Surface-treated galvanized steel sheet

By forming a film of specific components on the galvanized steel plate, the problem of delayed fracture of the steel plate under low temperature environment is solved, and the manufacturing cost is reduced, thereby achieving high strength and corrosion resistance of the steel plate.

CN118891390APending Publication Date: 2024-11-01JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093657.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2022-10-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is prone to delayed fracture when increasing the strength of steel, especially in low temperature environments, and the effects are unclear, and commonly used protective measures are costly, such as the use of expensive materials such as bismuth.

Method used

The galvanized steel plate is formed with 10% to 50% of aliphatic dicarboxylic acid and alkyl amine salts, aromatic monocarboxylic acid and alkyl amine salts as the main components. These additives inhibit hydrogen invasion and thereby improve the steel plate. Retardant fracture resistance.

Benefits of technology

The excellent delay-retardant fracture resistance of steel plates in low temperature environments is achieved, and the manufacturing cost is reduced, avoiding the need for using expensive materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891390A_ABST
    Figure CN118891390A_ABST
Patent Text Reader

Abstract

Provided is a surface-treated galvanized steel sheet which has excellent delayed fracture resistance characteristics regardless of the composition of a base steel sheet even in a low-temperature environment, and which can be produced at low cost. The surface-treated galvanized steel sheet comprises a steel sheet having a tensile strength of 1180 MPa or more, a zinc plating layer formed on at least one surface of the steel sheet, and a coating film formed on the zinc plating layer, wherein the coating film contains 10-50 mass% of an additive in terms of solid content. The additive is at least one type selected from the group consisting of salts of an aliphatic dicarboxylic acid having 2-8 carbon atoms and an alkylamine having 6-18 carbon atoms, salts of an aliphatic dicarboxylic acid having 2-8 carbon atoms and a cycloalkylamine having 6-18 carbon atoms, and salts of an aromatic monocarboxylic acid having 7-12 carbon atoms and an alkylamine having 6-18 carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to surface treated galvanized steel sheets. Background Art

[0002] In recent years, in the automotive field, from the perspective of environmental protection, it is required to reduce CO2 emissions by lightweighting the vehicle body. In addition, from the perspective of protecting occupants, it is also required to improve collision safety and seek high strength of automotive steel plates. However, it is known that when the strength of steel is increased, a phenomenon called delayed fracture is likely to occur. Delayed fracture refers to the following phenomenon: when high-strength steel is subjected to static load stress (load stress less than tensile strength), brittle fracture suddenly occurs without plastic deformation after a certain period of time.

[0003] It is known that delayed fracture is caused by hydrogen intruding into steel from the environment (hydrogen embrittlement), and the hydrogen intrusion path includes pickling process, wet plating process, and corrosion in the atmospheric environment during the manufacturing and processing of steel sheets. Non-patent document 1 reports that delayed fracture occurs in high-strength steel sheets with a tensile strength of 1180 MPa or more.

[0004] In order to prevent delayed fracture in high-strength steel sheets, surface treatment of steel sheets has been studied. As a surface treatment technology to prevent hydrogen from invading galvanized steel sheets in an atmospheric corrosion environment, for example, the following technology is known: a chemical conversion treatment layer containing bismuth is formed on the surface of a galvanized high-strength steel sheet, thereby suppressing the generation of hydrogen on the surface of the steel sheet (Patent Document 1). In addition, a technology for suppressing hydrogen intrusion by forming a zinc-nickel plating layer with Ni added to the plating on the surface of a high-strength steel sheet has been proposed (Patent Document 2).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-209585

[0008] Patent Document 2: Japanese Patent Application Publication No. 2019-26893

[0009] Non-patent literature

[0010] Non-patent document 1: Tian Lu et al., "Evaluation method of hydrogen embrittlement resistance of high-strength thin steel plate", Iron and Steel, Vol. 95, No. 12 (2009) 887 Summary of the invention

[0011] However, bismuth is very expensive, so the manufacturing cost becomes high. In addition, the technology of the above patent document can be seen to be effective at temperatures above room temperature, but the effect in low temperature environments such as cold regions is not yet clear.

