Preparation method of high-strength high-thermal-conductivity heat-resistant aluminum heat dissipation plate for new energy automobile

By using aerosolization preparation and multi-process processing in aluminum alloys, the problem of insufficient strength, thermal conductivity and heat resistance of aluminum alloy heat dissipation plates in new energy vehicles is solved, and high efficiency and low cost are achieved Performance improvement.

CN118989329APending Publication Date: 2024-11-22ALTI ADVANCED MATERIALS (XIANGHE) CO LTD

Patent Information

Application Number
CN202411136942.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high strength, high thermal conductivity and high heat resistance in aluminum alloys at the same time, and the process is complex or costly, so it is unable to effectively replace copper materials in the use of new energy vehicle heat sinks.

Method used

Ultrafine ultrapure aluminum powder is prepared by aerosolization, and nanoscale alumina particles are formed through cold isostatic pressure forming, sintering, hot extrusion, forging and stress removal annealing, and nanoscale alumina particles are formed to improve the mechanical and thermal conductivity of the aluminum heat dissipation plate.

Benefits of technology

It achieves a coordinated improvement of high strength, excellent heat resistance and high thermal conductivity, reduces production costs and process complexity, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989329A_ABST
    Figure CN118989329A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a high-strength high-thermal-conductivity heat-resistant aluminum heat dissipation plate for a new energy automobile, and relates to the technical field of aluminum alloy powder metallurgy. The preparation method of the high-strength high-thermal-conductivity heat-resistant aluminum heat dissipation plate for the new energy automobile comprises the steps of preparation of superfine ultra-pure aluminum powder, powder forming, compact sintering densification, hot extrusion forming of aluminum ingots, forging forming of the aluminum heat dissipation plate, stress relief annealing of the aluminum heat dissipation plate and machining. According to the preparation method disclosed by the invention, the prepared alloy powder is used for preparing the heat dissipation aluminum plate and can synergistically improve the mechanical property, the heat-conducting property and the heat resistance of the heat dissipation aluminum plate by selecting the technological process of powder preparation, cold isostatic pressing, sintering, thermal deformation, forging, stress relief annealing and finish machining; the method is high in resource utilization rate, low in cost, short in process, high in efficiency and beneficial to industrial large-scale production and popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy powder metallurgy, and in particular to a method for preparing a high-strength, high-thermal-conductivity, and heat-resistant aluminum heat sink for new energy vehicles. Background Art

[0002] At present, the main component of the heat sink of the OBD integrated module used in new energy vehicles is copper. In the context of the current shortage of copper resources, the cost of preparing copper heat sinks is getting higher and higher in the long run. Among common metal materials, the thermal conductivity of aluminum is only lower than that of copper. At the same time, aluminum is the most abundant metal element in the earth's crust, so in the selection of heat sink components, "replacing copper with aluminum" has broad market prospects.

[0003] However, there are three problems with aluminum and aluminum alloys, which makes it difficult to prepare heat sinks using "aluminum instead of copper": First, pure aluminum has high thermal conductivity, but low strength and hardness; and if alloying elements are added to make an aluminum alloy, although the strength can be improved, the thermal conductivity will be drastically reduced. Second, compared with copper, aluminum alloys have a low melting point, and grains are more likely to grow during the same heating process, resulting in poor heat resistance. Third, aluminum nitride is added to aluminum alloys to increase thermal conductivity and strength, but the improvement in thermal conductivity is not large, not exceeding 230W / (m·K). In general, to achieve the preparation of heat sinks using "aluminum instead of copper", it is necessary to simultaneously meet the performance requirements of high strength, high heat resistance, and high thermal conductivity.

[0004] Chinese patent CN115261660A discloses a method for preparing a high-strength and high-thermal-conductivity aluminum alloy material, which requires first preparing an alkyl aluminum intermediate, then separating the solid intermediate and mixing it evenly with aluminum alloy powder, vacuum heating to obtain a mixed powder of aluminum nitride and aluminum alloy, and die-pressing and sintering to obtain a high-strength and high-thermal-conductivity aluminum alloy material; obviously, this method improves the mechanical properties and thermal conductivity of aluminum alloy products through aluminum nitride, but the mechanical properties are effectively improved among the synergistically improved properties, while the thermal conductivity improvement effect is not good, and the process flow is relatively complicated, which is not suitable for large-scale production.

[0005] Chinese patent CN115058614A discloses a preparation method and smelting device for a high-strength and high-thermal-conductivity aluminum alloy. Although the purity of the aluminum alloy is improved by setting the device structure, the preparation method is through smelting and casting, and the mechanical properties and thermal conductivity are not improved synergistically. The special device structure has high cost, the casting structure contains relatively large grains, and the heat resistance problem is still not solved.

[0006] Chinese patent CN116463529A discloses a high-conductivity and high-heat-resistant die-cast aluminum alloy for new energy vehicles and a preparation method thereof. It is necessary to melt a chlorine element and then add a single element and an intermediate alloy to cast an aluminum alloy ingot, which is then melted again and injected into a die-casting mold to obtain a casting. Obviously, the material prepared by this method is a cast structure. Although the alloy composition is used to improve the performance, the tensile strength and thermal conductivity are relatively low, and the alloy cost is relatively high. Summary of the invention

[0007] In order to solve the technical problems that the prior art improves the performance of high-strength, high-thermal-conductivity, and heat-resistant aluminum heat sinks for new energy vehicles by adding alloy elements, improving the preparation method, and adding hard phases, the cost is high, the efficiency is low, the mechanical properties are improved but the thermal conductivity is reduced, or the thermal conductivity is not improved much on the basis of the mechanical properties, and does not reach 230W / (m·K); therefore, the embodiment of the present invention provides a preparation method of a high-strength, high-thermal-conductivity, and heat-resistant aluminum heat sink for new energy vehicles that can synergistically improve the mechanical properties and thermal conductivity. The technical solution is as follows:

