Degradable paper pulp molded product and preparation method thereof
Through specific combinations of waste pulp suspensions and modified fillers, high-performance degradable pulp molded products are prepared, solving the problem of poor overall performance of existing pulp molded packaging materials, and achieving environmental protection, functionality and economicality Improvement.
Patent Information
- Application Number
- CN202411026041.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The comprehensive performance of existing pulp molded packaging materials is not ideal and it is difficult to meet environmental protection, functional and economic requirements.
Using specific waste pulp suspensions, cellulose, liquor lees enzymatic solution and modified fillers as raw materials, a degradable pulp molded product, including waste pulp suspensions and carboxymethylcellulose , hydroxypropyl methyl cellulose, alumina, zinc oxide and carbon nanotubes, etc., are molded through specific process steps.
It significantly improves the comprehensive performance of biodegradable pulp molded products, including environmental protection, buffering performance, versatility, printing adaptability, anti-static and stackability, reduces production costs and enhances the market competitiveness of the products.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of pulp molded products, and in particular relates to a degradable pulp molded product and a preparation method thereof. Background Art
[0002] Pulp molded packaging material is an environmentally friendly packaging material. It is made of natural fibers such as sugarcane pulp, bamboo pulp, paper scraps, waste paper (such as newspapers, carton paper), etc. as the main raw materials and is manufactured through a series of processes. The production process of this packaging material includes hydraulic pulping, vacuum adsorption molding on a metal mold, and direct curing molding. Due to its unique production process and material properties, pulp molded packaging materials have the following characteristics: Environmental protection: Since the main raw material is renewable plant fiber and recycled paper can be used in the production process, pulp molded packaging materials are recyclable and biodegradable, and have little impact on the environment. Buffering performance: Pulp molded packaging has good buffering and shockproof functions, which is determined by the elasticity and toughness of the fiber material itself. It can replace traditional foamed plastic packaging and performs well in protecting products from shock and vibration. Versatility: Pulp molded packaging can be customized according to the shape and size of different products, and is suitable for packaging of various types of items, such as electronic products, food, cosmetics, etc. Cost-effectiveness: Although the initial investment may be higher, in the long run, molded pulp packaging can reduce waste and lower overall costs due to its recyclability. Printability: The surface of molded pulp packaging can be printed, including hot stamping, silk screen printing, UV printing, etc., which enables it to carry brand logos and marketing information, enhancing product appeal. Anti-static: Compared with some traditional packaging materials, molded pulp packaging performs better in anti-static, which is especially important for the packaging of electronic products. Stackability: Molded pulp packaging is usually designed to be easy to stack, saving storage and transportation space. Molded pulp packaging has a wide range of applications, from industrial cushioning packaging to consumer product packaging, and even in the catering industry (such as tableware and lunch boxes). With the growing global demand for environmentally friendly packaging, molded pulp packaging is gradually becoming a popular green packaging solution. The comprehensive performance of existing molded pulp packaging materials is not ideal. Summary of the invention
[0003] The purpose of the present invention is to provide a degradable pulp molded product and a preparation method thereof.
[0004] In order to achieve the above object, the present invention provides the following technical solutions: A degradable pulp molded product comprises the following raw materials in parts by mass: 50-55 parts of waste pulp suspension, 25-30 parts of cellulose, 10-15 parts of white wine lees enzymatic hydrolyzate, 6-10 parts of modified filler, 5-7 parts of waterproofing agent, 0.03-0.07 parts of retention aid and 1-2 parts of bleaching agent.
[0005] Furthermore, the cellulose is selected from one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether.
[0006] Furthermore, the cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1:0.3-0.7:1.4-1.8.
[0007] Furthermore, the preparation method of the white wine lees enzymatic hydrolyzate is as follows: by mass, 1 part of white wine lees is added to 8-10 parts of deionized water, followed by adding 0.2-0.4 parts of sodium hydroxide, and stirring the reaction at 55-60° C. for 4-5 hours; after the reaction is completed, dilute hydrochloric acid is added to adjust the pH to neutral, followed by adding 0.02 parts of neutral protease, and enzymolysis is carried out at 27-30° C. for 1.5-2 hours. After the enzymolysis is completed, sterilization is carried out to obtain the white wine lees enzymatic hydrolyzate.
