration time is 2-5s; S6. Preheating treatment: Place the crankshaft on a drying table, use hot air to dry the crankshaft surface, remove water stains on the crankshaft surface, and preheat the crankshaft surface at the same time; S7, galvanizing treatment: put the crankshaft into the hot-dip galvanizing tank, and immerse the crankshaft completely in the zinc liquid in the hot-dip galvanizing tank. The zinc liquid temperature is 450-460℃, and the zinc immersion time is 1-2min. The zinc liquid is completely coated on the surface of the crankshaft, and then cooled after galvanizing; S8, passivation treatment: spray the passivation liquid on the surface of the galvanized crankshaft to form a passivation film on the crankshaft surface, and rinse the passivated crankshaft surface at a rinsing temperature of 30-45°C and a rinsing time of 1-2 minutes; S9. Inspection and processing: Check whether there is any missing plating, zinc nodules, zinc thorns, or color difference on the crankshaft surface. Grind the zinc nodules and zinc thorns on the crankshaft surface, test the thickness of the zinc layer on the crankshaft surface, and pack and store the qualified crankshafts as required.
2. A compressor crankshaft surface treatment galvanizing process according to claim 1, characterized in that: In S1, the cleaning time is 20-25 minutes, the cleaning frequency is 20-30kHz, and the sound wave intensity is 0.5-0.8W / cm 2 .
3. A compressor crankshaft surface treatment galvanizing process according to claim 1, characterized in that: In S2, the degreasing liquid is an aqueous solution containing 4-7% sodium hydroxide, the temperature of the degreasing liquid is 60° C.-80° C., and the immersion time of the degreasing liquid is 8-15 minutes.
4. A compressor crankshaft surface treatment galvanizing process according to claim 1, characterized in that: In S3, the pickling solution is a hydrochloric acid solution with a mass concentration of 13-15%, and the soaking time of the pickling solution is 8-16 minutes.
5. A compressor crankshaft surface treatment galvanizing process according to claim 1, characterized in that: In S4, a multi-angle synchronous spraying method is used to spray and wash the crankshaft surface in all directions to clean the crankshaft surface. The washing time is 20-30 minutes.
6. A compressor crankshaft surface treatment galvanizing process according to claim 1, characterized in that: In S5, the plating-assisting solution includes the following raw materials in parts by weight: 7-10 parts of ammonium chloride, 12-15 parts of zinc chloride, 18-22 parts of citric acid and 160-180 parts of water.
7. A compressor crankshaft surface treatment galvanizing process according to claim 1, characterized in that: In S6, the hot air temperature is 80-120°C, so that the crankshaft is preheated to 120-180°C.
8. A compressor crankshaft surface treatment galvanizing process according to claim 1, characterized in that: In S7, the cooling water temperature is 35-50°C. During cooling, the crankshaft is completely immersed in the cooling water, and the cooling water is kept flowing.
9. A compressor crankshaft surface treatment galvanizing process according to claim 1, characterized in that: In the step S8, the passivation solution is a chromium-free passivation solution.
Citation Information
Patent Citations
Manufacturing method of compressor crankshaft
CN107876780A