AR film with better physical properties and preparation process thereof
By using materials such as alumina or yttrium oxide as durable layers in the AR film and combining with other optical layers to optimize the layer structure, the problem of insufficient physical performance of the AR film is solved, and the hardness, heat resistance and wear resistance are improved. .
Patent Information
- Application Number
- CN202411023812.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-01
AI Technical Summary
The physical properties of existing AR films, such as hardness, heat resistance and wear resistance, are difficult to meet the increasingly high requirements for use.
By providing alumina or yttrium oxide as a durable layer in the AR film, and combining the first niobium oxide, silica, and silicon-aluminum mixed layer, the coordination between layers is optimized to improve the physical properties of the AR film.
The hardness, heat resistance and wear resistance of the AR film are significantly improved, so that it has excellent physical properties while maintaining high light transmission and stability.
Smart Images

Figure CN118884582A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of AR films, and in particular relates to an AR film with better physical properties and a preparation process thereof. Background Art
[0002] AR film, also known as anti-reflection film or anti-reflection film, is a highly transparent optical film that allows light to pass through more completely. It can reduce or eliminate the reflected light from optical surfaces such as prisms and plane mirrors, thereby increasing the light transmittance of these components and presenting the light to the user's eyes to the greatest extent. Due to the performance of the AR film itself, it is usually applied to display device protection screens such as car displays, televisions, computers, mobile phones, tablets and other electronic products that increase transmittance and reduce reflectivity. The AR film effectively increases the glass transmittance and reduces the glass reflectivity.
[0003] As the application of AR films becomes more and more extensive, the requirements for the performance of AR films are becoming higher and higher, especially the physical properties of AR films such as hardness, heat resistance and wear resistance. Therefore, the physical properties of existing AR films need to be further improved.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] The purpose of the present invention is to provide an AR film with better physical properties and a preparation process thereof. The AR film has excellent hardness, heat resistance and wear resistance.
[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0007] The AR film with better physical properties comprises a substrate layer, an upper coating layer, a primer layer, a durable layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, and a silicon-aluminum mixed layer which are stacked in sequence;
[0008] The durable layer is an aluminum oxide layer or a yttrium oxide layer, and the thickness of the durable layer is 1-20 nm.
[0009] In one or more embodiments of the present invention, the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (85-98): (15-2).
[0010] In one or more embodiments of the present invention, the base layer material is selected from SiO2, Ti, Si, Al, MgF2, SiO, HfO2, Sn and Y.
[0011] In one or more embodiments of the present invention, the substrate layer is selected from a PET layer, a PI layer, a SRF layer, a TAC layer, a COP layer and a PC layer.
[0012] In one or more embodiments of the present invention, a lower coating layer is provided on the side of the substrate layer facing away from the upper coating layer, and both the upper coating layer and the lower coating layer are formed by coating an acrylic resin coating liquid. The thickness of the upper coating layer is 50-500nm, and the thickness of the lower coating layer is 0.2-4.1μm.
[0013] In one or more embodiments of the present invention, an AF layer is provided on the side of the silicon-aluminum mixed layer facing away from the second niobium oxide layer.
[0014] In one or more embodiments of the present invention, the thickness of the AF layer is 2-190 nm.
[0015] In one or more embodiments of the present invention, the thickness of the substrate layer is 5.7-250 μm; and / or the thickness of the base layer is 0.1-10 nm; and / or the thickness of the first niobium oxide layer is 5-200 nm; and / or the thickness of the silicon dioxide layer is 10-260 nm; and / or the thickness of the second niobium oxide layer is 5-280 nm; and / or the thickness of the silicon-aluminum mixed layer is 50-310 nm.
[0016] A method for preparing an AR film with better physical properties comprises the following steps:
[0017] An upper coating layer and a lower coating layer are respectively arranged on both sides of the substrate layer, and a high temperature protective film is arranged on the lower coating layer;
[0018] A primer layer, a durable layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer;
[0019] An AF layer is coated on the silicon-aluminum mixed layer, and an upper protective film is disposed on the AF layer.