[0008] Furthermore, the preparation method of the modified filler is: (1) mixing aluminum oxide, zinc oxide and carbon nanotubes to obtain a filler; (2) Mix filler, 60-65wt% ethanol aqueous solution and silane coupling agent KH550 in a mass ratio of 1:6-8:0.02-0.03, stir and react at 60-65°C for 2-4h, filter and obtain a solid, wash and dry to obtain a modified filler.
[0009] Furthermore, the filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1:1.3-1.5:0.4-0.8.
[0010] Furthermore, the alumina particle size is 1-10 μm, and the specific surface area is 3-6 m 2 / g.
[0011] Furthermore, the particle size of zinc oxide is 30-50nm and the specific surface area is 15-30m 2 / g.
[0012] Furthermore, the diameter of the carbon nanotubes is 2-4 nm, the length is 40-60 μm, and the specific surface area is 400-600 m 2 / g.
[0013] The present invention provides a method for preparing a degradable pulp molded product, comprising the following steps: S1. The waste coated paper is crushed, soaked, pulped and filtered to obtain a residue, which is then washed to prepare a waste paper pulp suspension; S2. After bleaching the waste paper pulp suspension, send it to a pulping tank, add cellulose and white wine lees enzymatic hydrolyzate, add a retention agent, stir evenly, then add a modified filler, and obtain a primary pulp after stirring; S3. The primary slurry is uniformly adsorbed on the lower mold of the molding mold by negative pressure, and immersed in a waterproofing agent solution for 22-25min, and then molded with the upper mold of the molding mold, and the pulp molding wet blank is obtained after the mold is opened; S4. Dry the wet pulp molding to a moisture content of 3-5%, put it into a mold for compression molding, and obtain a degradable pulp molding product.
[0014] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows: the present invention selects specific waste paper pulp suspension, cellulose, white wine lees enzymatic hydrolyzate and modified filler as raw materials, which interact with each other and synergistically enhance the effect, thereby improving the comprehensive performance of the degradable pulp molded products. DETAILED DESCRIPTION
[0015] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] Example 1 The present embodiment provides a degradable pulp molded product, comprising the following raw materials in parts by weight: 52 parts of waste pulp suspension, 27 parts of cellulose, 13 parts of white wine lees enzymatic hydrolyzate, 8 parts of modified filler, 6 parts of waterproofing agent, 0.04 parts of retention aid, and 1.5 parts of bleaching agent.
[0017] The cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1:0.5:1.6.
[0018] The preparation method of the white wine lees enzymatic hydrolyzate is as follows: by weight, 1 part of white wine lees is added to 9 parts of deionized water, followed by adding 0.3 parts of sodium hydroxide, and reacting at 57° C. with stirring for 4-5 hours; after the reaction is completed, dilute hydrochloric acid is added to adjust the pH to neutral, followed by adding 0.02 parts of neutral protease, and enzymolysis is performed at 28° C. for 1.7 hours. After the enzymolysis is completed, sterilization is performed to obtain the white wine lees enzymatic hydrolyzate.
[0019] The preparation method of the modified filler is: (1) mixing aluminum oxide, zinc oxide and carbon nanotubes to obtain a filler; (2) A filler, a 63 wt % ethanol aqueous solution, and a silane coupling agent KH550 were mixed in a mass ratio of 1:7:0.02, stirred at 62° C. for 3 h, and the solid was filtered, washed, and dried to obtain a modified filler.
[0020] The filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1:1.4:0.6.
[0021] The alumina particle size is 1-10 μm and the specific surface area is 3-6 m 2 / g.
[0022] The particle size of zinc oxide is 30-50nm and the specific surface area is 15-30m 2 / g.
[0023] The diameter of carbon nanotubes is 2-4nm, the length is 40-60μm, and the specific surface area is 400-600m 2 / g.
