Method, medium and device for measuring volume change of rubber material after hydrogen absorption

By obtaining the initial volume and diffusion coefficient of the rubber sample, performing time measurements while standing and rapidly decompression, the expansion rate of the hydrogen absorption saturation volume is calculated based on the fitting relationship, and the volume after hydrogen absorption of rubber materials in the prior art is solved. The problem of calculating the expansion rate is improved by improving measurement accuracy and safety.

CN118883918APending Publication Date: 2024-11-01ZHEJIANG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410899065.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, there are large errors in the calculation of the volume expansion rate of rubber materials after hydrogen absorption, resulting in inaccurate detection results, affecting its service life and safety in high-pressure hydrogen systems.

Method used

By obtaining the initial volume and diffusion coefficient of the rubber sample, performing time measurements while standing and rapidly decompressing, the expansion rate of the hydrogen absorbing saturation volume is calculated based on the fitting relationship between the diffusion coefficient and the compensation coefficient, and reducing the calculation error.

Benefits of technology

It improves the accuracy of measuring volume change of rubber material after hydrogen absorption, reduces detection errors, and ensures the safety and reliability of rubber material in high-pressure hydrogen systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118883918A_ABST
    Figure CN118883918A_ABST
Patent Text Reader

Abstract

The invention discloses a method, medium and device for measuring the volume change of a rubber material after hydrogen absorption. The method comprises the following steps: acquiring the initial volume and diffusion coefficient of a rubber sample to be measured; carrying out standing hydrogen absorption on the to-be-tested rubber sample in the test container, and after the standing hydrogen absorption duration reaches a first preset duration, carrying out rapid hydrogen pressure reduction on the test container; timing after the rapid pressure reduction of the hydrogen is completed, and measuring the to-be-measured rubber sample when the timing reaches a second preset duration, so as to obtain a first volume of the to-be-measured rubber sample after hydrogen absorption; calculating a corresponding compensation coefficient based on a fitting relationship between the diffusion coefficient and the compensation coefficient according to the diffusion coefficient of the to-be-tested rubber sample, and calculating the hydrogen absorption saturation volume expansion rate of the to-be-tested rubber sample according to the compensation coefficient and the first volume after hydrogen absorption; the calculation error of the hydrogen absorption saturation volume expansion rate in the detection process after the rubber material absorbs hydrogen can be reduced, and the accuracy of a final measurement result is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of material inspection, and in particular to a method, medium and device for measuring the volume change of a rubber material after hydrogen absorption. Background Art

[0002] Rubber materials are widely used in high-pressure hydrogen systems, such as high-pressure hydrogen storage containers, valves, sealing parts of hydrogen compressors, rubber hoses and pipes for transporting hydrogen, vibration dampeners, etc. After hydrogen comes into contact with rubber materials, it dissolves into the rubber materials, causing the rubber materials to expand and increase in volume significantly. After the rubber materials absorb hydrogen and expand, the internal molecular structure changes, and the mechanical properties deteriorate. This change may cause the rubber material to become more fragile and lose its original elasticity and toughness, thereby shortening its service life in the high-pressure hydrogen system and increasing the risk of leakage or failure in the system. Therefore, accurately measuring the expansion coefficient can help us predict the behavior of rubber materials in practical applications and ensure their safety and reliability in key areas such as hydrogen storage and transportation.

[0003] In the related art, when testing the properties of rubber materials after hydrogen absorption, most of them directly calculate the ratio of the difference between the initial volume and the volume after the test of the rubber material to be tested and the initial volume, and use the ratio as the hydrogen absorption saturation volume expansion rate of the rubber. It can be understood that in the process of hydrogen absorption test of rubber, after the rubber completes hydrogen absorption, it is necessary to reduce the hydrogen pressure in the test container; and it takes a certain amount of time (generally about 15 minutes) from the start of reducing the hydrogen pressure to the completion of the volume measurement after the test; the hydrogen diffusion coefficient of different rubber materials can differ by 2 orders of magnitude. Therefore, there is a large error in calculating the hydrogen absorption saturation volume expansion rate of the rubber in the above manner, resulting in inaccurate final test results. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, one purpose of the present invention is to provide a method for measuring the volume change of a rubber material after hydrogen absorption, which can reduce the calculation error of the hydrogen absorption saturation volume expansion rate during the detection process of the rubber material after hydrogen absorption and improve the accuracy of the final measurement result.

[0005] In a first aspect, an embodiment of the present invention provides a method for measuring the volume change of a rubber material after hydrogen absorption, comprising the following steps: obtaining an initial volume and a diffusion coefficient of a rubber sample to be tested; allowing the rubber sample to be tested to absorb hydrogen in a test container, and after the standing hydrogen absorption time reaches a first preset time, rapidly decompressing the test container with hydrogen; timing after the rapid hydrogen decompression is completed, and when the timing reaches a second preset time, measuring the rubber sample to be tested to obtain a first volume of the rubber sample to be tested after hydrogen absorption; based on a fitting relationship between the diffusion coefficient and the compensation coefficient, calculating a corresponding compensation coefficient according to the diffusion coefficient of the rubber sample to be tested, and calculating the hydrogen absorption saturated volume expansion rate of the rubber sample to be tested according to the compensation coefficient and the first volume after hydrogen absorption.