[0020] In one or more embodiments of the present invention, the high temperature protection film and the upper protection film are both PET films.
[0021] Compared with the prior art, the present invention provides an aluminum oxide layer or an yttrium oxide layer on the base layer and cooperates between layers, so that the AR film has excellent optical properties while the physical properties such as hardness, heat resistance and wear resistance are effectively improved, making the AR film exhibit excellent physical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 It is a structural diagram of an AR film with better physical properties in one embodiment of the present invention;
[0024] Figure 2 This is a comparison chart of the reflection curves of Example 1 of the present invention and the comparative example 1380-780nm;
[0025] Figure 3 It is a comparison chart of the reflection curves of Example 1 of the present invention and the comparative example 1400-700nm.
[0026] Description of main reference numerals:
[0027] 1-high temperature protective film, 2-lower coating layer, 3-substrate layer, 4-upper coating layer, 5-priming layer, 6-durable layer, 7-first niobium oxide layer, 8-silicon dioxide layer, 9-second niobium oxide layer, 10-silicon aluminum mixed layer, 11-AF layer, 12, upper protective film. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0029] A specific embodiment of the present invention provides an AR film with better physical properties, including a substrate layer, an upper coating layer, a primer layer, a durable layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, and a silicon-aluminum mixed layer stacked in sequence; the durable layer is an aluminum oxide layer or an yttrium oxide layer, and the thickness of the durable layer is 1-20nm.
[0030] Specifically, the higher the hardness of the AR film, the better the wear resistance, and the less likely it is to be scratched. Its heat resistance and corrosion resistance determine its stability and service life during use. The present invention uses aluminum oxide or yttrium oxide as a durable layer to make the AR film have high hardness, heat resistance and corrosion resistance, thereby improving the physical properties of the AR film.
[0031] Alumina has high hardness, strength and chemical stability, which can significantly improve the physical properties of AR film. In addition, alumina also has a low refractive index and a wide light transmittance range, which can improve the light transmittance of AR film. Yttrium oxide has a high melting point and excellent wear resistance, heat resistance and corrosion resistance, which can give AR film excellent physical properties. Yttrium oxide has high light transmittance and a wide transmission range, which can significantly improve the optical properties of AR film.
[0032] A first niobium oxide layer for increasing transmittance, a silicon dioxide layer for reducing reflection, a second niobium oxide layer for increasing transmittance and a silicon-aluminum mixed layer for reducing reflection are arranged on the durable layer. Compared with the silicon dioxide layer, the silicon-aluminum mixed layer is on the surface of the AR film, has harder and more wear-resistant properties, and has more stable performance. When it is on the surface of the AR film, it can make the physical and optical properties of the AR film more stable.
[0033] In one specific embodiment, the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (85-98):(15-2).
[0034] Specifically, the silicon content of the silicon-aluminum mixed layer is greater than the aluminum content. The high silicon content can promote the formation of more Si-O bonds in the AR film, which helps to improve the thermal stability of the AR film, and at the same time make the AR film have a higher refractive index and higher adhesion; appropriate doping with aluminum can improve the hardness and corrosion resistance of the AR film. Therefore, by controlling the silicon-aluminum molar ratio, the AR film can have both high light transmittance and physical properties.
[0035] In one specific embodiment, the base layer material is selected from SiO2, Ti, Si, Al, MgF2, SiO, HfO2, Sn and Y.
[0036] Specifically, the primer layer can improve the adhesion of the AR film.
[0037] In a specific embodiment, the substrate layer is selected from a PET layer, a PI layer, a SRF layer, a TAC layer, a COP layer and a PC layer.
[0038] Specifically, the PET layer is a polyethylene terephthalate layer, the PI layer is a polyimide layer, the SRF layer is a super-reflective polyester film layer, the TAC layer is a triacetate cellulose film, the COP layer is a cycloolefin polymer layer, and the PC layer is a polycarbonate layer. The above-mentioned substrate layers are used to make the AR film have better physical properties.