[0024] The method for preparing the degradable pulp molded product comprises the following steps: S1. The waste coated paper is crushed, soaked, pulped and filtered to obtain a residue, which is then washed to prepare a waste paper pulp suspension; S2. After bleaching the waste paper pulp suspension, send it to a pulping tank, add cellulose and white wine lees enzymatic hydrolyzate, add a retention agent, stir evenly, then add a modified filler, and obtain a primary pulp after stirring; S3. The primary slurry is uniformly adsorbed on the lower mold of the molding mold by negative pressure, and immersed in a waterproofing agent solution for 23 minutes, and then molded with the upper mold of the molding mold, and the pulp molding wet blank is obtained after the mold is opened; S4. Dry the wet pulp molding to a moisture content of 4%, put it into a mold for compression molding, and obtain a degradable pulp molding product.
[0025] Example 2 The present embodiment provides a degradable pulp molded product, comprising the following raw materials in parts by weight: 50 parts of waste pulp suspension, 25 parts of cellulose, 10 parts of white wine lees enzymatic hydrolyzate, 6 parts of modified filler, 5 parts of waterproofing agent, 0.03 parts of retention aid, and 1 part of bleaching agent.
[0026] The cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1:0.3:1.4.
[0027] The preparation method of the white wine lees enzymatic hydrolyzate is as follows: by weight, 1 part of white wine lees is added to 8 parts of deionized water, followed by adding 0.2 parts of sodium hydroxide, and reacting at 55° C. with stirring for 4 hours; after the reaction is completed, dilute hydrochloric acid is added to adjust the pH to neutral, followed by adding 0.02 parts of neutral protease, and enzymolysis is performed at 27° C. for 1.5 hours. After the enzymolysis is completed, sterilization is performed to obtain the white wine lees enzymatic hydrolyzate.
[0028] The preparation method of the modified filler is: (1) mixing aluminum oxide, zinc oxide and carbon nanotubes to obtain a filler; (2) A filler, a 60 wt% ethanol aqueous solution, and a silane coupling agent KH550 were mixed in a mass ratio of 1:6:0.02, stirred at 60°C for 2 h, and the solid was filtered, washed, and dried to obtain a modified filler.
[0029] The filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1:1.3:0.4.
[0030] The alumina particle size is 1-10 μm and the specific surface area is 3-6 m 2 / g.
[0031] The particle size of zinc oxide is 30-50nm and the specific surface area is 15-30m 2 / g.
[0032] The diameter of carbon nanotubes is 2-4nm, the length is 40-60μm, and the specific surface area is 400-600m 2 / g.
[0033] The method for preparing the degradable pulp molded product comprises the following steps: S1. The waste coated paper is crushed, soaked, pulped and filtered to obtain a residue, which is then washed to prepare a waste paper pulp suspension; S2. After bleaching the waste paper pulp suspension, send it to a pulping tank, add cellulose and white wine lees enzymatic hydrolyzate, add a retention agent, stir evenly, then add a modified filler, and obtain a primary pulp after stirring; S3. The primary slurry is uniformly adsorbed on the lower mold of the molding mold by negative pressure, and immersed in a waterproofing agent solution for 22 minutes, and then molded with the upper mold of the molding mold, and the pulp molding wet blank is obtained after the mold is opened; S4. Dry the wet pulp molding to a moisture content of 3%, put it into a mold for compression molding, and obtain a degradable pulp molding product.
[0034] Example 3 The present embodiment provides a degradable pulp molded product, comprising the following raw materials in parts by weight: 55 parts of waste pulp suspension, 30 parts of cellulose, 15 parts of white wine lees enzymatic hydrolyzate, 10 parts of modified filler, 7 parts of waterproofing agent, 0.07 parts of retention aid, and 2 parts of bleaching agent.
[0035] The cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1: 0.7: 1.8.
[0036] The preparation method of the white wine lees enzymatic hydrolyzate is as follows: by weight, 1 part of white wine lees is added to 10 parts of deionized water, and then 0.4 parts of sodium hydroxide is added, and the mixture is stirred and reacted at 60° C. for 5 hours; after the reaction is completed, dilute hydrochloric acid is added to adjust the pH to neutral, and then 0.02 parts of neutral protease are added, and enzymolysis is performed at 30° C. for 2 hours. After the enzymolysis is completed, the mixture is sterilized to obtain the white wine lees enzymatic hydrolyzate.