[0012] The purpose of the present disclosure is to solve the problems of the prior art as described above and to provide a surface-treated galvanized steel sheet that has excellent delayed fracture resistance regardless of the composition of the base steel sheet even in a low-temperature environment and can be manufactured at low cost.

[0013] In order to solve the above problems, the inventors of the present invention have repeatedly conducted in-depth studies and research on the suppression of hydrogen intrusion by surface treatment of steel sheets. As a result, it was found that the delayed fracture of the steel sheet can be effectively suppressed by forming a film containing 10% to 50% by mass of at least one additive component selected from the group consisting of salts of aliphatic dicarboxylic acids and alkylamines, salts of aliphatic dicarboxylic acids and cycloalkylamines, and salts of aromatic monocarboxylic acids and alkylamines in terms of solid content on a galvanized steel sheet.

[0014] The present disclosure is completed based on the above findings. That is, the gist of the present disclosure is as follows.

[0015] [1] A surface-treated galvanized steel sheet having:

[0016] Steel plates with a tensile strength of 1180 MPa or more,

[0017] A galvanized layer formed on at least one surface of the steel sheet, and

[0018] The film formed on the zinc plating layer,

[0019] The film contains 10% to 50% by mass of additives in terms of solid content.

[0020] Here, the additive is at least one selected from the group consisting of salts of aliphatic dicarboxylic acids having 2 to 8 carbon atoms and alkylamines having 6 to 18 carbon atoms, salts of aliphatic dicarboxylic acids having 2 to 8 carbon atoms and cycloalkylamines having 6 to 18 carbon atoms, and salts of aromatic monocarboxylic acids having 7 to 12 carbon atoms and alkylamines having 6 to 18 carbon atoms.

[0021] [2] The surface-treated galvanized steel sheet according to [1], wherein the aliphatic dicarboxylic acid having 2 to 8 carbon atoms is at least one selected from oxalic acid, maleic acid, fumaric acid, malonic acid, succinic acid, glutaric acid and adipic acid,

[0022] The aromatic monocarboxylic acid having 7 to 12 carbon atoms is at least one selected from benzoic acid, m-aminobenzoic acid, p-aminobenzoic acid, p-nitrobenzoic acid, salicylic acid, p-hydroxybenzoic acid, toluic acid, p-tert-butylbenzoic acid and β-hydroxynaphthoic acid,

[0023] The alkylamine having 6 to 18 carbon atoms is at least one selected from the group consisting of octadecylamine, dodecylamine, decylamine, monooctylamine, monohexylamine, monodecylamine, monododecylamine and mono-2-ethylhexylamine.

[0024] The cycloalkylamines having 6 to 18 carbon atoms are cyclohexylamine, dicyclohexylamine and tricyclohexylamine.

[0025] [3] The surface-treated galvanized steel sheet according to [1] or [2], wherein the hydrogen permeation current density iH measured by adding 1 g / L of the additive to a solution simulating a corrosive environment is t The hydrogen permeation current density iH0 measured without adding the above additive to the above solution satisfies the following formula (1).

[0026] i t / iH0≤0.50···(1)

[0027] Here, the hydrogen permeation current density iH is measured as follows: a zinc plate and a test steel plate are brought into electrical contact, one surface of the zinc plate and the test steel plate is exposed to the solution and the one surface is used as a hydrogen intrusion surface,

[0028] The other surface of the test steel plate was used as a hydrogen detection surface having a palladium-plated film.

[0029] The measurement was performed using an electrochemical cell provided on the above-mentioned hydrogen detection surface.

[0030] [4] The surface-treated galvanized steel sheet according to any one of [1] to [3] above, wherein a base film is provided between the galvanized layer and the film.