[0039] In a specific embodiment, a lower coating layer is provided on the side of the substrate layer away from the upper coating layer. Both the upper coating layer and the lower coating layer are formed by coating an acrylic resin coating liquid. The thickness of the upper coating layer is 50-500nm, and the thickness of the lower coating layer is 0.2-4.1μm.
[0040] In a specific embodiment, an AF layer is disposed on the side of the silicon-aluminum mixed layer facing away from the second niobium oxide layer.
[0041] In one embodiment, the thickness of the AF layer is 2-190 nm.
[0042] Specifically, the AF layer is formed by coating with an AF coating liquid, the main component of which is a perfluoropolyether polymer. Coating the AF coating liquid on the surface of the silicon-aluminum mixed layer can give the AR film low friction and easy wiping properties, thereby reducing the possibility of scratches on the AR film surface.
[0043] In one specific embodiment, the thickness of the substrate layer is 5.7-250 μm; the thickness of the primer layer is 0.1-10 nm; the thickness of the first niobium oxide layer is 5-200 nm; the thickness of the silicon dioxide layer is 10-260 nm; the thickness of the second niobium oxide layer is 5-280 nm; and the thickness of the silicon-aluminum mixed layer is 50-310 nm.
[0044] Specifically, by controlling the thickness of each layer, the AR film has better physical properties.
[0045] Another specific embodiment of the present invention provides a method for preparing an AR film with better physical properties, comprising the following steps:
[0046] An upper coating layer and a lower coating layer are respectively coated on both sides of the substrate layer by a coating process, and a high-temperature protective film is arranged on the lower coating layer;
[0047] A primer layer, a durable layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer;
[0048] An AF coating liquid is applied to the silicon-aluminum mixed layer to form an AF layer, and a protective film is provided on the AF layer.
[0049] Specifically, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, and the acrylic resin coating liquid is a conventional product in the prior art, and its main components are copolymer resins of (meth) acrylic acid esters and (meth) hydroxy acrylic acid esters.
[0050] In a specific embodiment, the high temperature protection film and the upper protection film are both PET films.
[0051] The present invention is further described in detail below in conjunction with specific embodiments.
[0052] Example 1
[0053] The AR film with better physical properties includes, from bottom to top, a 30μm thick PET film, a 2.7μm thick lower coating layer, a 5.7μm thick substrate layer, a 50nm thick upper coating layer, a 0.1nm thick primer layer, a 15nm thick aluminum oxide layer, an 87nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 132nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick AF layer and a 50μm thick PET film.
[0054] Among them, the substrate layer is a PI layer, i.e. a polyimide layer, the base layer material is MgF2, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, the AF layer is formed by coating with an AF coating liquid, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0055] Example 2
[0056] The AR film with better physical properties includes, from bottom to top, a PET film with a thickness of 114 μm, a lower coating layer with a thickness of 0.2 μm, a substrate layer with a thickness of 134 μm, an upper coating layer with a thickness of 500 nm, a primer layer with a thickness of 4 nm, an aluminum oxide layer with a thickness of 1 nm, a first niobium oxide layer with a thickness of 5 nm, a silicon dioxide layer with a thickness of 260 nm, a second niobium oxide layer with a thickness of 280 nm, a silicon-aluminum mixed layer with a thickness of 207 nm, an AF layer with a thickness of 126 nm, and a PET film with a thickness of 50 μm.
[0057] Among them, the substrate layer is a PI layer, i.e. a polyimide layer, the base layer material is MgF2, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, the AF layer is formed by coating with an AF coating liquid, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0058] Example 3
[0059] The AR film with better physical properties includes, from bottom to top, a 188μm thick PET film, a 4.1μm thick lower coating layer, a 250μm thick substrate layer, a 262nm thick upper coating layer, a 10nm thick primer layer, a 20nm thick aluminum oxide layer, a 200nm thick first niobium oxide layer, a 94nm thick silicon dioxide layer, a 5nm thick second niobium oxide layer, a 310nm thick silicon-aluminum mixed layer, a 190nm thick AF layer and a 50μm thick PET film.
