Continuous production of carbon foam structures at atmospheric pressure
Through the continuous kiln process under atmospheric pressure and inert atmosphere, the problems of high cost and low efficiency of autoclave manufacturing process are solved, and the production of high-quality crack-free carbon foam is achieved, which has enhanced the market potential.
Patent Information
- Application Number
- CN202380024999.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-01
- Filing Date
- 2023-02-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure CN118891228A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This patent application claims the benefit of provisional patent application 63 / 315,235 filed on March 1, 2022, the entire contents of which are incorporated herein by reference in their entirety.
[0003] Statement Regarding Federally Funded Research
[0004] This invention was made with government support under Grant DE-FE0031992 from the Department of Energy. The government has certain rights in this invention. Technical Field
[0005] The present invention relates to a method for manufacturing carbon foam structures in a single piece flow through a continuous kiln under an inert atmosphere at atmospheric pressure. The process can significantly reduce manufacturing costs by reducing manufacturing time and improving the ability to integrate automated equipment. Background Art
[0006] In a typical carbon-containing carbon foam manufacturing process, coal is heated in a nitrogen atmosphere so that it does not burn. The precursor first melts when heated, and then releases gases to foam the material. The foaming step is usually carried out under high pressure (about 400psi) to help regulate the rate at which the precursor transforms into a liquid phase, forms bubbles and reacts to form a solid foam, thereby producing a high-quality foam. This foaming step is carried out at a temperature of about 25°C to 470°C, during which oxygen and some hydrogen are eliminated. The foam product is then fired in a kiln under nitrogen at atmospheric pressure to eliminate most of the remaining hydrogen and further cross-link the carbon until only glassy carbon remains at 1000°C.
[0007] Making carbon-containing carbon foams at high pressures in autoclaves is expensive, time-consuming, capital-intensive, and limited to batch operations. In addition, the size of the product is limited to the size of the autoclave that the process conditions allow, or certainly to the size of the autoclave that the company can afford. The higher the pressure, the more expensive the autoclave, and the more its size is limited by engineering constraints. As a result, the market for carbon foams has been limited and the market size has remained small because the cost has been high. In order to reach a larger, broader market, the cost of the current process must be reduced by making carbon foams in a continuous manner at atmospheric pressure. This task has been difficult given the advantages provided by high pressure, which helps regulate the reactions that occur when coal is heated. When carbon foam processing is carried out at atmospheric pressure, the reaction rate of the coal is altered, making it more difficult to form an attractive, crack-free carbon foam.
[0008] Thus, suitable substantially crack-free carbon foam cannot be produced when coal is simply added to a vessel and conveyed through a continuous kiln using a thermal profile similar to that used in an autoclave. Figure 1As shown, a typical carbon foam board produced in an autoclave using only coal processed under high pressure is essentially crack-free; some extraneous cracks may be seen on the surface of the raw bun coming out of the autoclave, but these are easily processed away to reveal crack-free sections. When coal is simply added to a container and conveyed through a continuous kiln using a thermal profile similar to that used in an autoclave, it is not possible to produce such a carbon foam board. Figure 1 Attractive carbon foam parts as shown. Figure 2 and Figure 3 As shown in Figure 1, even relatively small parts produced in this way can produce cracks and unsightly products, with the control sample made using only coal mined from the Bailey coal mine near Graysville, Pennsylvania, USA. Both were processed in a continuous kiln, using Figure 4 A “good” thermal curve is shown. Figure 3 The sample diameter is 8 inches, Figure 4 The samples were 9.5 inches by 12 inches. Note that both samples contained large cracks 10. Based on these results, it is clear that additional controls are needed to produce a substantially crack-free product. Summary of the invention
[0009] A continuous method for producing a substantially crack-free carbon foam structure comprises the following steps: pulverizing a carbonaceous feedstock into a powder; mixing the powder and at least one of a chemical additive or a particulate additive to form a coal mixture; placing the coal mixture into a carbon foam structure mold, the carbon foam structure mold being configured to be continuously processed in a kiln at atmospheric pressure and under an inert gas; heating the mold and the coal mixture at a kiln temperature of about 700°F under the inert gas at a rate of about 6°F per minute; maintaining the kiln temperature at about 700°F for a period of time to heat treat the coal mixture; further heating the mold and the coal mixture in the kiln at a temperature of about 900°F until a carbon foam structure is formed; and cooling the carbon foam structure under atmospheric conditions; wherein the carbon foam structure is substantially crack-free.