[0037] The preparation method of the modified filler is: (1) mixing aluminum oxide, zinc oxide and carbon nanotubes to obtain a filler; (2) A filler, a 60-65 wt% ethanol aqueous solution, and a silane coupling agent KH550 were mixed in a mass ratio of 1:8:0.03, stirred at 65°C for 4 hours, filtered to obtain a solid, washed, and dried to obtain a modified filler.
[0038] The filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1: 1.5: 0.8.
[0039] The alumina particle size is 1-10 μm and the specific surface area is 3-6 m 2 / g.
[0040] The particle size of zinc oxide is 30-50nm and the specific surface area is 15-30m 2 / g.
[0041] The diameter of carbon nanotubes is 2-4nm, the length is 40-60μm, and the specific surface area is 400-600m 2 / g.
[0042] The method for preparing the degradable pulp molded product comprises the following steps: S1. The waste coated paper is crushed, soaked, pulped and filtered to obtain a residue, which is then washed to prepare a waste paper pulp suspension; S2. After bleaching the waste paper pulp suspension, send it to a pulping tank, add cellulose and white wine lees enzymatic hydrolyzate, add a retention agent, stir evenly, then add a modified filler, and obtain a primary pulp after stirring; S3. The primary slurry is uniformly adsorbed on the lower mold of the molding mold by negative pressure, and immersed in a waterproofing agent solution for 25 minutes, and then molded with the upper mold of the molding mold, and the pulp molding wet blank is obtained after the mold is opened; S4. Dry the wet pulp molding to a moisture content of 5%, put it into a mold for compression molding, and obtain a degradable pulp molding product.
[0043] Comparative Example 1 The difference between this comparative example and Example 1 is that the proportions of waste paper pulp suspension and cellulose are different. A degradable pulp molded product comprises the following raw materials in parts by weight: 45 parts of waste pulp suspension, 34 parts of cellulose, 13 parts of white wine lees enzymatic hydrolyzate, 8 parts of modified filler, 6 parts of waterproofing agent, 0.04 parts of retention aid, and 1.5 parts of bleaching agent.
[0044] The cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1:0.5:1.6.
[0045] The preparation method of the white wine lees enzymatic hydrolyzate is as follows: by weight, 1 part of white wine lees is added to 9 parts of deionized water, followed by adding 0.3 parts of sodium hydroxide, and reacting at 57° C. with stirring for 4-5 hours; after the reaction is completed, dilute hydrochloric acid is added to adjust the pH to neutral, followed by adding 0.02 parts of neutral protease, and enzymolysis is performed at 28° C. for 1.7 hours. After the enzymolysis is completed, sterilization is performed to obtain the white wine lees enzymatic hydrolyzate.
[0046] The preparation method of the modified filler is: (1) mixing aluminum oxide, zinc oxide and carbon nanotubes to obtain a filler; (2) A filler, a 63 wt % ethanol aqueous solution, and a silane coupling agent KH550 were mixed in a mass ratio of 1:7:0.02, stirred at 62° C. for 3 h, and the solid was filtered, washed, and dried to obtain a modified filler.
[0047] The filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1:1.4:0.6.
[0048] The alumina particle size is 1-10 μm and the specific surface area is 3-6 m 2 / g.
[0049] The particle size of zinc oxide is 30-50nm and the specific surface area is 15-30m 2 / g.
[0050] The diameter of carbon nanotubes is 2-4nm, the length is 40-60μm, and the specific surface area is 400-600m 2 / g.
[0051] The method for preparing the degradable pulp molded product comprises the following steps: S1. The waste coated paper is crushed, soaked, pulped and filtered to obtain a residue, which is then washed to prepare a waste paper pulp suspension; S2. After bleaching the waste paper pulp suspension, send it to a pulping tank, add cellulose and white wine lees enzymatic hydrolyzate, add a retention agent, stir evenly, then add a modified filler, and obtain a primary pulp after stirring; S3. The primary slurry is uniformly adsorbed on the lower mold of the molding mold by negative pressure, and immersed in a waterproofing agent solution for 23 minutes, and then molded with the upper mold of the molding mold, and the pulp molding wet blank is obtained after the mold is opened; S4. Dry the wet pulp molding to a moisture content of 4%, put it into a mold for compression molding, and obtain a degradable pulp molding product.