[0008] A method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, the method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles comprises the following steps:

[0009] S1. Preparation of ultrafine ultrapure aluminum powder: preparing pure aluminum powder from molten aluminum by gas atomization;

[0010] S2, powder forming: S1 pure aluminum powder is encapsulated in a silicone sheath or a rubber sheath, and is formed by cold isostatic pressing to obtain an aluminum green body;

[0011] S3, compact sintering and densification: the S2 aluminum green billet is subjected to pressureless sintering or pressure sintering to obtain an aluminum billet;

[0012] S4, aluminum ingot hot extrusion forming: S3 aluminum ingot is subjected to hot deformation processing to prepare fully dense aluminum sheet and strip;

[0013] S5, forging and forming of aluminum heat sink: cutting the fully dense aluminum sheet and strip in S4 to obtain cut aluminum sheet and strip, forging the cut aluminum sheet and strip, and finally obtaining a powder metallurgy pure aluminum heat sink blank;

[0014] S6. Stress relief annealing of aluminum heat sink: using corresponding process to perform stress relief annealing on the aluminum heat sink to obtain a low residual stress powder metallurgy pure aluminum heat sink blank;

[0015] S7, mechanical processing: fine-processing the powder metallurgy aluminum heat sink blank obtained above to finally obtain an aluminum heat sink product.

[0016] Optionally, the gas atomization in S1 is nitrogen atomization, the temperature of the molten aluminum liquid is 830-900° C., the nitrogen pressure is 6.5-8.0 MPa, and the obtained pure aluminum powder is spherical and / or nearly spherical in shape, with an average particle size of 2-40 μm and a surface oxide film thickness of 10-100 nm.

[0017] Optionally, the size of the silica gel sheath in S2 is 250-300 mm×800-900 mm, the cold isostatic pressing is performed at a pressure of 120-250 MPa for 80-240 seconds, and the size of the aluminum green billet is 200-220 mm×600-700 mm.

[0018] Optionally, the pressureless sintering in S3 is carried out in a nitrogen atmosphere at 350-400°C for 0.5-1h, and then the temperature is continuously raised at a rate of 3-7°C / min to a sintering temperature of 590-640°C, and the temperature is maintained for 2-8h, and the relative density reaches above 97.7%.

[0019] Optionally, the vacuum sintering in S3 is carried out in a vacuum atmosphere at 350-400°C for 0.5-1h, and then the temperature is continuously raised at a rate of 3-7°C / min to a sintering temperature of 590-640°C, and the temperature is maintained for 2-8h, until the relative density reaches above 97.5%.

[0020] Optionally, the pressure sintering in S3 is carried out under a pressure environment, the temperature is raised to 580-640°C at a rate of 3-7°C / min, the temperature is kept for 20-60 minutes for pre-sintering, and then the temperature is reduced by 10-20°C. At the same time, nitrogen is used to increase the gas pressure to 3-10MPa, and low-pressure sintering is performed for 2-7 hours, and the relative density reaches 100%.

[0021] Optionally, the hot deformation processing technology in S4 is hot extrusion, the hot extrusion temperature is 300-550°C, the deformation amount is 10-100%, and the cross-section of the fully dense aluminum sheet and strip is 70-130mm wide and 8-13mm thick.

[0022] Optionally, the size of the aluminum plate strip after cutting in S5 is 70-130mm×8-13mm×80-120mm, the forging is one of room temperature forging or warm forging, the room temperature forging temperature is room temperature, the warm forging temperature is 150-350℃, and the forging method is closed die forging; the powder metallurgy pure aluminum heat sink blank is a multi-needle aluminum heat sink.

[0023] Optionally, the annealing atmosphere for stress relief annealing in S6 can be one of air atmosphere, nitrogen atmosphere, and vacuum atmosphere, the annealing temperature is 300-550°C, the time is 20-180min, the tensile strength of the low residual stress powder metallurgy pure aluminum heat sink blank is 190-280MPa, the yield strength is 140-230MPa, the yield strength ratio is 0.73-0.83, the elongation is 30-40%, the hardness is 42-55HV, the residual strength value after annealing at 350°C is 91-93%, and the thermal conductivity is 232-237W / (m·K).

[0024] Optionally, the finishing process in S7 is to remove forging residues and perform drilling for assembly, and the performance of the aluminum heat sink product is not changed after the finishing process.

[0025] Technical principle of the present invention:

[0026] (1) Due to the very active nature of metallic aluminum, an aluminum oxide film with a thickness of nanometer scale will be formed on the surface during the powder making process. These aluminum oxide films will form discontinuous segmented structures after pressing and sintering. The nanometer-scale aluminum oxide particles formed after extrusion and forging deformation can play a role in dispersion strengthening and pin dislocations and grain boundaries. Therefore, high-strength powder metallurgy aluminum is obtained under the multiple strengthening mechanisms of fine grain strengthening, dislocation strengthening and dispersion strengthening.

[0027] (2) Since the heat sink used in new energy vehicles needs to undergo pre-deformation and welding processes during assembly, high temperatures exist in the environment of these processes. Alumina is very stable in these temperature ranges. During the heating process of the product, alumina can still pin dislocations and grain boundaries, giving it excellent heat resistance.

[0028] (3) The heat transfer nature of pure metal materials is mainly the movement of free electrons. Nano-alumina particles will not cause lattice distortion of the matrix, and their mass fraction is very low, rarely causing electron scattering. Therefore, the heat sink prepared by this preparation method can maintain a high thermal conductivity while having high strength and high heat resistance.