[0010] A substantially crack-free carbon foam structure made by a continuous process, the method comprising the steps of: pulverizing a carbonaceous feedstock into a powder; mixing the powder and at least one of a chemical additive or a particulate additive to form a coal mixture; placing the coal mixture into a carbon foam structure mold, the carbon foam structure mold being configured to be continuously processed in a kiln at atmospheric pressure and in an inert atmosphere; heating the mold and the coal mixture at a kiln temperature of about 700°F under the inert gas at a rate of about 6°F per minute; maintaining the kiln temperature at about 700°F for a period of time to heat treat the coal mixture; further heating the mold and the coal mixture at a kiln temperature of about 900°F until a carbon foam structure is formed; and cooling the carbon foam structure under atmospheric conditions; wherein the carbon foam structure is substantially crack-free and has a compressive strength of about 1200 psi when normalized to about 40 pounds per cubic foot. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 A photographic rendering showing a typical attractive carbon foam board produced using only coal under high pressure in an autoclave.
[0012] Figure 2 and Figure 3 Rendering showing a photograph of a control sample made using only high volatile coal. Both were processed in a continuous kiln, with Figure 4 A “good” thermal curve is shown.
[0013] Figure 4 Graphs of two different thermal profiles used in the manufacture of carbon foam panels.
[0014] Figure 5 For use in continuous kilns Figure 4 A "good" thermal curve is shown, a rendering of a photograph of a substantially crack-free plate made using a high volatile coal containing 1 wt% polyethylene oxide, 1 wt% phenolic resin and 4 wt% graphite.
[0015] Figure 6 Rendering showing a picture of a carbon foam panel produced in a continuous kiln at atmospheric pressure after being processed into a shape of approximately 1.25 inches by 17 inches by 22 inches.
[0016] Figure 7 A rendering of a picture of a carbon foam sheet containing 4 wt % graphite is shown.
[0017] Figure 8 A rendering of a picture of a carbon foam sheet containing 4 wt% alumina is shown.
[0018] Fig. 9A comparison of the compressive strength as a function of density for carbon foams made in an autoclave and carbon foams produced at atmospheric pressure using medium or high volatility coals. DETAILED DESCRIPTION
[0019] This section describes some embodiments of the present invention in detail, which is sufficient to enable those skilled in the art to implement the present invention without excessive experimentation. However, it should be understood that the fact that a limited number of preferred embodiments are described does not in any way limit the scope of the present invention set forth in the claims.
[0020] It should be understood that whenever a numerical range is described herein, whether in this section or in any other section of this patent document, the range includes the endpoints and every point between the endpoints, just as if each such point had been clearly described. Unless otherwise stated, the words "about" and "substantially" used herein should be understood as normal measurement and / or manufacturing limitations associated with the value or condition modified by the word "about" or "substantially". Unless otherwise expressly stated, the term "embodiment" used herein means an embodiment of the present invention. The term "substantially crack-free" refers to a structure that has no internal cracks or internal defects that may cause cracks when stress is applied to the structure.
[0021] A method for manufacturing carbon foam structures in a single-piece flow through a continuous kiln under an inert atmosphere at atmospheric pressure is disclosed. The process significantly reduces manufacturing costs by reducing manufacturing time and increasing the ability to integrate automated equipment.