[0006] According to the method for measuring the volume change of a rubber material after hydrogen absorption of an embodiment of the present invention, first, the initial volume and diffusion coefficient of the rubber sample to be tested are obtained; then, the rubber sample to be tested is allowed to stand in a test container to absorb hydrogen, and after the standing hydrogen absorption time reaches a first preset time, the test container is rapidly decompressed by hydrogen; then, timing is performed after the rapid hydrogen decompression is completed, and when the timing reaches a second preset time, the rubber sample to be tested is measured to obtain the first volume of the rubber sample to be tested after hydrogen absorption; then, based on the fitting relationship between the diffusion coefficient and the compensation coefficient, the corresponding compensation coefficient is calculated according to the diffusion coefficient of the rubber sample to be tested, and the hydrogen absorption saturated volume expansion rate of the rubber sample to be tested is calculated according to the compensation coefficient and the first volume after hydrogen absorption. In this way, the calculation error of the hydrogen absorption saturated volume expansion rate in the process of detecting the rubber material after hydrogen absorption is reduced, and the accuracy of the final measurement result is improved.

[0007] In some embodiments, the measurement method further includes: calculating the corresponding permanent volume change time according to the diffusion coefficient of the rubber sample to be tested based on the fitting relationship between the diffusion coefficient and the permanent volume change time, and measuring the rubber sample to be tested according to the permanent volume change time to obtain a second volume of the rubber sample to be tested after hydrogen absorption; and calculating the permanent volume change rate of the rubber sample to be tested according to the first volume after hydrogen absorption and the second volume after hydrogen absorption.

[0008] In some embodiments, the compensation coefficient is calculated by the following formula:

[0009]

[0010] Where ξ represents the compensation coefficient, and D represents the diffusion coefficient of the rubber sample to be tested.

[0011] In some embodiments, the hydrogen absorption saturation volume expansion rate is calculated by the following formula:

[0012] V R1 =ξ×V R2

[0013] V R2 =(V2-V0) / V0

[0014] Among them, V R1 represents the volume expansion rate of hydrogen absorption saturation, V0 represents the initial volume, V2 represents the volume after the first hydrogen absorption, V R2 It represents the volume expansion rate corresponding to the volume after the first hydrogen absorption.

[0015] In some embodiments, the permanent volume change time is calculated by the following formula:

[0016]

[0017] Wherein, t represents the permanent volume change time, and D represents the diffusion coefficient of the rubber sample to be tested.

[0018] In some embodiments, the compensation coefficient is calculated by a two-dimensional non-steady finite boundary diffusion model.

[0019] In some embodiments, the diffusion coefficient ranges from 1×10 -10 m 2 / s to 1×10 -8 m 2 / s.

[0020] In a second aspect, an embodiment of the present invention provides a computer-readable storage medium on which a program for measuring the volume change of a rubber material after hydrogen absorption is stored. When the program for measuring the volume change of a rubber material after hydrogen absorption is executed by a processor, the method for measuring the volume change of a rubber material after hydrogen absorption as described above is implemented.

[0021] According to the computer-readable storage medium of the embodiment of the present invention, by storing a volume change measurement program of a rubber material after hydrogen absorption, the processor implements the volume change measurement method of a rubber material after hydrogen absorption when executing the volume change measurement program of a rubber material after hydrogen absorption; thereby reducing the calculation error of the hydrogen absorption saturation volume expansion rate in the detection process of the rubber material after hydrogen absorption, and improving the accuracy of the final measurement result.

[0022] In a third aspect, an embodiment of the present invention provides a device for measuring the volume change of a rubber material after hydrogen absorption, comprising: an acquisition module, the acquisition module being used to acquire the initial volume and diffusion coefficient of a rubber sample to be tested; a test module, the test module being used to statically absorb hydrogen on the rubber sample to be tested in a test container, and to rapidly decompress the test container with hydrogen after the static hydrogen absorption time reaches a first preset time; a measurement module, the measurement module being used to time after the rapid hydrogen decompression is completed, and to measure the rubber sample to be tested when the timing reaches a second preset time to obtain a first volume of the rubber sample to be tested after hydrogen absorption; a calculation module, the calculation module being used to calculate a corresponding compensation coefficient according to the diffusion coefficient of the rubber sample to be tested based on a fitting relationship between the diffusion coefficient and the compensation coefficient, and to calculate the hydrogen absorption saturated volume expansion rate of the rubber sample to be tested according to the compensation coefficient and the first volume after hydrogen absorption.