[0029] Compared with the prior art, the above technical solution has at least the following beneficial effects:

[0030] The above scheme, the present invention proposes a method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, which can solve many technical problems existing in the prior art in order to improve the performance of high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, thereby making the mechanical properties, thermal conductivity and heat resistance of the prepared heat sink synergistically improved.

[0031] The present invention forms an aluminum oxide film with a thickness of nanometer scale on the surface during the powder making process, and processes the aluminum oxide film in situ generated on the surface of the aluminum powder into nanometer scale aluminum oxide particles after extrusion and forging deformation, so that the product has high strength, excellent heat resistance and thermal conductivity.

[0032] The present invention requires pre-deformation and welding processes during assembly. Through the pinning dislocation and grain boundary effects of stable aluminum oxide at high temperatures, the heat resistance of the heat dissipation aluminum plate at high temperatures is improved, so that the heat dissipation aluminum plate can dissipate heat stably and efficiently, and its service life is extended.

[0033] The low residual stress powder metallurgy pure aluminum heat sink blank subjected to stress relief annealing of the present invention has a tensile strength of 190-280 MPa, a yield strength of 140-230 MPa, a yield strength ratio of 0.73-0.83, an elongation of 30-40%, a hardness of 42-55 HV, a strength residual value of 91-93% after annealing at 350°C, and a thermal conductivity of 232-237 W / (m·K).

[0034] The performance of the aluminum heat sink product is not changed after fine processing.

[0035] In summary, compared with other traditional methods, the method of the present invention, through the process selection of powder making, cold isostatic pressing, sintering, hot deformation, forging, stress relief annealing and finishing, makes the prepared alloy powder used in the preparation of heat dissipation aluminum plate able to synergistically improve its mechanical properties, thermal conductivity and heat resistance; it has high resource utilization, low cost, short process and high efficiency, which is conducive to large-scale industrial production and promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0037] Figure 1 This is a microstructure diagram of the distribution of aluminum oxide after sintering in the method for preparing a high-strength, high-thermal-conductivity, and heat-resistant aluminum heat sink for new energy vehicles according to Example 1 of the present invention;

[0038] Figure 2 This is a microstructure diagram of aluminum oxide distribution after extrusion and forging in a method for preparing a high-strength, high-thermal-conductivity, and heat-resistant aluminum heat sink for new energy vehicles according to Example 1 of the present invention;

[0039] Figure 3 This is a grain size diagram of a final product in a method for preparing a high-strength, high-thermal-conductivity, and heat-resistant aluminum heat sink for new energy vehicles according to Example 1 of the present invention. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is described below in conjunction with the accompanying drawings.

[0041] In the embodiments of the present invention, words such as "exemplarily" and "for example" are used to indicate examples, illustrations or explanations. Any embodiment or design described as "example" in the present invention should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of the word "example" is intended to present the concept in a specific way. In addition, in the embodiments of the present invention, the meaning expressed by "and / or" can be both, or it can be either of the two.

[0042] In the embodiments of the present invention, "image" and "picture" may sometimes be used interchangeably. It should be noted that when the distinction between them is not emphasized, the meanings they intend to express are consistent.

[0043] In the embodiments of the present invention, sometimes a subscript such as W1 may be written as a non-subscript such as W1. When the difference is not emphasized, the meanings to be expressed are the same.

[0044] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0045] A method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, the method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles comprises the following steps:

[0046] S1. Preparation of ultrafine ultrapure aluminum powder: preparing pure aluminum powder from molten aluminum by gas atomization;

[0047] S2, powder forming: S1 pure aluminum powder is encapsulated in a silicone sheath or a rubber sheath, and is formed by cold isostatic pressing to obtain an aluminum green body;

[0048] S3, compact sintering and densification: the S2 aluminum green billet is subjected to pressureless sintering or pressure sintering to obtain an aluminum billet;

[0049] S4, aluminum ingot hot extrusion forming: S3 aluminum ingot is subjected to hot deformation processing to prepare fully dense aluminum sheet and strip;

[0050] S5, forging and forming of aluminum heat sink: cutting the fully dense aluminum sheet and strip in S4 to obtain cut aluminum sheet and strip, forging the cut aluminum sheet and strip, and finally obtaining a powder metallurgy pure aluminum heat sink blank;

[0051] S6. Stress relief annealing of aluminum heat sink: using corresponding process to perform stress relief annealing on the aluminum heat sink to obtain a low residual stress powder metallurgy pure aluminum heat sink blank;

[0052] S7, mechanical processing: fine-processing the powder metallurgy aluminum heat sink blank obtained above to finally obtain an aluminum heat sink product.

[0053] In particular, the gas atomization in S1 is nitrogen atomization, the temperature of the molten aluminum liquid is 830-900°C, the nitrogen pressure is 6.5-8.0MPa, and the obtained pure aluminum powder is spherical and / or nearly spherical in shape, with an average particle size of 2-40μm and a surface oxide film thickness of 10-100nm.

[0054] In particular, the size of the silicone sheath in S2 is 250-300 mm×800-900 mm, the cold isostatic pressing is performed at a pressure of 120-250 MPa for 80-240 seconds, and the size of the aluminum green billet is 200-220 mm×600-700 mm.

[0055] In particular, the pressureless sintering in S3 is carried out in a nitrogen atmosphere at 350-400°C for 0.5-1h, and then the temperature is continuously raised at a rate of 3-7°C / min to a sintering temperature of 590-640°C, and the temperature is maintained for 2-8h, and the relative density reaches above 97.7%.