[0031] [5] A surface-treated galvanized steel sheet according to any one of [1] to [4] above, wherein the coating comprises one or more selected from epoxy resin, acrylic resin, polyurethane resin, vinyl resin, phenolic resin, polyester resin, fluororesin, polyolefin resin and epoxy ester resin.

[0032] According to the present disclosure, it is possible to provide a surface-treated galvanized steel sheet which has excellent delayed fracture resistance regardless of the composition of the base steel sheet even in a low-temperature environment and can be manufactured at low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1A This is a diagram for explaining a method for measuring hydrogen permeation current density.

[0034] Figure 1B This is a diagram for explaining a method for measuring hydrogen permeation current density.

[0035] Figure 2 It is a schematic diagram showing a device for measuring the amount of intruding hydrogen.

[0036] Figure 3 This is a diagram showing an example of the measurement results of the hydrogen permeation current density.

[0037] Figure 4 This is a diagram for explaining a test piece for evaluating delayed fracture resistance.

[0038] Figure 5 This is a diagram for explaining a dry-wet repeated test for evaluating delayed fracture resistance. DETAILED DESCRIPTION

[0039] The following is an explanation of the embodiment of the surface treated galvanized steel sheet disclosed in the present invention. It should be noted that the present invention is not limited to the following embodiments. It should be noted that in this specification, the numerical range represented by "~" refers to a range that includes the numerical values ​​recorded before and after "~" as the lower limit and upper limit.

[0040] First, the surface-treated galvanized steel sheet disclosed in the present invention is briefly described. The surface-treated galvanized steel sheet disclosed in the present invention comprises a steel sheet having a tensile strength of 1180 MPa or more, a galvanized layer formed on at least one side of the steel sheet, and a coating formed on the galvanized layer. The surface-treated galvanized steel sheet is described in detail below.

[0041] The steel plate that becomes the base steel plate of the surface-treated galvanized steel plate is described. The steel plate is a high-strength steel plate with a tensile strength of 1180 MPa or more. The tensile strength of the steel plate is preferably 1470 MPa or more. In a steel plate with low tensile strength, delayed fracture is not easy to occur. The effect of having excellent delayed fracture resistance even in a low temperature environment is also shown in a steel plate with low tensile strength, but is significantly shown in a steel plate with a tensile strength of 1180 MPa or more, and is more significantly shown in a steel plate with a tensile strength of 1470 MPa or more.

[0042] The tensile strength of the steel plate is measured as follows. A JIS No. 5 tensile test piece is taken from the steel plate in a manner such that the rolling right angle direction is the long side direction (tensile direction), and the tensile strength (TS) is measured by a tensile test according to JIS Z2241 (1998). It should be noted that when evaluating the tensile strength of a steel plate (base steel plate) of a surface-treated galvanized steel plate, as described later, the galvanized layer and the film can be removed from the surface-treated galvanized steel plate to separate a single steel plate and the tensile strength of the steel plate can be evaluated for the steel plate, or the tensile strength of the surface-treated galvanized steel plate can be regarded as the tensile strength of the steel plate.