[0023] According to the apparatus for measuring the volume change of a rubber material after hydrogen absorption of an embodiment of the present invention, a test module is provided for allowing the rubber sample to be statically absorbed with hydrogen in a test container, and after the static hydrogen absorption time reaches a first preset time, the test container is rapidly decompressed with hydrogen; a measuring module is used for timing after the rapid hydrogen decompression is completed, and when the timing reaches a second preset time, the rubber sample to be tested is measured to obtain a first volume of the rubber sample after hydrogen absorption; a calculation module is used for calculating a corresponding compensation coefficient according to the diffusion coefficient of the rubber sample to be tested based on a fitting relationship between the diffusion coefficient and the compensation coefficient, and calculating the hydrogen absorption saturated volume expansion rate of the rubber sample to be tested according to the compensation coefficient and the first volume after hydrogen absorption; thereby reducing the calculation error of the hydrogen absorption saturated volume expansion rate in the detection process of the rubber material after hydrogen absorption, and improving the accuracy of the final measurement result.

[0024] In some embodiments, the calculation module is further used to calculate the corresponding permanent volume change time according to the diffusion coefficient of the rubber sample to be tested based on the fitting relationship between the diffusion coefficient and the permanent volume change time; the measurement module is further used to measure the rubber sample to be tested according to the permanent volume change time to obtain the second volume of the rubber sample to be tested after hydrogen absorption, and calculate the permanent volume change rate of the rubber sample to be tested according to the first volume after hydrogen absorption and the second volume after hydrogen absorption.

[0025] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a flow chart of a method for measuring volume change of a rubber material after hydrogen absorption according to an embodiment of the present invention;

[0027] Figure 2 4 is a block diagram of a device for measuring volume change of a rubber material after hydrogen absorption according to an embodiment of the present invention. DETAILED DESCRIPTION

[0028] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0029] The following describes a method for measuring the volume change of a rubber material after hydrogen absorption according to an embodiment of the present invention with reference to the accompanying drawings.

[0030] See also Figure 1 , Figure 1 FIG. 1 is a flow chart of a method for measuring volume change of a rubber material after hydrogen absorption according to an embodiment of the present invention. Figure 1 As shown, the method for measuring the volume change of the rubber material after hydrogen absorption comprises the following steps:

[0031] S101, obtaining the initial volume and diffusion coefficient of the rubber sample to be tested.

[0032] That is, the rubber sample to be tested is first measured to obtain the initial volume of the rubber sample to be tested, and the corresponding diffusion coefficient is obtained by means of a hydrogen permeation test of the rubber material or by querying the material properties of the rubber sample to be tested.

[0033] S102, allowing the rubber sample to absorb hydrogen in a test container, and after the hydrogen absorption time reaches a first preset time, rapidly decompressing the hydrogen in the test container.

[0034] S103, timing is performed after the rapid decompression of hydrogen is completed, and when the timing reaches a second preset time, the rubber sample to be tested is measured to obtain a first volume of the rubber sample to be tested after hydrogen absorption.

[0035] That is, a hydrogen absorption test is performed on the rubber sample to be tested in a test container; and the first volume after hydrogen absorption of the rubber sample to be tested is measured after the test result.

[0036] As an example, first, a test container that meets the test pressure requirements and the test temperature requirements is used, and the rubber sample to be tested is placed in the container; then, a gas replacement procedure is performed to make the pressure in the test container reach the target test pressure and temperature; then, the test container is allowed to stand for a first preset time (the first preset time can be adjusted as needed, preferably, the first preset time is 24 hours); then, the test container is rapidly decompressed with hydrogen, and the hydrogen pressure in the test container is reduced to below 1 MPa within 10 seconds; then, after completing the gas replacement procedure, the test container is opened to take out the rubber sample to be tested, and the rubber sample to be tested is measured 15 minutes after the decompression is completed to obtain the first volume after hydrogen absorption.

[0037] S104, calculating a corresponding compensation coefficient according to the diffusion coefficient of the rubber sample to be tested based on a fitting relationship between the diffusion coefficient and the compensation coefficient, and calculating the hydrogen absorption saturated volume expansion rate of the rubber sample to be tested according to the compensation coefficient and the volume after the first hydrogen absorption.

[0038] In some embodiments, the compensation coefficient is calculated by the following formula:

[0039]

[0040] Where ξ represents the compensation coefficient, and D represents the diffusion coefficient of the rubber sample to be tested.

[0041] In some embodiments, the hydrogen absorption saturation volume expansion rate is calculated by the following formula:

[0042] V R1 =ξ×V R2

[0043] V R2 =(V2-V0) / V0

[0044] Among them, V R1 represents the volume expansion rate of hydrogen absorption saturation, V0 represents the initial volume, V2 represents the volume after the first hydrogen absorption, V R2 It represents the volume expansion rate corresponding to the volume after the first hydrogen absorption.

[0045] In some embodiments, the compensation coefficient is calculated using a two-dimensional non-steady finite boundary diffusion model.

[0046] In some embodiments, the two-dimensional non-steady finite boundary diffusion model is expressed by the following formula:

[0047]

[0048] The initial conditions of the two-dimensional unsteady finite boundary diffusion model are:

[0049]

[0050] The boundary conditions of the two-dimensional unsteady finite boundary diffusion model are:

[0051]

[0052] Wherein, c represents the hydrogen concentration in the rubber sample to be tested, c1 represents the hydrogen concentration inside the rubber sample to be tested when the hydrogen absorption is saturated, t represents the decompression time, D represents the diffusion coefficient, x represents the horizontal coordinate of a certain position in the rubber sample to be tested, and y represents the vertical coordinate of a certain position in the rubber sample to be tested.