[0056] In particular, the vacuum sintering in S3 is carried out in a vacuum atmosphere at 350-400°C for 0.5-1h, and then the temperature is continuously raised at a rate of 3-7°C / min to a sintering temperature of 590-640°C, and the temperature is maintained for 2-8h, and the relative density reaches more than 97.5%.

[0057] In particular, the pressure sintering in S3 is carried out under a pressure environment, with the temperature rising to 580-640°C at a rate of 3-7°C / min, pre-sintering for 20-60 minutes, and then cooling by 10-20°C. At the same time, nitrogen is used to increase the gas pressure to 3-10MPa, and low-pressure sintering is carried out for 2-7 hours, and the relative density reaches 100%.

[0058] In particular, the hot deformation processing technology in S4 is hot extrusion, the hot extrusion temperature is 300-550°C, the deformation amount is 10-100%, and the cross-section of the fully dense aluminum sheet and strip is 70-130mm wide and 8-13mm thick.

[0059] In particular, the size of the aluminum plate strip after cutting in S5 is 70-130mm×8-13mm×80-120mm, the forging is one of room temperature forging or warm forging, the room temperature forging temperature is room temperature, the warm forging temperature is 150-350℃, and the forging method is closed die forging; the powder metallurgy pure aluminum heat sink blank is a multi-needle aluminum heat sink.

[0060] In particular, the annealing atmosphere for stress relief annealing in S6 can be one of air atmosphere, nitrogen atmosphere, and vacuum atmosphere, the annealing temperature is 300-550°C, the time is 20-180min, the tensile strength of the low residual stress powder metallurgy pure aluminum heat sink blank is 190-280MPa, the yield strength is 140-230MPa, the yield strength ratio is 0.73-0.83, the elongation is 30-40%, the hardness is 42-55HV, the residual strength value after annealing at 350°C is 91-93%, and the thermal conductivity is 232-237W / (m·K).

[0061] In particular, the finishing process in S7 is to remove the forging residues and perform drilling for assembly. The performance of the aluminum heat sink product is not changed after finishing.

[0062] Example 1

[0063] A method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, the method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles comprises the following steps:

[0064] S1. Preparation of ultrafine ultrapure aluminum powder: preparing pure aluminum powder from molten aluminum by gas atomization; wherein the gas atomization is nitrogen atomization, the temperature of the molten aluminum is 900° C., the nitrogen pressure is 8.0 MPa, and the obtained pure aluminum powder is spherical and / or nearly spherical in shape, with an average particle size of 2-5 μm and a surface oxide film thickness of 10-50 nm;

[0065] S2, powder forming: S1 pure aluminum powder is encapsulated in a silicone sheath or a rubber sheath, the size of the silicone sheath is 270 mm in diameter × 900 mm in length; cold isostatic pressing is performed, and the cold isostatic pressing is performed at a pressure of 180 MPa for 150 seconds to obtain an aluminum green billet with a size of 203 mm in diameter × 600 mm;

[0066] S3, compact sintering densification: S2 aluminum green billet is subjected to pressureless sintering to obtain aluminum ingot. After sintering, the microstructure of alumina distribution is as follows: Figure 1 As shown; the pressureless sintering is carried out in a nitrogen atmosphere at 400°C for 2 hours, and then the temperature is continued to rise at a rate of 4°C / min to a sintering temperature of 640°C, and the temperature is kept for 3 hours, and the relative density reaches 98.8%;

[0067] S4, hot extrusion forming of aluminum ingot: the S3 aluminum ingot is subjected to a hot deformation process, the hot deformation process is hot extrusion, the hot extrusion temperature is 450°C, the deformation amount is 97.6%, and a fully dense aluminum plate strip with a cross-sectional width of 80 mm and a thickness of 10 mm is prepared;

[0068] S5. Forging of aluminum heat sink: The fully dense aluminum sheet and strip of S4 are cut to obtain the cut aluminum sheet and strip. The size of the cut aluminum sheet and strip is 134 mm long × 80 mm wide × 10 mm thick. The forging is room temperature forging. The room temperature forging temperature is room temperature. The forging method is closed die forging. The cut aluminum sheet and strip are forged to finally obtain a powder metallurgy pure aluminum heat sink blank. The powder metallurgy pure aluminum heat sink blank is a multi-needle aluminum heat sink. The microstructure of the aluminum oxide distribution after extrusion and forging is as follows: Figure 2 As shown;

[0069] S6. Stress relief annealing of aluminum heat sink: The aluminum heat sink is subjected to stress relief annealing by a corresponding process to obtain a low residual stress powder metallurgy pure aluminum heat sink blank; wherein the annealing atmosphere for stress relief annealing can be one of air atmosphere, nitrogen atmosphere, and vacuum atmosphere, the annealing temperature is 450°C, the time is 15min, the tensile strength of the low residual stress powder metallurgy pure aluminum heat sink blank is 280MPa, the yield strength is 230MPa, the yield strength ratio is 0.82, the elongation is 30%, the hardness is 55HV, and the residual strength value after annealing at 350°C is 93%, and the thermal conductivity is 232W / (m·K); the grain size of the final product is as follows Figure 3 As shown;

[0070] S7. Mechanical processing: The powder metallurgy aluminum heat sink blank obtained above is subjected to fine processing to finally obtain an aluminum heat sink product; wherein, the fine processing is to remove the forging residues and perform drilling for assembly, and the performance of the aluminum heat sink product is not changed after fine processing.