[0022] The carbonaceous raw coal used for these carbon foam structures may include bituminous, anthracite or even lignite, or mixtures of these coals, having a "free expansion index" of about 3.5 to about 9.0 as measured by ASTM D720, but is preferably bituminous coal, agglomerated coal that has been crushed to a suitable particle size, preferably a fine powder passing through about 60 mesh to 80 mesh. In addition, according to a further particularly preferred embodiment of the present invention, the coal-carbonaceous raw material of the present invention has all or at least some of the following characteristics: 1) the volatile matter content (dry basis, ash-free basis) defined in ASTM D3175 "Test Method for Volatile Matter in Coal and Coke Analysis" is about 35% to about 45%; 2) the fixed carbon (dry basis) defined in ASTM D3172 "Procedure for Proximate Analysis of Coal and Coke" is about 50% to about 60; 3) the Gisele initial softening temperature measured in accordance with ASTM D2639 "Test Method for Plastic Properties of Coal Using Constant Torque Gisele (Giesler) Plasticometer" is about 380°C to about 400°C; 4) the plastic temperature measured in accordance with ASTM D2639 is above about 50°C; 5) the plastic temperature measured in accordance with ASTM D2639 has a maximum flowability of at least 300 ddpm (divisions per minute), preferably greater than about 2000 ddpm; 6) an expansion ratio greater than about 20%, preferably greater than about 100%, as determined by Arnu expansion; 7) a vitrinite reflectance of about 0.80 to about 0.95 as determined by ASTM D2798, "Test Method for Microscopic Determination of Vitrinite Reflectance in Polished Coal Samples"; 8) less than about 30% of inert maceral materials such as hemibiotite, micas, fumarates, and minerals as determined by ASTM D2798; and 9) the coal is not significantly oxidized (0.0 volume % moderate or severe oxidation) as determined by ASTM D2798 and non-maceral analysis. A low softening point (380°C to 400°C) is important so that the material softens and becomes plastic before volatilization and coking occur. A large plastic working range or "plastic range" is important because it allows the coal to flow plastically while losing mass due to volatilization and coking. The vitrinite reflectance, fixed carbon content and volatile matter content are important in classifying these carbonaceous feedstocks as "high volatile" bituminous coals, which provide the best results in the process of the present invention.
[0023] The present invention may include introducing a particle pore stabilizer into the carbonaceous feedstock. A particle pore stabilizer is a material that increases the stability of the bubbles formed during the foaming process, preferably helping to promote the nucleation of bubbles throughout the foam volume, not just at the sides and bottom of the carbon foam sheet. In some embodiments, the particle pore stabilizer preferably provides a wetting angle or contact angle between the particles and the liquid phase of about 50 degrees to about 105 degrees. The wetting (contact) angle is measured at the foam-bubble interface to better quantify wettability.
[0024] In some embodiments, the particulate pore stabilizer may include, but is not limited to, carbon black; oxides such as alumina, silica, kyanite, boric acid, and titanium dioxide; ceramics such as silicon carbide, aluminosilicate clays, and fine metal powders. Preferably, the particulate pore stabilizer has no significant adverse effect on the final properties of the carbon foam. Alternatively, the particulate pore stabilizer may be selected to increase or adjust the properties of the carbon foam. In some embodiments, a particular pore stabilizer is capable of withstanding the heat treatment temperatures during the carbon foam manufacturing process without melting or otherwise decomposing. Further combinations or mixtures of different particulate pore stabilizers may be used.
[0025] The particle pore stabilizer may be added in an amount of about 0.1% to about 10% by weight. In some embodiments, the particle pore stabilizer may be added in an amount less than about 1% by weight. In some embodiments, the majority of the particle sizes in the particle pore stabilizer are preferably less than 10 μm. Preferably, the particle size is less than about 5 μm. In some embodiments, the particle size in the particle pore stabilizer may be about 3 μm to about 4 μm.
[0026] Additionally, several chemical or particulate additives are used to mitigate some of the processing issues when making carbon foam structures using continuous processing. These are used in conjunction with changes in the thermal profile to adjust the process and create acceptable carbon foam panels. Some chemical or particulate additives that have a positive impact include:
[0027] Polyethylene – This material may increase the liquid phase.
[0028] Polyethylene oxide - This material may help absorb the low viscosity fluid discharged from the coal and maintain a higher viscosity for the liquid phase that is formed.