[0053] In some embodiments, the diffusion coefficient ranges from 1×10 -10 m 2 / s to 1×10 -8 m 2 / s.

[0054] As an example, the transmission of hydrogen in rubber can be expressed by Fick's law. Fick's second law represents the non-steady-state diffusion of gas in solid. When the rubber sample to be tested is placed in a hydrogen environment, the initial hydrogen concentration inside is 0, and increases with time until the hydrogen concentration inside the rubber sample to be tested reaches a stable state, that is, hydrogen absorption saturation. It is assumed that the hydrogen concentration inside the rubber sample to be tested is c1 at this time. At this time, the volume of the rubber sample to be tested will expand due to the dissolved hydrogen. When the pressure is reduced, hydrogen will precipitate. It is assumed that the volume of the rubber sample to be tested after hydrogen absorption saturation is V1. The rubber sample to be tested is then taken out. The hydrogen concentration at the boundary of the rubber sample to be tested is 0, and hydrogen diffuses outward. The concentration gradient of hydrogen in the rubber sample to be tested changes with time. It should be noted that the rubber sample to be tested adopts a Φ13mm×2mm disc-shaped rubber sample; in this way, the boundary condition in the two-dimensional non-steady-state finite boundary diffusion model is set to -0.001 <x<0.001,-0.0065<y<0.0065。

[0055] Specifically, the two-dimensional unsteady finite boundary diffusion model expression is:

[0056]

[0057] The initial conditions of the two-dimensional unsteady finite boundary diffusion model are:

[0058]

[0059] The boundary conditions of the two-dimensional unsteady finite boundary diffusion model are:

[0060]

[0061] The diffusion coefficient D is in the range of 1×10 -10 m 2 / s to 1×10-8 m 2 / s.

[0062] It is known from the research that the volume expansion rate of rubber V R It is linearly related to the internal hydrogen content W, and the volume expansion rate of the rubber material V R As the decompression time t changes continuously, then:

[0063]

[0064] Where V R1 , W1 is the volume expansion rate and hydrogen content of hydrogen saturated rubber; V R2 W2 is the rubber volume expansion rate and hydrogen content of the rubber sample to be tested measured 15 minutes after the decompression is completed; the rubber volume expansion rate V R =(V-V0) / V0, where V0 is the initial volume of the rubber sample to be tested; the hydrogen content can be replaced by the average concentration in the calculation process, then formula (4) can be written as

[0065]

[0066] In the formula, c1 is the concentration of hydrogen saturation of the rubber sample to be tested, The average concentration of rubber in the rubber sample to be tested 15 minutes after the decompression is completed;

[0067] The software can be used to calculate the average concentration of hydrogen when it diffuses in the rubber sample to be tested. The explicit difference method FTCS is used to solve the model expression (1) and discretize it into a difference equation. Given that the grid points are spaced Δx and Δy and the time step is Δt, the discretized equation is:

[0068]

[0069] The concentration values ​​on all grids are summed and averaged, that is:

[0070]

[0071] Where N x ×N y Number of grids;

[0072] Calculate the hydrogen saturation content or concentration of the rubber sample to be tested and the hydrogen content or average concentration of the rubber sample to be tested 15 minutes after the decompression is completed, and obtain V R2 V R1 The compensation coefficient ξ is used to correct the rubber volume expansion rate V measured 15 minutes after the decompression is completed. R2 , and the hydrogen absorption saturation volume expansion rate V R1 ,Right now:

[0073] V R1 =ξ×V R2 (8)

[0074] According to current standards, rubber hydrogen compatibility tests, including hydrogen exposure, hydrogen damage, hydrogen cycle and other tests, usually measure the volume of the rubber sample within 15 minutes after decompression. R2 V R1 The compensation coefficient ξ is used to obtain the volume expansion rate of the rubber when it absorbs hydrogen. When t = 15 min, substitute into formula (5) to obtain the curve of ξ changing with the rubber diffusion coefficient D. According to the curve, the ExpDec1 model equation y = ae -x / b +c to get the fitting ξ-D relationship:

[0075]

[0076] The determination coefficient R of the fitting ξ-D relationship (9) 2 =1; standard error is 2.43×10 -8 .

[0077] In some embodiments, the measurement method further includes: calculating the corresponding permanent volume change time according to the diffusion coefficient of the rubber sample to be tested based on the fitting relationship between the diffusion coefficient and the permanent volume change time, and measuring the rubber sample to be tested according to the permanent volume change time to obtain a second volume of the rubber sample to be tested after hydrogen absorption; and calculating the permanent volume change rate of the rubber sample to be tested according to the first volume after hydrogen absorption and the second volume after hydrogen absorption.

[0078] In some embodiments, the permanent volume change time is calculated by the following formula:

[0079]

[0080] Wherein, t represents the permanent volume change time, and D represents the diffusion coefficient of the rubber sample to be tested.