[0071] Example 2

[0072] A method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, the method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles comprises the following steps:

[0073] S1. Preparation of ultrafine ultrapure aluminum powder: preparing pure aluminum powder from molten aluminum by gas atomization; wherein the gas atomization is nitrogen atomization, the temperature of the molten aluminum is 850°C, the nitrogen pressure is 6.5MPa, and the obtained pure aluminum powder is spherical and / or nearly spherical in shape, with an average particle size of 15-30μm and a surface oxide film thickness of 20-70nm;

[0074] S2, powder forming: S1 pure aluminum powder is encapsulated in a silicone sheath or a rubber sheath, the size of the silicone sheath is 260 mm in diameter × 800 mm; cold isostatic pressing is performed, and the cold isostatic pressing is performed at a pressure of 180 MPa for 150 seconds to obtain an aluminum green billet with a size of 210 mm in diameter × 650 mm in length;

[0075] S3, compact sintering densification: vacuum sinter the S2 aluminum green billet to obtain an aluminum ingot; vacuum sintering is performed under vacuum atmosphere at a rate of 4°C / min, rising to a sintering temperature of 610°C, keeping the temperature for 1 hour, and the relative density reaches 98.1%;

[0076] S4, aluminum ingot hot extrusion forming: The S3 aluminum ingot is subjected to a hot deformation process, wherein the hot deformation process is hot extrusion, the hot extrusion temperature is 460°C, the deformation amount is 97%, and a fully dense aluminum plate strip with a cross-sectional width of 80 mm and a thickness of 10 mm is prepared;

[0077] S5. Forging of aluminum heat sink: The fully dense aluminum sheet and strip of S4 are cut to obtain cut aluminum sheet and strip, the size of the cut aluminum sheet and strip is 134 mm long × 80 mm wide × 10 mm thick, the forging is room temperature forging, the room temperature forging temperature is room temperature, and the forging method is closed die forging; the cut aluminum sheet and strip are forged to finally obtain a powder metallurgy pure aluminum heat sink blank; the powder metallurgy pure aluminum heat sink blank is a multi-needle aluminum heat sink;

[0078] S6. Stress relief annealing of aluminum heat sink: Use corresponding process to perform stress relief annealing on aluminum heat sink to obtain low residual stress powder metallurgy pure aluminum heat sink blank; wherein, the annealing atmosphere of stress relief annealing can be one of air atmosphere, nitrogen atmosphere and vacuum atmosphere, the annealing temperature is 400℃, the time is 15min, the tensile strength of low residual stress powder metallurgy pure aluminum heat sink blank is 210MPa, the yield strength is 180MPa, the yield strength ratio is 0.76, the elongation is 34%, the hardness is 45HV, and the residual strength value after annealing at 350℃ is 91.7%, and the thermal conductivity is 235W / (m·K);

[0079] S7. Mechanical processing: The powder metallurgy aluminum heat sink blank obtained above is subjected to fine processing to finally obtain an aluminum heat sink product; wherein, the fine processing is to remove the forging residues and perform drilling for assembly, and the performance of the aluminum heat sink product is not changed after fine processing.

[0080] Example 3

[0081] A method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, the method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles comprises the following steps:

[0082] S1. Preparation of ultrafine ultrapure aluminum powder: preparing pure aluminum powder from molten aluminum by gas atomization; wherein the gas atomization is nitrogen atomization, the temperature of the molten aluminum is 830° C., the nitrogen pressure is 6.5 MPa, and the obtained pure aluminum powder is spherical and / or nearly spherical in shape, with an average particle size of 25-40 μm and a surface oxide film thickness of 55-100 nm;

[0083] S2, powder forming: S1 pure aluminum powder is encapsulated in a silicone sheath or a rubber sheath, the size of the silicone sheath is 255 mm in diameter and 800 mm in length; cold isostatic pressing is performed, and the cold isostatic pressing is performed at a pressure of 180 MPa for 150 seconds to obtain an aluminum green billet with a size of 210 mm in diameter and 650 mm in length;

[0084] S3, compact sintering densification: S2 aluminum green billet is pressure sintered to obtain aluminum ingot; pressure sintering is carried out in a vacuum atmosphere, at a rate of 5 °C / min, the sintering temperature is raised to 600 °C, the temperature is kept for 1 hour, and nitrogen is used to increase the gas pressure to 5MPa, and hot isostatic pressing is performed for 1 hour, and the relative density reaches 100%;

[0085] S4, aluminum ingot hot extrusion forming: The S3 aluminum ingot is subjected to a hot deformation process, wherein the hot deformation process is hot extrusion, the hot extrusion temperature is 420°C, the deformation amount is 97%, and a fully dense aluminum plate strip with a cross-sectional width of 80 mm and a thickness of 10 mm is prepared;

[0086] S5. Forging of aluminum heat sink: The fully dense aluminum sheet and strip of S4 are cut to obtain cut aluminum sheet and strip, the size of the cut aluminum sheet and strip is 134 mm long × 80 mm wide × 10 mm thick, the forging is room temperature forging, the room temperature forging temperature is room temperature, and the forging method is closed die forging; the cut aluminum sheet and strip are forged to finally obtain a powder metallurgy pure aluminum heat sink blank; the powder metallurgy pure aluminum heat sink blank is a multi-needle aluminum heat sink;

[0087] S6. Stress relief annealing of aluminum heat sink: The aluminum heat sink is subjected to stress relief annealing by a corresponding process to obtain a low residual stress powder metallurgy pure aluminum heat sink blank; wherein the annealing atmosphere for stress relief annealing can be one of air atmosphere, nitrogen atmosphere, and vacuum atmosphere, the annealing temperature is 400°C, the time is 15min, the tensile strength of the low residual stress powder metallurgy pure aluminum heat sink blank is 190MPa, the yield strength is 140MPa, the yield strength ratio is 0.72, the elongation is 36%, the hardness is 42HV, the residual strength value after annealing at 350°C is 91%, and the thermal conductivity is 237W / (m·K);

[0088] S7. Mechanical processing: The powder metallurgy aluminum heat sink blank obtained above is subjected to fine processing to finally obtain an aluminum heat sink product; wherein, the fine processing is to remove the forging residues and perform drilling for assembly, and the performance of the aluminum heat sink product is not changed after fine processing.