[0043] The steel sheet has no particular limitation on the composition of the steel sheet as long as it has the above-mentioned tensile strength. For example, the steel sheet may have the following composition: containing C: 0.1 mass% to 0.4 mass%, Si: 0 mass% to 2.5 mass%, Mn: 1 mass% to 3.5 mass%, P: 0 mass% to 0.05 mass%, S: 0 mass% to 0.005 mass%, and the remainder is composed of Fe and inevitable impurities. Preferably, the steel sheet has the following composition: containing C: 0.1 mass% to 0.4 mass%, Si: 0.01 mass% to 2.5 mass%, Mn: 1 mass% to 3.5 mass%, P: 0.0001 mass% to 0.05 mass%, S: 0.0001 mass% to 0.005 mass%, and the remainder is composed of Fe and inevitable impurities. The component composition of the steel plate may further contain one or more selected from Cu: 1.0 mass% or less, Ti: 0.2 mass% or less, V: 0.5 mass% or less, sol.Al: 0.1 mass% or less, Cr: 1.0 mass% or less, Nb: 0.2 mass% or less, W: 0.5 mass% or less, Zr: 0.1 mass% or less, B: 0.005 mass% or less, N: 0.0005 mass% to 0.0100 mass%, Ni: 0.01 mass% to 2.00 mass%, Mo: 0.005 mass% to 2.000 mass%, Ca: 0.002 mass% to 0.0050 mass%, REM: 00002 mass% to 0.0050 mass%, Sb: 0.002 mass% to 0.200 mass%, and Sn: 0.002 mass% to 0.200 mass% as arbitrary elements. These arbitrary elements are preferably added in an amount limited to about 4 mass % in total. In addition, as the lower limit of any element, preferably sol.Al, Cr: 0.01 mass %, Cu, Ti, V, Nb, W, Zr: 0.005 mass %, B: about 0.0001 mass %. In order to improve various properties such as mechanical properties, the steel plate can be, for example, a composition that can be solid solution strengthened by adding intrusive solid solution elements such as C and N and substitutional solid solution elements such as Si, Mn, P, and Cr. The steel plate can also be a composition that can be precipitation strengthened by carbonitrides such as Ti, Nb, V, and Al. The composition of the steel plate can include strengthening elements such as W, Zr, B, Cu, and rare earth elements.

[0044] The steel structure of the steel plate is not particularly limited. Various organizational or structural modifications can be made to the steel plate alone or in combination. For example, toughening can be performed by recovery annealing at a temperature where recrystallization does not occur, partial recrystallization strengthening can be performed by not completely recrystallizing and leaving unrecrystallized areas, strengthening can be performed by using phase transformation structures such as bainite, martensite single phase transformation or ferrite and these phase transformation structures composite organization, and the Hall-Petch formula when the ferrite grain size is set to d: σ=σ0+kd -1 / 2The microstructure or structural modification such as grain refinement strengthening represented by (wherein σ is stress, σ0 is internal stress, and k is material constant) and work strengthening by rolling etc. is performed alone or in combination of multiple types.

[0045] Examples of commercially available steel plates include JFE-CA1180, JFE-CA1320, JFE-CA1470, JFE-CA1180SF, JFE-CA1180Y1, JFE-CA1180Y2 (all manufactured by JFE-CA1180Y), SAFC1180D (manufactured by Nippon Steel Corporation), etc. In addition, both cold-rolled steel plates and hot-rolled steel plates can be used as high-strength steel plates.

[0046] In addition, the thickness of the steel plate is not particularly limited. In one example, the thickness of the steel plate may be 0.8 mm or more and 5 mm or less. The thickness of the steel plate is more preferably 1.2 mm or more and 2.0 mm or less.

[0047] The surface treated galvanized steel sheet disclosed in the present invention has a galvanized layer on at least one side of the steel sheet. The galvanized layer can be formed by any plating method such as hot dip plating, electroplating, electroless plating, vapor deposition coating, etc., but is generally a hot dip galvanized layer and an electroplated galvanized layer in industry. In addition, the hot dip galvanized steel sheet includes an alloyed hot dip galvanized steel sheet obtained by alloying after hot dip galvanizing.

[0048] The surface treated galvanized steel sheet disclosed in the present invention has a film containing the additives described below on the zinc coating layer of the galvanized steel sheet as described above. As a result, the intrusion of hydrogen in a corrosive environment is suppressed, and excellent delayed fracture resistance is obtained. Here, the additive contained in the film is at least one selected from the salt of an aliphatic dicarboxylic acid having 2 to 8 carbon atoms and an alkylamine having 6 to 18 carbon atoms, the salt of an aliphatic dicarboxylic acid having 2 to 8 carbon atoms and a cycloalkylamine having 6 to 18 carbon atoms, and the salt of an aromatic monocarboxylic acid having 7 to 12 carbon atoms and an alkylamine having 6 to 18 carbon atoms.