[0081] As an example, first, according to the above-mentioned two-dimensional non-steady-state finite boundary diffusion model, the concentration state c3 when the hydrogen is completely released is set as the concentration value corresponding to the rubber volume not changing with the hydrogen content. For the convenience of calculation, the hydrogen concentration c3 at the center of the model at this time is set to one ten-thousandth of the initial concentration, that is, c3=0.0001c1; the software code is used to solve the time t when the internal concentration of the rubber reaches c3, which is the measurement time of the permanent volume change rate of the rubber, in min.

[0082] The curves of different diffusion coefficients D and the corresponding permanent volume change rate measurement time t are calculated cyclically. The condition for the code loop to terminate is c3≤0.0001c1. The curve of diffusion coefficient D and permanent volume change rate measurement time t is obtained. According to the curve, the Allometric1 model equation y=ax b The fitting tD relationship is obtained:

[0083]

[0084] The determination coefficient R of the fitting tD relationship (10) 2 =1, and the standard error is 6.44×10 -8 , the diffusion coefficient D ranges from 1×10 -10 m 2 / s to 1×10 -8 m 2 / s. By fitting the tD relation (10), the time for measuring the permanent volume change rate of different rubber materials after hydrogen exposure, hydrogen damage, hydrogen cycle and other tests can be determined according to the diffusion coefficient of rubber, thereby reducing the impact of rubber diffusion that is too fast or too slow on the results, and streamlining the test process to reduce the waste of human and financial resources.

[0085] At this time, the volume V3 of the rubber sample is measured to obtain the permanent volume change rate V R3 =(V3-V0) / V0.

[0086] As a specific embodiment of the present invention, it is assumed that the rubber sample to be tested is EPDM, a rubber sealing ring material commonly used in 70MPa hydrogenation stations; the diffusion coefficient of this EPDM material is 5.2×10 -10 m 2 / s. First, take a Φ13mm×2mm disc-shaped EPDM sample and measure its volume. The volume of the EPDM sample before the test is V0=2.66×10 -7 m 3 ; Next, hydrogen exposure is performed, that is, a test container that meets the test pressure and temperature requirements is used, the EPDM sample is placed in the test container, and after the gas replacement procedure is completed, the test container is loaded to 1.25 times the nominal working pressure of 87.5MPa at room temperature and left to stand for 24h; then, hydrogen rapid decompression is performed, specifically, the hydrogen pressure in the test container is reduced to below 1MPa within 10 seconds, and after the gas replacement procedure is completed, the test container is opened to take out the EPDM sample; the hydrogen rapid decompression process must be completed within 10s; then, the rubber hydrogen absorption saturation volume expansion rate is measured: the volume of the rubber sample is measured 15min after decompression to obtain V2=3.28×10 -7 m 3 Furthermore, according to the fitting ξ-D relationship, the compensation coefficient of the EPDM sample can be obtained as follows:

[0087]

[0088] At this time, the hydrogen absorption saturation volume expansion rate of the EPDM sample is:

[0089]

[0090] The volume of the EPDM sample immediately after decompression is:

[0091] V1=V R1 ×V0+V0=91.1%×2.66×10 -7 +2.66×10 -7 =5.08×10 -7 m 3

[0092] That is, the volume of the EPDM sample immediately after decompression is 5.08×10 -7 m 3 .

[0093] Thus, the rubber volume expansion rate calculated based on the first hydrogen absorption volume measured 15 minutes after the decompression is completed is:

[0094]

[0095] Therefore, for a diffusion coefficient of 5.2×10 -10 m 2 / s, the actual rubber hydrogen absorption saturation volume expansion rate obtained by the compensation coefficient calculation method is 91.1%, which is nearly 4 times the volume expansion rate of 23.3% at 15 minutes after decompression. This calculation method improves the accuracy of the measurement of the rubber hydrogen absorption saturation volume expansion rate.

[0096] Then, measure the permanent volume change rate of the rubber: determine the time for measuring the permanent volume change rate of the rubber, and the time t for measuring the permanent volume change rate of the EPDM material can be obtained according to the fitting tD relationship:

[0097]

[0098] Therefore, the permanent volume change rate of the EPDM material can be measured about 2 hours after decompression, at which time the hydrogen in the EPDM sample has been completely released.