[0052] Comparative Example 2 The difference between this comparative example and Example 1 is that the waste paper pulp suspension and the white wine lees enzymatic hydrolyzate are different in the amounts.
[0053] A degradable pulp molded product comprises the following raw materials in parts by mass: 45 parts of waste pulp suspension, 27 parts of cellulose, 20 parts of white wine lees enzymatic hydrolyzate, 8 parts of modified filler, 6 parts of waterproofing agent, 0.04 parts of retention aid and 1.5 parts of bleaching agent.
[0054] The cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1:0.5:1.6.
[0055] The preparation method of the white wine lees enzymatic hydrolyzate is as follows: by weight, 1 part of white wine lees is added to 9 parts of deionized water, followed by adding 0.3 parts of sodium hydroxide, and reacting at 57° C. with stirring for 4-5 hours; after the reaction is completed, dilute hydrochloric acid is added to adjust the pH to neutral, followed by adding 0.02 parts of neutral protease, and enzymolysis is performed at 28° C. for 1.7 hours. After the enzymolysis is completed, sterilization is performed to obtain the white wine lees enzymatic hydrolyzate.
[0056] The preparation method of the modified filler is: (1) mixing aluminum oxide, zinc oxide and carbon nanotubes to obtain a filler; (2) A filler, a 63 wt % ethanol aqueous solution, and a silane coupling agent KH550 were mixed in a mass ratio of 1:7:0.02, stirred at 62° C. for 3 h, and the solid was filtered, washed, and dried to obtain a modified filler.
[0057] The filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1:1.4:0.6.
[0058] The alumina particle size is 1-10 μm and the specific surface area is 3-6 m 2 / g.
[0059] The particle size of zinc oxide is 30-50nm and the specific surface area is 15-30m 2 / g.
[0060] The diameter of carbon nanotubes is 2-4nm, the length is 40-60μm, and the specific surface area is 400-600m 2 / g.
[0061] The method for preparing the degradable pulp molded product comprises the following steps: S1. The waste coated paper is crushed, soaked, pulped and filtered to obtain a residue, which is then washed to prepare a waste paper pulp suspension; S2. After bleaching the waste paper pulp suspension, send it to a pulping tank, add cellulose and white wine lees enzymatic hydrolyzate, add a retention agent, stir evenly, then add a modified filler, and obtain a primary pulp after stirring; S3. The primary slurry is uniformly adsorbed on the lower mold of the molding mold by negative pressure, and immersed in a waterproofing agent solution for 23 minutes, and then molded with the upper mold of the molding mold, and the pulp molding wet blank is obtained after the mold is opened; S4. Dry the wet pulp molding to a moisture content of 4%, put it into a mold for compression molding, and obtain a degradable pulp molding product.
[0062] Comparative Example 3 The difference between this comparative example and Example 1 is that the portions of cellulose and white wine lees enzymatic hydrolysate are different.
[0063] A degradable pulp molded product comprises the following raw materials in parts by weight: 52 parts of waste pulp suspension, 20 parts of cellulose, 20 parts of white wine lees enzymatic hydrolyzate, 8 parts of modified filler, 6 parts of waterproofing agent, 0.04 parts of retention aid, and 1.5 parts of bleaching agent.
[0064] The cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1:0.5:1.6.
[0065] The preparation method of the white wine lees enzymatic hydrolyzate is as follows: by weight, 1 part of white wine lees is added to 9 parts of deionized water, followed by adding 0.3 parts of sodium hydroxide, and reacting at 57° C. with stirring for 4-5 hours; after the reaction is completed, dilute hydrochloric acid is added to adjust the pH to neutral, followed by adding 0.02 parts of neutral protease, and enzymolysis is performed at 28° C. for 1.7 hours. After the enzymolysis is completed, sterilization is performed to obtain the white wine lees enzymatic hydrolyzate.