[0029] Phenolic resin - This material may increase the liquid phase, but also tends to react to form solids and carbonize at high temperatures.
[0030] Microcrystalline cellulose – This material may help stabilize the bubbles in the foam and carbonize at high temperatures.
[0031] Graphite – This material may help stabilize the bubbles in the foam and reduce the thermal gradient of the foam by increasing its thermal conductivity.
[0032] When these types of chemical additives or particulate additives are applied to the same coal, and an acceptable thermal profile is applied, e.g. Figure 4 The "good" curve shown produces more attractive panels with larger sizes, more difficult rectangular shapes and a foam structure that is essentially crack-free. Figure 5 The plate shown is a substantially crack-free plate which was produced in a continuous kiln using Figure 4The "good" thermal curve shown was made using Bailey coal containing 1 wt% polyethylene oxide, 1 wt% phenolic resin and 4 wt% graphite. As shown, the board measures approximately 19 inches by 23 inches. Note that the discontinuity 12 on the surface is from a piece of paper used as a release agent. Figure 6 As shown, the board is easily machined to produce a substantially crack-free carbon foam board 14 having a smooth surface. The substantially crack-free carbon foam board 14 is produced in a continuous kiln at atmospheric pressure and machined into a shape of approximately 1.25 inches by 17 inches by 22 inches.
[0033] Applicants have noted that a slight change in the thermal profile makes it impossible to produce substantially crack-free panels. When a very similar profile is used, but the maximum temperature is only 878°F instead of 932°F, as Figure 4 As shown in the "bad" curve in Figure 1, the plate cracked during the heat treatment. Applicants have determined that temperature differences in the thermal curves can be the difference between a material with sufficient strength or insufficient strength to prevent failure due to thermal stresses. These data indicate that the carbon foam must be fired to a minimum temperature to ensure survival under the relatively rapid cooling in the continuous process.
[0034] like Figure 4 As shown in the "good" curve for the , an initial heating rate of 6°F per minute and time spent at 700°F are acceptable in producing substantially crack-free carbon foam structures. Applicants have determined that these parameters are critical to obtaining substantially crack-free quality carbon foam in a continuous kiln at atmospheric pressure. Initial trials used a heating rate of 8°F per minute, but failed to produce substantially crack-free foam board structures. Initial rates that were too fast or too slow, or insufficient time spent at temperatures near 700°F, will not produce substantially crack-free quality foam in a continuous process. Note that these target values will vary slightly depending on the type of coal and chemical or particulate additives used.
[0035] For a sufficiently long continuous kiln, the maximum temperature and degree of carbonization of the coal can be increased to the maximum required, assuming that the container (mould) used to hold the coal has sufficient refractoriness and redox properties.
[0036] Applicants have also found that adding graphite can be critical to producing large plates at an acceptable rate through the kiln. Figure 7 As shown, the board containing 4 wt% thermally conductive graphite powder produced a substantially crack-free board or structure. Figure 8As shown, a similar formulation using non-thermally conductive alumina powder instead of graphite produced cracked plates with numerous cracks 10. Applicants have determined that graphite helps reduce thermal gradients and resulting mechanical stress gradients in the plate, a phenomenon that is exacerbated by processing the material through a kiln more quickly. Therefore, Applicants have determined that adding graphite can increase the speed at which plates can be processed through a continuous kiln.
[0037] A method of making carbon foam in a continuous process at atmospheric pressure is disclosed wherein the maximum temperature at which the parts are processed is sufficiently high to provide the material with adequate strength and to avoid cracking during cooling. Applicants have determined this temperature to be about 900°F. The rate of heating of the coal mixture is about 6°F per minute. After the coal mixture is preheated, it may be placed in a kiln at a temperature of about 700°F for a period of time before the temperature is raised. A graphite additive is used to increase the rate at which the carbon foam is processed through the continuous kiln. Fig. 9 As shown, the substantially crack-free carbon foam structural product produced by this method has a compressive strength of about 1200 psi when normalized to a density of about 40 pounds per cubic foot.