[0060] Among them, the substrate layer is a PI layer, i.e. a polyimide layer, the base layer material is MgF2, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, the AF layer is formed by coating with an AF coating liquid, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0061] Example 4
[0062] The AR film with better physical properties includes, from bottom to top, a 30μm thick PET film, a 2.7μm thick lower coating layer, a 5.7μm thick substrate layer, a 50nm thick upper coating layer, a 0.1nm thick primer layer, a 1nm thick aluminum oxide layer, an 87nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 132nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick AF layer and a 50μm thick PET film.
[0063] Among them, the substrate layer is a PI layer, i.e. a polyimide layer, the base layer material is MgF2, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, the AF layer is formed by coating with an AF coating liquid, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0064] Example 5
[0065] The AR film with better physical properties includes, from bottom to top, a 30μm thick PET film, a 2.7μm thick lower coating layer, a 5.7μm thick substrate layer, a 50nm thick upper coating layer, a 0.1nm thick primer layer, a 20nm thick aluminum oxide layer, an 87nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 132nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick AF layer and a 50μm thick PET film.
[0066] Among them, the substrate layer is a PI layer, i.e. a polyimide layer, the base layer material is MgF2, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, the AF layer is formed by coating with an AF coating liquid, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0067] Example 6
[0068] The AR film with better physical properties includes, from bottom to top, a 30μm thick PET film, a 2.7μm thick lower coating layer, a 5.7μm thick substrate layer, a 50nm thick upper coating layer, a 0.1nm thick primer layer, a 15nm thick yttrium oxide layer, an 87nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 132nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick AF layer and a 50μm thick PET film.
[0069] Among them, the substrate layer is a PI layer, i.e. a polyimide layer, the base layer material is MgF2, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, the AF layer is formed by coating with an AF coating liquid, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0070] Example 7
[0071] The AR film with better physical properties includes, from bottom to top, a 30μm thick PET film, a 2.7μm thick lower coating layer, a 5.7μm thick substrate layer, a 50nm thick upper coating layer, a 0.1nm thick primer layer, a 15nm thick aluminum oxide layer, an 87nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 132nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick AF layer and a 50μm thick PET film.
[0072] Among them, the substrate layer is a PI layer, i.e. a polyimide layer, the base layer material is MgF2, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, the AF layer is formed by coating with an AF coating liquid, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 98:2.
[0073] Example 8
[0074] The AR film with better physical properties includes, from bottom to top, a 30μm thick PET film, a 2.7μm thick lower coating layer, a 5.7μm thick substrate layer, a 50nm thick upper coating layer, a 0.1nm thick primer layer, a 15nm thick aluminum oxide layer, an 87nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 132nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick AF layer and a 50μm thick PET film.
[0075] Among them, the substrate layer is a PI layer, i.e. a polyimide layer, the base layer material is MgF2, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, the AF layer is formed by coating with an AF coating liquid, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 75:15.
[0076] Comparative Example 1
[0077] The AR film with better physical properties includes, from bottom to top, a 30μm thick PET film, a 2.7μm thick lower coating layer, a 20.7μm thick substrate layer, a 50nm thick upper coating layer, a 0.1nm thick primer layer, an 87nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 132nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick AF layer and a 50μm thick PET film.
[0078] Among them, the substrate layer is a PI layer, i.e. a polyimide layer, the base layer material is MgF2, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, the AF layer is formed by coating with an AF coating liquid, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0079] Comparative Example 2
[0080] The AR film with better physical properties includes, from bottom to top, a 30μm thick PET film, a 2.7μm thick lower coating layer, a 5.7μm thick substrate layer, a 50nm thick upper coating layer, a 0.1nm thick primer layer, a 0.4nm thick aluminum oxide layer, an 87nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 132nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick AF layer and a 50μm thick PET film.