[0066] The preparation method of the modified filler is: (1) mixing aluminum oxide, zinc oxide and carbon nanotubes to obtain a filler; (2) A filler, a 63 wt % ethanol aqueous solution, and a silane coupling agent KH550 were mixed in a mass ratio of 1:7:0.02, stirred at 62° C. for 3 h, and the solid was filtered, washed, and dried to obtain a modified filler.
[0067] The filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1:1.4:0.6.
[0068] The alumina particle size is 1-10 μm and the specific surface area is 3-6 m 2 / g.
[0069] The particle size of zinc oxide is 30-50nm and the specific surface area is 15-30m 2 / g.
[0070] The diameter of carbon nanotubes is 2-4nm, the length is 40-60μm, and the specific surface area is 400-600m 2 / g.
[0071] The method for preparing the degradable pulp molded product comprises the following steps: S1. The waste coated paper is crushed, soaked, pulped and filtered to obtain a residue, which is then washed to prepare a waste paper pulp suspension; S2. After bleaching the waste paper pulp suspension, send it to a pulping tank, add cellulose and white wine lees enzymatic hydrolyzate, add a retention agent, stir evenly, then add a modified filler, and obtain a primary pulp after stirring; S3. The primary slurry is uniformly adsorbed on the lower mold of the molding mold by negative pressure, and immersed in a waterproofing agent solution for 23 minutes, and then molded with the upper mold of the molding mold, and the pulp molding wet blank is obtained after the mold is opened; S4. Dry the wet pulp molding to a moisture content of 4%, put it into a mold for compression molding, and obtain a degradable pulp molding product.
[0072] Comparative Example 4 The difference between this comparative example and Example 1 is that the filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1:1:1. A degradable pulp molded product comprises the following raw materials in parts by weight: 52 parts of waste pulp suspension, 27 parts of cellulose, 13 parts of white wine lees enzymatic hydrolyzate, 8 parts of modified filler, 6 parts of waterproofing agent, 0.04 parts of retention aid, and 1.5 parts of bleaching agent.
[0073] The cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1:0.5:1.6.
[0074] The preparation method of the white wine lees enzymatic hydrolyzate is as follows: by weight, 1 part of white wine lees is added to 9 parts of deionized water, followed by adding 0.3 parts of sodium hydroxide, and reacting at 57° C. with stirring for 4-5 hours; after the reaction is completed, dilute hydrochloric acid is added to adjust the pH to neutral, followed by adding 0.02 parts of neutral protease, and enzymolysis is performed at 28° C. for 1.7 hours. After the enzymolysis is completed, sterilization is performed to obtain the white wine lees enzymatic hydrolyzate.
[0075] The preparation method of the modified filler is: (1) mixing aluminum oxide, zinc oxide and carbon nanotubes to obtain a filler; (2) A filler, a 63 wt % ethanol aqueous solution, and a silane coupling agent KH550 were mixed in a mass ratio of 1:7:0.02, stirred at 62° C. for 3 h, and the solid was filtered, washed, and dried to obtain a modified filler.
[0076] The filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1:1:1.
[0077] The alumina particle size is 1-10 μm and the specific surface area is 3-6 m 2 / g.
[0078] The particle size of zinc oxide is 30-50nm and the specific surface area is 15-30m 2 / g.
[0079] The diameter of carbon nanotubes is 2-4nm, the length is 40-60μm, and the specific surface area is 400-600m 2 / g.
[0080] The method for preparing the degradable pulp molded product comprises the following steps: S1. The waste coated paper is crushed, soaked, pulped and filtered to obtain a residue, which is then washed to prepare a waste paper pulp suspension; S2. After bleaching the waste paper pulp suspension, send it to a pulping tank, add cellulose and white wine lees enzymatic hydrolyzate, add a retention agent, stir evenly, then add a modified filler, and obtain a primary pulp after stirring; S3. The primary slurry is uniformly adsorbed on the lower mold of the molding mold by negative pressure, and immersed in a waterproofing agent solution for 23 minutes, and then molded with the upper mold of the molding mold, and the pulp molding wet blank is obtained after the mold is opened; S4. Dry the wet pulp molding to a moisture content of 4%, put it into a mold for compression molding, and obtain a degradable pulp molding product.