[0049] Galvanized steel sheets are widely used for parts that require corrosion resistance in atmospheric environments. This is because zinc has an excellent sacrificial anti-corrosion effect. However, as a counter-reaction to the sacrificial anti-corrosion reaction, a hydrogen generation reaction occurs on the steel base of the galvanized steel sheet. The hydrogen intrusion into the galvanized steel sheet is mainly due to the hydrogen generation reaction. Therefore, the inventors of the present invention thought of suppressing the hydrogen intrusion by suppressing the increase of the exposed portion of the steel base as the hydrogen generation site, thereby completing the present disclosure. In the present disclosure, the additives added to the film are classified as adsorption film-type rust-proof additives that exhibit rust resistance by adsorption on the metal surface. It is known that adsorption film-type rust-proof additives exhibit rust resistance by protecting the surface of the steel sheet from the influence of the corrosive environment, but the inventors of the present invention have newly discovered through independent research that the effect of significantly improving the delayed fracture resistance by preventing the intrusion of hydrogen generated by the sacrificial anti-corrosion reaction. It is believed that the additive having an amide group dissolves from the film and adsorbs on the metal surface, thereby covering the exposed portion of the steel base as the hydrogen generation site, suppressing hydrogen generation, and thus suppressing hydrogen intrusion.

[0050] The alkylamine or cycloalkylamine contained in the additive is preferably a primary amine or a secondary amine because it easily forms a salt with a carboxylate. As the alkylamine having 6 to 18 carbon atoms, at least one selected from octadecylamine, dodecylamine, decylamine, monooctylamine, monohexylamine, monodecylamine, monododecylamine and mono-2-ethylhexylamine is preferred. As the cycloalkylamine having 6 to 18 carbon atoms, cyclohexylamine, dicyclohexylamine and tricyclohexylamine are preferred. The above alkylamines or cycloalkylamines may be used in combination of multiple types.

[0051] The aliphatic dicarboxylic acid having 2 to 8 carbon atoms or the aromatic monocarboxylic acid having 7 to 12 carbon atoms contained in the additive affects the ease of forming a salt with an alkylamine or a cycloalkylamine. When an aliphatic dicarboxylic acid having 2 to 8 carbon atoms or an aromatic monocarboxylic acid having 7 to 12 carbon atoms is used as the carboxylic acid, the salt formation between the carboxylic acid and the amine becomes easy, and the solubility of the amine is improved.

[0052] As the aliphatic carboxylic acid, an aliphatic dicarboxylic acid having 2 to 8 carbon atoms is used. In this case, as an additive, a diamine salt obtained from 1 mol of an aliphatic dicarboxylic acid and 2 mol of an amine, or a monoamine salt obtained from 1 mol of an aliphatic dicarboxylic acid and 1 mol of an amine is used. If the aliphatic dicarboxylic acid has 2 to 8 carbon atoms, the acid strength becomes high, the formation of an amine salt becomes easy, and the amine is easily freed in the film, and the solubility of the amine is improved. On the other hand, when the aliphatic dicarboxylic acid has 9 or more carbon atoms, it is difficult to form an amine salt (especially a diamine salt), and the pH of the salt of the component is easily reduced.

[0053] The carbon number of 2 to 8 of the aliphatic dicarboxylic acid includes the carbon number of the aliphatic group and the carbon number of the carboxylic acid. Therefore, the carbon number excluding the dicarboxylic acid is 0 to 6. The carbon number of the aliphatic dicarboxylic acid is preferably 6 or less. As the aliphatic group constituting the aliphatic dicarboxylic acid, an alkylene group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms is preferred. As the alkylene group, an alkylene group having 1 to 4 carbon atoms is more preferred. In addition, as the alkenyl group, an alkenyl group having 2 to 4 carbon atoms is more preferred. The aliphatic dicarboxylic acid having 2 to 8 carbon atoms may be oxalic acid in which the carbon of the carboxyl group is connected by a single bond. As the aliphatic dicarboxylic acid having 2 to 8 carbon atoms, at least one selected from oxalic acid, maleic acid, fumaric acid, malonic acid, succinic acid, glutaric acid and adipic acid is preferred.