[0081] Among them, the substrate layer is a PI layer, i.e. a polyimide layer, the base layer material is MgF2, the upper coating layer and the lower coating layer are both formed by coating with an acrylic resin coating liquid, the AF layer is formed by coating with an AF coating liquid, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0082] The AR films in the examples and comparative examples were prepared by the above-mentioned preparation method, and the following performance tests were performed.
[0083] (1) The total light transmittance and 400-700 nm spectrophotometer light transmittance of the films in Example 1 and Comparative Example 1 were tested. The results are shown in Table 1.
[0084] Table 1 Optical transmittance test results
[0085]
[0086] It can be seen from Table 1 that the total light transmittance of the films in Example 1 and Comparative Example 1 is above 95%, and the spectrophotometer transmittance is above 93%, indicating that the optical properties of the films in Example 1 and Comparative Example 1 can meet the requirements.
[0087] (5) The films in Example 1 and Comparative Example 1 were tested using an Olympus reflectometer, and the reflection curves at 380-780 nm and 400-700 nm were compared. The results are as follows: Figure 2 and Figure 3 As shown in the figure, the existing scheme 1 refers to Example 1, and the old scheme refers to Comparative Example 1.
[0088] According to the optical test requirements, the average reflection value of 380-780nm is less than 1.0%, and the average reflection value of 400-700nm is less than 0.5%. Figure 2 and Figure 3It can be seen that the average reflection value of the film material at 380-780nm in Example 1 is 0.76%, and the average reflection value at 400-700nm is 0.24%. The average reflection value of the film material at 380-780nm in Comparative Example 1 is 0.76%, and the average reflection value at 400-700nm is 0.25%. There is not much difference between the reflection curve in Example 1 and the reflection curve in Comparative Example 1, indicating that the optical properties of the films in Example 1 and Comparative Example 1 can meet the requirements.
[0089] (2) Pencil hardness test: The film is placed on a glass panel, and the pencil hardness tester is loaded with 500g and 750g respectively. A 3H hardness pencil and a 4H hardness pencil are used to test the hardness of the coating surface. During the test, 5 lines are drawn at each position, and the number of lines without scratches is recorded. Result judgment: 3 or more (including 3) lines without scratches out of 5 lines are judged as OK, and less than 3 lines are judged as NG. The results are shown in Table 2.
[0090] Table 2 Pencil hardness test results
[0091]
[0092]
[0093]
[0094] (3) Steel wool wear test: The film was placed on a glass panel and the wear tester was loaded with 1000g. The number of scratches after 1000, 2000 and 2500 frictions was recorded. A scratch number ≥4 was judged as NG and a scratch number ≤3 was judged as OK. The results are shown in Table 3.
[0095] Table 3 Steel wool wear test results
[0096]
[0097]
[0098] (3) The back of the film is bonded with OCA optical glue and then bonded to transparent glass. After bonding, the film is degassed with a degassing machine. After degassing, the surface is wiped clean. The film is then boiled in 100°C water for 3h and 5h, placed at double 85 (i.e., high temperature 85°C, high humidity 85%) for 32 days and 36 days, placed at 95°C for 32 days and 36 days, placed at -40°C for 32 days and 36 days, and exposed to sunlight (light intensity 0.55w / (m 2·nm), wavelength 340nm, filter Extended UV-Q / B, 3.8h of light + 1h of darkness as one cycle. The temperature of the blackboard during the light exposure was set at 89℃, the temperature of the box was 63℃, and the humidity was 50%; the temperature of the box and blackboard was set at 38℃ and the humidity was 95% during the dark stage) for 32 days and 36 days, and then a hundred grids were cut with a hundred grid knife, and then 3M company 681 type tape was used. After pressing and sticking, the tape was pulled off after standing for more than 30s. No peeling was 5B, slight peeling was 3-4B, barely OK, and NG was judged below 2B. The results are shown in Table 4.