[0089] Example 4

[0090] A method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, the method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles comprises the following steps:

[0091] S1. Preparation of ultrafine ultrapure aluminum powder: preparing pure aluminum powder from molten aluminum by gas atomization; wherein the gas atomization is nitrogen atomization, the temperature of the molten aluminum is 830° C., the nitrogen pressure is 7.5 MPa, and the obtained pure aluminum powder is spherical and / or nearly spherical in shape, with an average particle size of 20-35 μm and a surface oxide film thickness of 40-90 nm;

[0092] S2, powder forming: S1 pure aluminum powder is encapsulated in a silicone sheath or a rubber sheath, the size of the silicone sheath is 300mm×900mm; cold isostatic pressing is performed, and the cold isostatic pressing is performed at a pressure of 180MPa for 150s to obtain an aluminum green billet with a size of 278mm×700mm;

[0093] S3, compact sintering densification: S2 aluminum green billet is subjected to pressureless sintering to obtain aluminum billet; pressureless sintering is carried out in a nitrogen atmosphere at 400°C for 30 minutes, and then the temperature is continuously raised at a rate of 4°C / min to a sintering temperature of 610°C, and the temperature is maintained for 3 hours, and the relative density reaches 98.3%;

[0094] S4, aluminum ingot hot extrusion forming: the S3 aluminum ingot is subjected to a hot deformation process, the hot deformation process is hot extrusion, the hot extrusion temperature is 420°C, the deformation amount is 98.3%, and a fully dense aluminum plate strip with a cross-sectional width of 100 mm and a thickness of 10 mm is prepared;

[0095] S5. Forging of aluminum heat sink: The fully dense aluminum sheet and strip of S4 is cut to obtain a cut aluminum sheet and strip, the size of the cut aluminum sheet and strip is 100mm×100mm×10mm, the forging is room temperature forging, the room temperature forging temperature is room temperature, and the forging method is closed die forging; the cut aluminum sheet and strip are forged to finally obtain a powder metallurgy pure aluminum heat sink blank; the powder metallurgy pure aluminum heat sink blank is a multi-needle aluminum heat sink;

[0096] S6. Stress relief annealing of aluminum heat sink: stress relief annealing is performed on the aluminum heat sink by using corresponding processes to obtain a low residual stress powder metallurgy pure aluminum heat sink blank; wherein the annealing atmosphere for stress relief annealing can be one of air atmosphere, nitrogen atmosphere, and vacuum atmosphere, the annealing temperature is 350°C, the time is 25min, the tensile strength of the low residual stress powder metallurgy pure aluminum heat sink blank is 205MPa, the yield strength is 155MPa, the yield strength ratio is 0.756, the elongation is 38%, the hardness is 43HV, and the residual strength value after annealing at 350°C is 91.7%, and the thermal conductivity is 233W / (m·K);

[0097] S7. Mechanical processing: The powder metallurgy aluminum heat sink blank obtained above is subjected to fine processing to finally obtain an aluminum heat sink product; wherein, the fine processing is to remove the forging residues and perform drilling for assembly, and the performance of the aluminum heat sink product is not changed after fine processing.

[0098] Example 5

[0099] A method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, the method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles comprises the following steps:

[0100] S1. Preparation of ultrafine ultrapure aluminum powder: preparing pure aluminum powder from molten aluminum by gas atomization; wherein the gas atomization is nitrogen atomization, the temperature of the molten aluminum is 870° C., the nitrogen pressure is 7 MPa, and the obtained pure aluminum powder is spherical and / or nearly spherical in shape, with an average particle size of 13-25 μm and a surface oxide film thickness of 15-65 nm;

[0101] S2, powder forming: S1 pure aluminum powder is encapsulated in a silicone sheath or a rubber sheath, the size of the silicone sheath is 295mm×870mm; after cold isostatic pressing, the cold isostatic pressing is carried out at a pressure of 180MPa and the pressure is maintained for 150s to obtain an aluminum green billet with a size of 278mm×700mm;

[0102] S3, compact sintering densification: vacuum sinter the S2 aluminum green billet to obtain an aluminum ingot; pressure sintering is carried out in a vacuum atmosphere at a rate of 4°C / min, rising to a sintering temperature of 620°C, and keeping the temperature for 3 hours, and the relative density reaches 98.1%;

[0103] S4, aluminum ingot hot extrusion forming: the S3 aluminum ingot is subjected to a hot deformation process, the hot deformation process is hot extrusion, the hot extrusion temperature is 490°C, the deformation amount is 97.3%, and a fully dense aluminum plate strip with a cross-sectional width of 100 mm and a thickness of 10 mm is prepared;

[0104] S5. Forging of aluminum heat sink: The fully dense aluminum sheet and strip of S4 is cut to obtain a cut aluminum sheet and strip, the size of the cut aluminum sheet and strip is 100mm×100mm×10mm, the forging is room temperature forging, the room temperature forging temperature is room temperature, and the forging method is closed die forging; the cut aluminum sheet and strip are forged to finally obtain a powder metallurgy pure aluminum heat sink blank; the powder metallurgy pure aluminum heat sink blank is a multi-needle aluminum heat sink;