[0054] As the aromatic carboxylic acid, an aromatic monocarboxylic acid having 7 to 12 carbon atoms is used. When the aromatic carboxylic acid having 7 to 12 carbon atoms is used as a salt with an amine, the amine salt is easily formed, and the amine is easily released in the film, thereby improving the solubility of the amine.

[0055] The number of carbon atoms of the aromatic monocarboxylic acid of 7 to 12 includes the number of carbon atoms constituting the aromatic group and the number of carbon atoms constituting the carboxylic acid. Therefore, the number of carbon atoms excluding the monocarboxylic acid is 6 to 11. As the aromatic ring contained in the aromatic monocarboxylic acid, a benzene ring or a naphthalene ring is preferred because of the ease of production. Substituents such as methyl, hydroxyl, amino, and nitro may be bonded to the aromatic ring. As the aromatic monocarboxylic acid having 7 to 12 carbon atoms, at least one selected from benzoic acid, m-aminobenzoic acid, p-aminobenzoic acid, p-nitrobenzoic acid, salicylic acid, p-hydroxybenzoic acid, toluic acid, p-tert-butylbenzoic acid, and β-hydroxynaphthoic acid is preferred.

[0056] The additive is preferably added to a solution simulating a corrosive environment at 1 g / L and the hydrogen permeation current density iH is measured. t The hydrogen permeation current density iH0 measured without adding an additive to the above solution satisfies the following formula (1).

[0057] i t / iH0≤0.50···(1)

[0058] Here, the hydrogen permeation current density iH is measured as follows: the zinc plate and the test steel plate are made conductive, one surface of the zinc plate and the test steel plate is exposed to the above-mentioned solution and the one surface is used as the hydrogen intrusion surface, and the other surface of the test steel plate is used as the hydrogen detection surface having a palladium-plated film, and the measurement is performed using an electrochemical cell arranged on the hydrogen detection surface.

[0059] The surface-treated galvanized steel sheet disclosed in the present invention has a film containing the above-mentioned additive, which inhibits the intrusion of hydrogen in a corrosive environment and has excellent delayed fracture resistance. However, by using an additive that satisfies the above-mentioned formula (1), the delayed fracture resistance can be further improved.

[0060] The combination of carboxylic acid and amine for obtaining an additive satisfying the above formula (1) is not necessarily clear. However, it is believed that the adsorption capacity of the obtained additive on the surface of the steel sheet itself varies depending on the carbon number, molecular weight, presence or absence of side chains of the carboxylic acid and amine as raw materials for obtaining the additive. In addition, it is believed that the shielding effect of the exposed part of the steel base is different due to the difference in the fluffiness of the obtained additive, resulting in a difference in the hydrogen intrusion suppression effect.