[0099] As another specific embodiment of the present invention, it is assumed that the rubber sample to be tested is NBR, a rubber sealing ring material commonly used in 35MPa hydrogenation stations; the diffusion coefficient of this NBR material is 1.1×10 -10 m 2 / s. First, take a Φ13mm×2mm round NBR sample and measure its volume. The volume of the NBR sample before the test is V0=2.66×10 -7 m 3 ; Next, hydrogen exposure is performed, that is, a test container that meets the test pressure and temperature requirements is used, the NBR sample is placed in the test container, and after the gas replacement procedure is completed, the test container is loaded to 1.25 times the nominal working pressure of 43.75MPa at room temperature and left to stand for 24h; then, hydrogen rapid decompression is performed, specifically, the hydrogen pressure in the test container is reduced to below 1MPa within 10 seconds, and after the gas replacement procedure is completed, the test container is opened to take out the NBR sample; the hydrogen rapid decompression process must be completed within 10s; then, the rubber hydrogen absorption saturation volume expansion rate is measured: the volume of the rubber sample is measured 15min after the decompression is completed, and V2=4.01×10 -7 m 3 Furthermore, according to the fitting ξ-D relationship, the compensation coefficient of the NBR sample at this time can be obtained as:

[0100]

[0101] At this time, the hydrogen absorption saturation volume expansion rate of the NBR sample is:

[0102]

[0103] The volume of the NBR sample immediately after decompression is:

[0104] V1=V R1 ×V0+V0=79.7%×2.66×10 -7 +2.66×10 -7 =4.78×10 -7 m 3

[0105] That is, the volume of the NBR sample immediately after decompression is 4.78×10 -7 m 3 .

[0106] Thus, the rubber volume expansion rate calculated based on the first volume after hydrogen absorption measured 15 minutes after decompression is:

[0107]

[0108] Therefore, for a diffusion coefficient of 1.1×10 -10 m 2 / s, the actual rubber hydrogen absorption saturated volume expansion rate obtained by the compensation coefficient calculation method is 79.7%, which is nearly 1.5 times the volume expansion rate of 50.8% at 15 minutes after decompression. This calculation method improves the accuracy of the measurement of the rubber hydrogen absorption saturated volume expansion rate.

[0109] Then, measure the permanent volume change rate of the rubber: determine the time for measuring the permanent volume change rate of the rubber, and the time t for measuring the permanent volume change rate of the NBR material can be obtained according to the fitting tD relationship:

[0110]

[0111] Therefore, the permanent volume change rate of the NBR material can be measured about 9.6 hours after decompression, at which time the hydrogen in the NBR sample has been completely released.

[0112] In summary, according to the method for measuring the volume change of a rubber material after hydrogen absorption according to the embodiment of the present invention, first, the initial volume and diffusion coefficient of the rubber sample to be tested are obtained; then, the rubber sample to be tested is allowed to stand in a test container to absorb hydrogen, and after the standing hydrogen absorption time reaches a first preset time, the test container is rapidly decompressed by hydrogen; then, timing is performed after the rapid hydrogen decompression is completed, and when the timing reaches a second preset time, the rubber sample to be tested is measured to obtain the first volume of the rubber sample to be tested after hydrogen absorption; then, the corresponding compensation coefficient is calculated according to the diffusion coefficient of the rubber sample to be tested based on the fitting relationship between the diffusion coefficient and the compensation coefficient, and the hydrogen absorption saturated volume expansion rate of the rubber sample to be tested is calculated according to the compensation coefficient and the first volume after hydrogen absorption. In this way, the calculation error of the hydrogen absorption saturated volume expansion rate in the process of detecting the rubber material after hydrogen absorption is reduced, and the accuracy of the final measurement result is improved.

[0113] In order to implement the above embodiment, an embodiment of the present invention proposes a computer-readable storage medium, on which a program for measuring the volume change of a rubber material after hydrogen absorption is stored. When the program for measuring the volume change of a rubber material after hydrogen absorption is executed by a processor, the method for measuring the volume change of a rubber material after hydrogen absorption as described above is implemented.

[0114] According to the computer-readable storage medium of the embodiment of the present invention, by storing a volume change measurement program of a rubber material after hydrogen absorption, the processor implements the volume change measurement method of a rubber material after hydrogen absorption when executing the volume change measurement program of a rubber material after hydrogen absorption; thereby reducing the calculation error of the hydrogen absorption saturation volume expansion rate in the detection process of the rubber material after hydrogen absorption, and improving the accuracy of the final measurement result.

[0115] In order to implement the above embodiment, the embodiment of the present invention provides a device for measuring the volume change of a rubber material after hydrogen absorption, such as Figure 2 As shown, the device for measuring the volume change of a rubber material after hydrogen absorption comprises: an acquisition module 10 , a test module 20 , a measurement module 30 and a calculation module 40 .

[0116] Wherein, the acquisition module 10 is used to obtain the initial volume and diffusion coefficient of the rubber sample to be tested;

[0117] The test module 20 is used to allow the rubber sample to absorb hydrogen in a test container, and to quickly decompress the hydrogen in the test container after the hydrogen absorption time reaches a first preset time.

[0118] The measuring module 30 is used to time after the rapid decompression of hydrogen is completed, and when the timing reaches a second preset time, measure the rubber sample to be tested to obtain a first volume of the rubber sample to be tested after hydrogen absorption;

[0119] The calculation module 40 is used to calculate the corresponding compensation coefficient according to the diffusion coefficient of the rubber sample to be tested based on the fitting relationship between the diffusion coefficient and the compensation coefficient, and calculate the hydrogen absorption saturated volume expansion rate of the rubber sample to be tested according to the compensation coefficient and the first volume after hydrogen absorption.