[0105] S6. Stress relief annealing of aluminum heat sink: stress relief annealing is performed on the aluminum heat sink by using corresponding processes to obtain a low residual stress powder metallurgy pure aluminum heat sink blank; wherein the annealing atmosphere for stress relief annealing can be one of air atmosphere, nitrogen atmosphere, and vacuum atmosphere, the annealing temperature is 380°C, the time is 25min, the tensile strength of the low residual stress powder metallurgy pure aluminum heat sink blank is 230MPa, the yield strength is 190MPa, the yield strength ratio is 0.826, the elongation is 35%, the hardness is 46HV, after annealing at 350°C, the residual strength value is 91.9%, and the thermal conductivity is 235W / (m·K);

[0106] S7. Mechanical processing: The powder metallurgy aluminum heat sink blank obtained above is subjected to fine processing to finally obtain an aluminum heat sink product; wherein, the fine processing is to remove the forging residues and perform drilling for assembly, and the performance of the aluminum heat sink product is not changed after fine processing.

[0107] Example 6

[0108] A method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, the method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles comprises the following steps:

[0109] S1. Preparation of ultrafine ultrapure aluminum powder: preparing pure aluminum powder from molten aluminum by gas atomization; wherein the gas atomization is nitrogen atomization, the temperature of the molten aluminum is 900° C., the nitrogen pressure is 7.5 MPa, and the obtained pure aluminum powder is spherical and / or nearly spherical in shape, with an average particle size of 5-15 μm and a surface oxide film thickness of 13-65 nm;

[0110] S2, powder forming: S1 pure aluminum powder is encapsulated in a silicone sheath or a rubber sheath, the size of the silicone sheath is 265mm×850mm; cold isostatic pressing is performed, and the cold isostatic pressing is performed at a pressure of 180MPa for 150s to obtain an aluminum green billet with a size of 203mm×630mm;

[0111] S3, compact sintering densification: S2 aluminum green billet is subjected to pressureless sintering to obtain aluminum billet; pressure sintering is carried out in a vacuum atmosphere, at a rate of 4°C / min, the sintering temperature is raised to 630°C, the temperature is kept at that temperature for 30 minutes, and after cooling to 620°C, 5MPa nitrogen is introduced into the furnace, and the relative density reaches 100%;

[0112] S4, aluminum ingot hot extrusion forming: The S3 aluminum ingot is subjected to a hot deformation process, wherein the hot deformation process is hot extrusion, the hot extrusion temperature is 480°C, the deformation amount is 96.5%, and a fully dense aluminum plate strip with a cross-sectional width of 110 mm and a thickness of 10 mm is prepared;

[0113] S5. Forging of aluminum heat sink: The fully dense aluminum sheet and strip of S4 is cut to obtain a cut aluminum sheet and strip, the size of the cut aluminum sheet and strip is 100 mm×110 mm×10 mm, the forging is room temperature forging, the room temperature forging temperature is room temperature, and the forging method is closed die forging; the cut aluminum sheet and strip are forged to finally obtain a powder metallurgy pure aluminum heat sink blank; the powder metallurgy pure aluminum heat sink blank is a multi-needle aluminum heat sink;

[0114] S6. Stress relief annealing of aluminum heat sink: stress relief annealing is performed on the aluminum heat sink by using corresponding processes to obtain a low residual stress powder metallurgy pure aluminum heat sink blank; wherein the annealing atmosphere for stress relief annealing can be one of air atmosphere, nitrogen atmosphere, and vacuum atmosphere, the annealing temperature is 430°C, the time is 25min, the tensile strength of the low residual stress powder metallurgy pure aluminum heat sink blank is 270MPa, the yield strength is 220MPa, the yield strength ratio is 0.814, the elongation is 32%, the hardness is 52HV, after annealing at 350°C, the residual strength value is 92.6%, and the thermal conductivity is 232W / (m·K);

[0115] S7. Mechanical processing: The powder metallurgy aluminum heat sink blank obtained above is subjected to fine processing to finally obtain an aluminum heat sink product; wherein, the fine processing is to remove the forging residues and perform drilling for assembly, and the performance of the aluminum heat sink product is not changed after fine processing.

[0116] The above scheme, the present invention proposes a method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, which can solve many technical problems existing in the prior art in order to improve the performance of high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, thereby making the mechanical properties, thermal conductivity and heat resistance of the prepared heat sink synergistically improved.

[0117] The present invention forms an aluminum oxide film with a thickness of nanometer scale on the surface during the powder making process, and processes the aluminum oxide film in situ generated on the surface of the aluminum powder into nanometer scale aluminum oxide particles after extrusion and forging deformation, so that the product has high strength, excellent heat resistance and thermal conductivity.

[0118] The present invention requires pre-deformation and welding processes during assembly. Through the pinning dislocation and grain boundary effects of stable aluminum oxide at high temperatures, the heat resistance of the heat dissipation aluminum plate at high temperatures is improved, so that the heat dissipation aluminum plate can dissipate heat stably and efficiently, and its service life is extended.

[0119] The low residual stress powder metallurgy pure aluminum heat sink blank subjected to stress relief annealing of the present invention has a tensile strength of 190-280 MPa, a yield strength of 140-230 MPa, a yield strength ratio of 0.73-0.83, an elongation of 30-40%, a hardness of 42-55 HV, a residual strength value of 91-93% after annealing at 350° C., and a thermal conductivity of 232-237 W / (m·K).

[0120] The performance of the aluminum heat sink product is not changed after fine processing.

[0121] In summary, compared with other traditional methods, the method of the present invention, through the process selection of powder making, cold isostatic pressing, sintering, hot deformation, forging, stress relief annealing and finishing, makes the prepared alloy powder used in the preparation of heat dissipation aluminum plate able to synergistically improve its mechanical properties, thermal conductivity and heat resistance; it has high resource utilization, low cost, short process and high efficiency, which is conducive to large-scale industrial production and promotion.