[0081] Comparative Example 5 The difference between this comparative example and Example 1 is that the cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1:1:1.
[0082] A degradable pulp molded product comprises the following raw materials in parts by weight: 52 parts of waste pulp suspension, 27 parts of cellulose, 13 parts of white wine lees enzymatic hydrolyzate, 8 parts of modified filler, 6 parts of waterproofing agent, 0.04 parts of retention aid, and 1.5 parts of bleaching agent.
[0083] The cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1:1:1.
[0084] The preparation method of the white wine lees enzymatic hydrolyzate is as follows: by weight, 1 part of white wine lees is added to 9 parts of deionized water, followed by adding 0.3 parts of sodium hydroxide, and reacting at 57° C. with stirring for 4-5 hours; after the reaction is completed, dilute hydrochloric acid is added to adjust the pH to neutral, followed by adding 0.02 parts of neutral protease, and enzymolysis is performed at 28° C. for 1.7 hours. After the enzymolysis is completed, sterilization is performed to obtain the white wine lees enzymatic hydrolyzate.
[0085] The preparation method of the modified filler is: (1) mixing aluminum oxide, zinc oxide and carbon nanotubes to obtain a filler; (2) A filler, a 63 wt % ethanol aqueous solution, and a silane coupling agent KH550 were mixed in a mass ratio of 1:7:0.02, stirred at 62° C. for 3 h, and the solid was filtered, washed, and dried to obtain a modified filler.
[0086] The filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1:1.4:0.6.
[0087] The alumina particle size is 1-10 μm and the specific surface area is 3-6 m 2 / g.
[0088] The particle size of zinc oxide is 30-50nm and the specific surface area is 15-30m 2 / g.
[0089] The diameter of carbon nanotubes is 2-4nm, the length is 40-60μm, and the specific surface area is 400-600m 2 / g.
[0090] The method for preparing the degradable pulp molded product comprises the following steps: S1. The waste coated paper is crushed, soaked, pulped and filtered to obtain a residue, which is then washed to prepare a waste paper pulp suspension; S2. After bleaching the waste paper pulp suspension, send it to a pulping tank, add cellulose and white wine lees enzymatic hydrolyzate, add a retention agent, stir evenly, then add a modified filler, and obtain a primary pulp after stirring; S3. The primary slurry is uniformly adsorbed on the lower mold of the molding mold by negative pressure, and immersed in a waterproofing agent solution for 23 minutes, and then molded with the upper mold of the molding mold, and the pulp molding wet blank is obtained after the mold is opened; S4. Dry the wet pulp molding to a moisture content of 4%, put it into a mold for compression molding, and obtain a degradable pulp molding product.
[0091] Performance Testing The pulp molded products prepared in Examples 1-3 and Comparative Examples 1-5 were subjected to performance tests. The dry tensile strength was tested according to GB / T12914-2018 "Determination of tensile strength of paper and paperboard - Constant rate stretching method", the sampling direction was longitudinal, the sample size was 250 mm × 15 mm, the stretching speed was 20 mm / min, and the samples were placed in an environment with a temperature of 23 ° C and a relative humidity of 50% for 24 hours before the test; the tear strength was tested according to the national standard GB / T455-2002 " Determination of tear strength of paper and paperboard", use a paper tearing tester to measure the tear strength of paper; Determination of water absorption: put a 50mm×50mm sample into a 50℃ oven for 24 hours, take it out, and weigh its mass m1. Then soak the sample in 30℃ tap water prepared in advance, take it out after 24 hours, dry it naturally, and gently wipe the water at the bottom of the sample with filter paper, weigh its mass m2, and calculate its water absorption, water absorption = (m2-m1) / m1×100%; the test results are shown in Table 1 below: Table 1 Performance test results
[0092] The results show that the products of Examples 1-3 have excellent comprehensive performance, especially Example 1 has the most outstanding comprehensive performance, which is mainly due to the good synergistic effect between the components.