[0120] In some embodiments, the calculation module 40 is further used to calculate the corresponding permanent volume change time according to the diffusion coefficient of the rubber sample to be tested based on the fitting relationship between the diffusion coefficient and the permanent volume change time;

[0121] The measuring module 30 is also used to measure the rubber sample to be tested according to the permanent volume change time to obtain the second volume of the rubber sample after hydrogen absorption, and calculate the permanent volume change rate of the rubber sample to be tested according to the first volume after hydrogen absorption and the second volume after hydrogen absorption.

[0122] In some embodiments, the compensation coefficient is calculated by the following formula:

[0123]

[0124] Where ξ represents the compensation coefficient, and D represents the diffusion coefficient of the rubber sample to be tested.

[0125] In some embodiments, the hydrogen absorption saturation volume expansion rate is calculated by the following formula:

[0126] V R1 =ξ×V R2

[0127] V R2 =(V2-V0) / V0

[0128] Among them, V R1represents the volume expansion rate of hydrogen absorption saturation, V0 represents the initial volume, V2 represents the volume after the first hydrogen absorption, V R2 It represents the volume expansion rate corresponding to the volume after the first hydrogen absorption.

[0129] In some embodiments, the permanent volume change time is calculated by the following formula:

[0130]

[0131] Wherein, t represents the permanent volume change time, and D represents the diffusion coefficient of the rubber sample to be tested.

[0132] In some embodiments, the compensation coefficient is calculated using a two-dimensional non-steady finite boundary diffusion model.

[0133] In some embodiments, the two-dimensional non-steady finite boundary diffusion model is expressed by the following formula:

[0134]

[0135] The initial conditions for the two-dimensional unsteady finite boundary diffusion model are:

[0136]

[0137] The boundary conditions of the two-dimensional unsteady finite boundary diffusion model are:

[0138]

[0139] Wherein, c represents the hydrogen concentration in the rubber sample to be tested, c1 represents the concentration of the rubber sample to be tested when it is saturated with hydrogen, t represents the decompression time, D represents the diffusion coefficient, x represents the horizontal coordinate of a certain position in the rubber sample to be tested, and y represents the vertical coordinate of a certain position in the rubber sample to be tested.

[0140] In some embodiments, the diffusion coefficient ranges from 1×10 -10 m 2 / s to 1×10 -8 m 2 / s.

[0141] It should be noted that the above description of the method for measuring the volume change of a rubber material after hydrogen absorption is also applicable to the device for measuring the volume change of a rubber material after hydrogen absorption, and will not be described in detail here.

[0142] In summary, according to the apparatus for measuring the volume change of a rubber material after hydrogen absorption of an embodiment of the present invention, a test module is provided for statically absorbing hydrogen on the rubber sample to be tested in a test container, and after the static hydrogen absorption time reaches a first preset time, the test container is rapidly decompressed by hydrogen; a measuring module is used to time after the rapid hydrogen decompression is completed, and when the timing reaches a second preset time, the rubber sample to be tested is measured to obtain a first volume of the rubber sample to be tested after hydrogen absorption; a calculation module is used to calculate a corresponding compensation coefficient according to the diffusion coefficient of the rubber sample to be tested based on a fitting relationship between the diffusion coefficient and the compensation coefficient, and calculate the hydrogen absorption saturated volume expansion rate of the rubber sample to be tested according to the compensation coefficient and the first volume after hydrogen absorption; thereby reducing the calculation error of the hydrogen absorption saturated volume expansion rate in the detection process of the rubber material after hydrogen absorption, and improving the accuracy of the final measurement result.

[0143] It should be noted that the logic and / or steps represented in the flowchart or otherwise described herein, for example, can be considered as a sequenced list of executable instructions for implementing logical functions, and can be specifically implemented in any computer-readable medium for use by an instruction execution system, device or apparatus (such as a computer-based system, a system including a processor, or other system that can fetch instructions from an instruction execution system, device or apparatus and execute instructions), or in combination with these instruction execution systems, devices or apparatuses. For the purposes of this specification, "computer-readable medium" can be any device that can contain, store, communicate, propagate or transmit a program for use by an instruction execution system, device or apparatus, or in combination with these instruction execution systems, devices or apparatuses. More specific examples of computer-readable media (a non-exhaustive list) include the following: an electrical connection portion with one or more wirings (electronic device), a portable computer disk box (magnetic device), a random access memory (RAM), a read-only memory (ROM), an erasable and programmable read-only memory (EPROM or flash memory), an optical fiber device, and a portable compact disk read-only memory (CDROM). In addition, the computer-readable medium may even be paper or other suitable medium on which the program is printed, since the program may be obtained electronically, for example, by optically scanning the paper or other medium and then editing, interpreting or processing in other suitable ways if necessary, and then stored in a computer memory.

[0144] It should be understood that the various parts of the present invention can be implemented by hardware, software, firmware or a combination thereof. In the above-mentioned embodiments, a plurality of steps or methods can be implemented by software or firmware stored in a memory and executed by a suitable instruction execution system. For example, if implemented by hardware, as in another embodiment, it can be implemented by any one of the following technologies known in the art or their combination: a discrete logic circuit having a logic gate circuit for implementing a logic function for a data signal, a dedicated integrated circuit having a suitable combination of logic gate circuits, a programmable gate array (PGA), a field programmable gate array (FPGA), etc.