[0038] The foregoing explanations, illustrations, diagrams, examples and discussions are intended to help readers understand the present invention and further demonstrate its usefulness and novelty, but are not intended to limit the scope of the present invention. The following claims, including all equivalents, are intended to define the scope of the present invention.
Claims
1. A continuous method for producing a substantially crack-free carbon foam structure comprising the steps of: crushing the carbonaceous raw material into powder; mixing the powder and at least one of a chemical additive or a particulate additive to form a coal mixture; placing the coal mixture into a carbon foam structural mold configured for continuous processing in a kiln at atmospheric pressure and under an inert gas; heating the mold and coal mixture at a kiln temperature of about 700°F under an inert gas at a rate of about 6°F per minute; maintaining the kiln temperature at about 700°F for a period of time to thermally treat the coal mixture; further heating the mold and coal mixture at a kiln temperature of about 900°F until a carbon foam structure is formed; and cooling the carbon foam structure under atmospheric conditions; The carbon foam structure is substantially free of cracks.
2. The method according to claim 1, wherein the carbonaceous raw material comprises bituminous coal, sub-bituminous coal, anthracite and lignite, and combinations thereof.
3. The method of claim 1, wherein the step of mixing further comprises adding a particle pore stabilizer to the carbonaceous feedstock.
4. The method of claim 3, wherein the particle pore stabilizer comprises carbon black, fine oxides of alumina, silica, boric acid, titanium dioxide, aluminosilicate clay, kyanite, fine powders of non-oxides of silicon carbide, metal powders, and mixtures thereof.
5. The method of claim 1, wherein the chemical additive or the particulate additive comprises at least one of the following substances: polyethylene, polyethylene oxide, phenolic resin, microcrystalline cellulose, graphite, and mixtures thereof.
6. The method of claim 1, wherein the period of time is from about 0.5 hours to about 12 hours.
7. A substantially crack-free carbon foam structure produced by a continuous process comprising the steps of: crushing the carbonaceous raw material into powder; mixing the powder with at least one of a chemical additive or a particulate additive to form a coal mixture; placing the coal mixture into a carbon foam structural mold configured for continuous processing in a kiln at atmospheric pressure and under an inert atmosphere; heating the mold and coal mixture at a kiln temperature of about 700°F under an inert gas at a rate of about 6°F per minute; maintaining the kiln temperature at about 700°F for a period of time to thermally treat the coal mixture; The mold and coal mixture are further heated at a kiln temperature of about 900°F until a carbon foam structure is formed; and cooling the carbon foam structure under atmospheric conditions; The carbon foam structure is substantially crack-free and has a compressive strength of about 1200 psi when normalized to about 40 pounds per cubic foot.
8. The substantially crack-free carbon foam structure of claim 7, wherein the carbonaceous feedstock comprises bituminous coal, sub-bituminous coal, anthracite, and lignite, and combinations thereof.
9. The substantially crack-free carbon foam structure of claim 7, wherein said step of mixing further comprises adding a particulate cell stabilizer to said carbonaceous feedstock.
10. The substantially crack-free carbon foam structure of claim 9, wherein the particulate cell stabilizer comprises carbon black, fine oxides of alumina, silica, boric acid, titanium dioxide, aluminosilicate clays, kyanite, fine non-oxide powders of silicon carbide, metal powders, and mixtures thereof.
11. The substantially crack-free carbon foam structure of claim 7, wherein the chemical additive or particulate additive comprises at least one of the following: polyethylene, polyethylene oxide, phenolic resin, microcrystalline cellulose, graphite, and mixtures thereof.
12. The substantially crack-free carbon foam structure of claim 7, wherein the period of time is from about 0.5 hours to about 12 hours.
Citation Information
Patent Citations
High density carbon foam
CN101189320A
Preparation method of coal-based carbon foam
CN102530916A
Processes and compositions for carbon foams and materials
US20190308881A1
Processes and compositions for carbon foam materials
US20210122640A1
Methods of making a carbon foam
US6544491B1