[0099] Table 4 Comparison of various environmental tests
[0100]
[0101] Combined with Tables 2 to 4, compared with Comparative Example 1, the film material in the embodiment of the present invention has better hardness and wear resistance, indicating that the provision of an aluminum oxide layer can improve the hardness and wear resistance of the film material. At the same time, it can be seen from Table 3 that the film material in the embodiment is also more stable under environmental influences.
[0102] Combining Example 1, Example 4, Example 5 and Comparative Example 2, it can be seen that the thickness of the aluminum oxide layer will affect the physical properties of the AR film. Plating the aluminum oxide layer with reference to the thickness range of 1-20 nm disclosed in the present invention can ensure that the AR film has better hardness and wear resistance.
[0103] It can be seen from Example 1 and Example 6 that the yttrium oxide layer also has a good effect of improving the physical properties of the AR film, so that the AR film has higher hardness and wear resistance.
[0104] In combination with Example 1, Example 7 and Example 8, a silicon-aluminum mixed layer is plated with the silicon-aluminum molar ratio of (85-98): (15-2) disclosed in the present invention, which can improve the hardness and wear resistance of the AR film, and also improve the adhesion of the AR film to the substrate, thereby ensuring the performance stability of the AR film.
[0105] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0106] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. AR film with better physical properties, characterized in that: It includes a substrate layer, an upper coating layer, a primer layer, a durable layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, and a silicon-aluminum mixed layer which are stacked in sequence; The durable layer is an aluminum oxide layer or a yttrium oxide layer, and the thickness of the durable layer is 1-20 nm.
2. The AR film with better physical properties according to claim 1, characterized in that: The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (85-98):(15-2).
3. The AR film with better physical properties according to claim 1, characterized in that: The base layer material is selected from SiO2, Ti, Si, Al, MgF2, SiO, HfO2, Sn and Y.
4. The AR film with better physical properties according to claim 1, characterized in that: The substrate layer is selected from the group consisting of a PET layer, a PI layer, a SRF layer, a TAC layer, a COP layer and a PC layer.
5. The AR film with better physical properties according to claim 1, characterized in that: A lower coating layer is disposed on the side of the substrate layer away from the upper coating layer. Both the upper coating layer and the lower coating layer are formed by coating an acrylic resin coating liquid. The thickness of the upper coating layer is 50-500nm, and the thickness of the lower coating layer is 0.2-4.1μm.
6. The AR film with better physical properties according to claim 1, characterized in that: An AF layer is disposed on the side of the silicon-aluminum mixed layer facing away from the second niobium oxide layer.
7. The AR film with better physical properties according to claim 6, characterized in that: The thickness of the AF layer is 2-190 nm.
8. The AR film with better physical properties according to claim 1, characterized in that: The thickness of the substrate layer is 5.7-250 μm; and / or the thickness of the base layer is 0.1-10 nm; and / or the thickness of the first niobium oxide layer is 5-200 nm; and / or the thickness of the silicon dioxide layer is 10-260 nm; and / or the thickness of the second niobium oxide layer is 5-280 nm; and / or the thickness of the silicon-aluminum mixed layer is 50-310 nm.
9. The process for preparing an AR film with better physical properties according to any one of claims 1 to 8, characterized in that: The steps include: An upper coating layer and a lower coating layer are respectively arranged on both sides of the substrate layer, and a high temperature protective film is arranged on the lower coating layer; A primer layer, a durable layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer; An AF layer is coated on the silicon-aluminum mixed layer, and an upper protective film is disposed on the AF layer.
10. The process for preparing an AR film with better physical properties according to claim 9, characterized in that: The high temperature protective film and the upper protective film are both PET films.
Citation Information
Patent Citations
Yttrium oxide / silica antireflection protective film for sapphire infrared windows and its preparation method
CN103287010A
Strong-alkali-resistant sapphire glass panel surface coating method
CN113862611A
AR film and preparation method and application thereof
CN115343787A
Hard film for airport runway light and preparation method of hard film
CN115961249A
Automobile side windshield AR film and preparation method thereof
CN117227296A
Cited By
AR film, light-transmitting assembly and electronic equipment
CN119471869A