[0145] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0146] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for measuring the volume change of a rubber material after hydrogen absorption, characterized in that: The following steps are involved: Obtain the initial volume and diffusion coefficient of the rubber sample to be tested; Allowing the rubber sample to absorb hydrogen in a test container, and after the hydrogen absorption time reaches a first preset time, rapidly reducing the hydrogen pressure in the test container; After the hydrogen rapid decompression is completed, timing is performed, and when the timing reaches a second preset time, the rubber sample to be tested is measured to obtain a first volume of the rubber sample to be tested after hydrogen absorption; The corresponding compensation coefficient is calculated according to the diffusion coefficient of the rubber sample to be tested based on the fitting relationship between the diffusion coefficient and the compensation coefficient, and the hydrogen absorption saturated volume expansion rate of the rubber sample to be tested is calculated according to the compensation coefficient and the first volume after hydrogen absorption.

2. The method for measuring volume change of a rubber material after hydrogen absorption according to claim 1, characterized in that: Also includes: Based on the fitting relationship between the diffusion coefficient and the permanent volume change time, the corresponding permanent volume change time is calculated according to the diffusion coefficient of the rubber sample to be tested, and the rubber sample to be tested is measured according to the permanent volume change time to obtain the second volume of the rubber sample to be tested after hydrogen absorption; The permanent volume change rate of the rubber sample to be tested is calculated according to the first volume after hydrogen absorption and the second volume after hydrogen absorption.

3. The method for measuring volume change of a rubber material after hydrogen absorption according to claim 1, characterized in that: The compensation coefficient is calculated by the following formula: Where ξ represents the compensation coefficient, and D represents the diffusion coefficient of the rubber sample to be tested.

4. The method for measuring volume change of a rubber material after hydrogen absorption according to claim 3, characterized in that: The hydrogen absorption saturation volume expansion rate is calculated by the following formula: In R1 =ξ×V R2 V R2 =(V2-V0) / V0 Among them, V R1 represents the volume expansion rate of hydrogen absorption saturation, V0 represents the initial volume, V2 represents the volume after the first hydrogen absorption, V R2 It represents the volume expansion rate corresponding to the volume after the first hydrogen absorption.

5. The method for measuring volume change of a rubber material after hydrogen absorption according to claim 2, characterized in that: The permanent volume change time is calculated by the following formula: Wherein, t represents the permanent volume change time, and D represents the diffusion coefficient of the rubber sample to be tested.

6. The method for measuring volume change of a rubber material after hydrogen absorption according to claim 1, characterized in that: The compensation coefficient is calculated by a two-dimensional non-steady-state finite boundary diffusion model; the initial concentration of the two-dimensional non-steady-state finite boundary diffusion model is the hydrogen absorption saturation concentration value of the rubber sample to be tested, and the model boundary concentration is zero.

7. The method for measuring volume change of a rubber material after hydrogen absorption according to claim 1, characterized in that: The diffusion coefficient ranges from 1×10 -10 m 2 / s to 1×10 -8 m 2 / s.

8. A computer-readable storage medium, characterized in that: A program for measuring the volume change of a rubber material after hydrogen absorption is stored thereon, and when the program for measuring the volume change of a rubber material after hydrogen absorption is executed by a processor, a method for measuring the volume change of a rubber material after hydrogen absorption as claimed in any one of claims 1 to 7 is implemented.

9. A device for measuring volume change of a rubber material after hydrogen absorption, characterized in that: include: An acquisition module, the acquisition module is used to acquire the initial volume and diffusion coefficient of the rubber sample to be tested; A test module, the test module is used to allow the rubber sample to absorb hydrogen in a test container, and to quickly decompress the hydrogen in the test container after the hydrogen absorption time reaches a first preset time; A measuring module, the measuring module is used to time after the hydrogen rapid decompression is completed, and when the timing reaches a second preset time, measure the rubber sample to be tested to obtain a first volume of the rubber sample to be tested after hydrogen absorption; A calculation module is used to calculate a corresponding compensation coefficient according to the diffusion coefficient of the rubber sample to be tested based on a fitting relationship between the diffusion coefficient and the compensation coefficient, and to calculate the hydrogen absorption saturated volume expansion rate of the rubber sample to be tested according to the compensation coefficient and the first volume after hydrogen absorption.

10. The device for measuring volume change of rubber material after hydrogen absorption as claimed in claim 9, characterized in that: The calculation module is also used to calculate the corresponding permanent volume change time according to the diffusion coefficient of the rubber sample to be tested based on the fitting relationship between the diffusion coefficient and the permanent volume change time; The measuring module is further used to measure the rubber sample to be tested according to the permanent volume change time to obtain a second volume of the rubber sample to be tested after hydrogen absorption, and calculate the permanent volume change rate of the rubber sample to be tested according to the first volume after hydrogen absorption and the second volume after hydrogen absorption.