[0122] It should be understood that the term "and / or" in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship, but it may also indicate an "and / or" relationship. Please refer to the context for specific understanding.

[0123] In the present invention, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, at least one of a, b, or c can mean: a, b, c, ab, ac, bc, or abc, where a, b, and c can be single or multiple.

[0124] It should be understood that in various embodiments of the present invention, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.

[0125] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles, characterized in that: The preparation method of the high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles comprises the following steps: S1. Preparation of ultrafine ultrapure aluminum powder: preparing pure aluminum powder from molten aluminum by gas atomization; S2, powder forming: S1 pure aluminum powder is encapsulated in a silicone sheath or a rubber sheath, and is formed by cold isostatic pressing to obtain an aluminum green body; S3, compact sintering and densification: the S2 aluminum green billet is subjected to pressureless sintering or pressure sintering to obtain an aluminum billet; S4, aluminum ingot hot extrusion forming: S3 aluminum ingot is subjected to hot deformation processing to prepare fully dense aluminum sheet and strip; S5, forging and forming of aluminum heat sink: cutting the fully dense aluminum sheet and strip in S4 to obtain cut aluminum sheet and strip, forging the cut aluminum sheet and strip, and finally obtaining a powder metallurgy pure aluminum heat sink blank; S6. Stress relief annealing of aluminum heat sink: using corresponding process to perform stress relief annealing on the aluminum heat sink to obtain a low residual stress powder metallurgy pure aluminum heat sink blank; S7, mechanical processing: fine-processing the powder metallurgy aluminum heat sink blank obtained above to finally obtain an aluminum heat sink product.

2. The method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles according to claim 1, characterized in that: The gas atomization in S1 is nitrogen atomization, the temperature of the molten aluminum liquid is 830-900°C, the nitrogen pressure is 6.5-8.0MPa, and the obtained pure aluminum powder is spherical and / or nearly spherical in shape, with an average particle size of 2-40μm and a surface oxide film thickness of 10-100nm.

3. The method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles according to claim 1, characterized in that: The size of the silicone sheath in S2 is 250-300mm×800-900mm, the cold isostatic pressing is performed at a pressure of 120-250MPa for 80-240s, and the size of the aluminum green billet is 200-220mm×600-700mm.

4. The method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles according to claim 1, characterized in that: The pressureless sintering in S3 is carried out in a nitrogen atmosphere at 350-400°C for 0.5-1h, and then the temperature is continued to rise at a rate of 3-7°C / min to a sintering temperature of 590-640°C, and kept for 2-8h, and the relative density reaches more than 97.7%.

5. The method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles according to claim 1, characterized in that: The vacuum sintering in S3 is carried out in a vacuum atmosphere at 350-400°C for 0.5-1h, and then the temperature is continuously raised at a rate of 3-7°C / min to a sintering temperature of 590-640°C, and the temperature is maintained for 2-8h, and the relative density reaches more than 97.5%.

6. The method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles according to claim 1, characterized in that: The pressure sintering in S3 is carried out under pressure environment, at a rate of 3-7℃ / min, the sintering temperature is raised to 580-640℃, kept at this temperature for 20-60min for pre-sintering, then cooled by 10-20℃, and nitrogen is used to increase the air pressure to 3-10MPa, and low-pressure sintering is carried out for 2-7h, and the relative density reaches 100%.

7. The method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles according to claim 1, characterized in that: The hot deformation processing technology of S4 is hot extrusion, the hot extrusion temperature is 300-550℃, the deformation amount is 10-100%, and the cross-section width of the fully dense aluminum plate and strip is 70-130mm and the thickness is 8-13mm.

8. The method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles according to claim 1, characterized in that: The size of the aluminum plate strip after cutting in S5 is 70-130mm×8-13mm×80-120mm, the forging is one of room temperature forging or warm forging, the room temperature forging temperature is room temperature, the warm forging temperature is 150-350℃, and the forging method is closed die forging; the powder metallurgy pure aluminum heat sink blank is a multi-needle aluminum heat sink.

9. The method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles according to claim 1, characterized in that: The annealing atmosphere for stress relief annealing in S6 can be one of air atmosphere, nitrogen atmosphere and vacuum atmosphere. The annealing temperature is 300-550℃, the time is 20-180min, and the tensile strength of the low residual stress powder metallurgy pure aluminum heat sink blank is 190-280MPa, the yield strength is 140-230MPa, the yield strength ratio is 0.73-0.83, the elongation is 30-40%, the hardness is 42-55HV, and the residual strength value after annealing at 350℃ is 91-93%, and the thermal conductivity is 232-237W / (m·K).

10. The method for preparing a high-strength, high-thermal-conductivity, heat-resistant aluminum heat sink for new energy vehicles according to claim 1, characterized in that: The finishing process in S7 is to remove the forging residues and drill holes for assembly. The performance of the aluminum heat sink product will not be changed after finishing.

Citation Information

Patent Citations

  • Preparation method and smelting device of high-strength and high-thermal-conductivity aluminum alloy

    CN115058614A

  • Preparation method of high-strength and high-thermal-conductivity aluminum alloy material

    CN115261660A

  • High-conductivity and high-heat-resistance die-casting aluminum alloy for new energy automobile and preparation method thereof

    CN116463529A

Cited By

  • Stainless steel water pump impeller and manufacturing method thereof

    CN119508264A

  • Cold forging forming process for red copper IGBT (Insulated Gate Bipolar Translator) radiating substrate

    CN121083329A

  • A red copper IGBT heat dissipation substrate cold forging forming process