[0093] However, the comparative example does not adopt the necessary technical solution, resulting in its performance being significantly worse than that of the embodiment in the corresponding performance test. The above experimental results further prove the importance of the technical solution defined in the present invention to its technical effect.
[0094] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A biodegradable pulp molded product, It is characterized in that The invention comprises the following raw materials in parts by weight: 50-55 parts of waste paper pulp suspension, 25-30 parts of cellulose, 10-15 parts of white wine lees enzymatic hydrolyzate, 6-10 parts of modified filler, 5-7 parts of waterproofing agent, 0.03-0.07 parts of retention aid and 1-2 parts of bleaching agent.
2. The degradable pulp molded product according to claim 1, It is characterized in that The cellulose is selected from one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether.
3. The degradable pulp molded product according to claim 2, It is characterized in that The cellulose is a mixture of carboxymethyl cellulose, hydroxypropyl methyl cellulose and cellulose ether in a mass ratio of 1:0.3-0.7:1.4-1.
8.
4. The degradable pulp molded product according to claim 1, It is characterized in that The preparation method of the white wine lees enzymatic hydrolyzate is as follows: by weight, 1 part of white wine lees is added to 8-10 parts of deionized water, followed by adding 0.2-0.4 parts of sodium hydroxide, and reacting by stirring at 55-60° C. for 4-5 hours; after the reaction is completed, dilute hydrochloric acid is added to adjust the pH to neutral, followed by adding 0.02 parts of neutral protease, and enzymolysis is performed at 27-30° C. for 1.5-2 hours. After the enzymolysis is completed, sterilization is performed to obtain the white wine lees enzymatic hydrolyzate.
5. The degradable pulp molded product according to claim 1, It is characterized in that The preparation method of the modified filler is: (1) mixing aluminum oxide, zinc oxide and carbon nanotubes to obtain a filler; (2) Mix filler, 60-65wt% ethanol aqueous solution and silane coupling agent KH550 in a mass ratio of 1:6-8:0.02-0.03, stir and react at 60-65°C for 2-4h, filter and obtain a solid, wash and dry to obtain a modified filler.
6. The degradable pulp molded product according to claim 5, It is characterized in that The filler is a composite of aluminum oxide, zinc oxide and carbon nanotubes in a mass ratio of 1:1.3-1.5:0.4-0.
8.
7. The degradable pulp molded product according to claim 6, It is characterized in that The alumina particle size is 1-10 μm and the specific surface area is 3-6 m 2 / g.
8. The degradable pulp molded product according to claim 6, It is characterized in that The particle size of zinc oxide is 30-50nm and the specific surface area is 15-30m 2 / g.
9. The degradable pulp molded product according to claim 6, It is characterized in that The diameter of carbon nanotubes is 2-4nm, the length is 40-60μm, and the specific surface area is 400-600m 2 / g.
10. A method for preparing the degradable pulp molded product according to any one of claims 1 to 9, It is characterized in that The following steps are involved: S1. The waste coated paper is crushed, soaked, pulped and filtered to obtain a residue, which is then washed to prepare a waste paper pulp suspension; S2. After bleaching the waste paper pulp suspension, send it to a pulping tank, add cellulose and white wine lees enzymatic hydrolyzate, add a retention agent, stir evenly, then add a modified filler, and obtain a primary pulp after stirring; S3. The primary slurry is uniformly adsorbed on the lower mold of the molding mold by negative pressure, and immersed in a waterproofing agent solution for 22-25min, and then molded with the upper mold of the molding mold, and the pulp molding wet blank is obtained after the mold is opened; S4. Dry the wet pulp molding to a moisture content of 3-5%, put it into a mold for compression molding, and obtain a degradable pulp molding product.
Citation Information
Patent Citations
Nano modified paper based on surface modification and preparation method thereof
CN105696408A
Reinforcement method for pulp molding product with PLA
CN109137599A
Waterproof paper pulp molding material with high compressive strength and preparation method thereof
CN112962356A
Paper pulp molding material prepared from vinasse biomass and preparation method of paper pulp molding material
CN116905287A