[0061] use Figure 1A and Figure 1B , the outline of the method for measuring the hydrogen permeation current density is described. Figure 1A As shown in the figure, in the sacrificial anti-corrosion reaction, the zinc coating is corroded first rather than the steel plate surface. At this time, the electrons generated by the corrosion of the zinc coating react with water to generate hydrogen, which intrudes into the steel. It is believed that the additive in the film is dissolved from the film and covers the exposed steel plate surface to prevent hydrogen intrusion. In order to quantitatively evaluate the effect of the additive, as shown in the figure, Figure 1B As shown, a model experiment was established to verify the effect of the additives contained in the film on the sacrificial corrosion protection reaction (galvanic corrosion) of the zinc coating when the steel base is exposed, and the hydrogen permeation current density was measured. Figure 1B As shown, the test steel plate 10 is clamped by two reaction tanks (hydrogen generation tank 20, hydrogen detection tank 21), and the zinc plate 40 and one surface 11 (hydrogen intrusion surface) of the test steel plate 10 are exposed to the solution of the simulated corrosion environment in the hydrogen generation tank 20 while the test steel plate 10 and the zinc plate 40 are connected. It should be noted that the composition of the zinc plate 40 is composed of zinc and inevitable impurities. In this way, the sacrificial anti-corrosion reaction of the zinc plate 40 occurs in the hydrogen generation tank 20, and the electron flow conducts to the test steel plate 10, and the hydrogen generation reaction occurs on one surface 11 of the test steel plate 10. As a result, hydrogen invades the steel from one surface 11 of the test steel plate 10, and the hydrogen diffuses and moves in the steel to the other surface 12 of the test steel plate 10. When a potential that can oxidize hydrogen into hydrogen ions is applied to the other surface 12 (hydrogen detection surface) of the test steel plate 10 facing the hydrogen detection tank 21, the hydrogen that diffuses and moves and reaches the hydrogen detection surface 12 is oxidized into hydrogen ions. At this time, the hydrogen intrusion behavior can be quantified by measuring the oxidation current (hydrogen permeation current) of the hydrogen detection surface 12. At this time, by adding additives to the solution in the hydrogen generation tank 20 where the sacrificial anti-corrosion reaction occurs, the influence of the additives on the hydrogen intrusion behavior into the test steel plate 10 can be investigated.

[0062] Figure 2Schematic diagram of an intrusion hydrogen amount measuring device 100 used in the measurement of hydrogen permeation current density. One surface 11 of a test steel plate 10 is exposed to a solution simulating a corrosion environment in a hydrogen generating tank 20 and serves as a hydrogen intrusion surface 11, and the other surface of the test steel plate 10 serves as a hydrogen detection surface 12. The hydrogen detection surface 12 is provided with a palladium-plated film 50 in a manner that minimizes reactions other than hydrogen oxidation reactions. In addition, an electrochemical cell for measuring the anode current is provided on the hydrogen detection surface 12. As the electrochemical cell, any electrochemical cell can be used as long as the anode current of the hydrogen detection surface 12 can be measured. Figure 1A and Figure 1B In the example shown, the electrochemical cell is a hydrogen detection cell 21 and includes an electrolyte, a storage body for storing the electrolyte, a reference electrode 23 and a counter electrode 24 provided inside the storage body.

[0063] In order to reduce the influence of detailed test conditions when measuring the hydrogen permeation current density, in the present disclosure, the hydrogen permeation current density iH is measured by adding 1 g / L of an additive to the solution in the hydrogen generation tank 20, rather than using a specific value of the hydrogen permeation current density iH. t The ratio iH to the hydrogen permeation current density iH0 measured without adding additives to the solution in the hydrogen generation tank 20 is t / iH0, the effect of the additive on the hydrogen intrusion behavior of the steel sheet is evaluated. Specifically, the additive contained in the film is preferably iH t / iH0 is an additive satisfying the following formula (1).

[0064] i t / iH0≤0.50···(1)

[0065] That is, if the hydrogen permeation current density iH0 measured without adding the additive to the solution is equal to the hydrogen permeation current density iH0 measured when the additive is added under the same conditions, t If the value is less than half, the additive can be evaluated as being able to appropriately reduce hydrogen intrusion into the steel. t / iH0 is more preferably 0.40 or less, and still more preferably 0.30 or less. t / iH0 is preferably low, and the lower limit is not particularly limited, but in one example it may be 0.01 or more.

[0066] The following describes the experimental conditions for the method of measuring the hydrogen permeation current density in more detail. The hydrogen generating tank 20 is assembled in such a manner that the zinc plate 40 and the test steel plate 10 are opposite to each other with the hydrogen generating tank 20 interposed therebetween. The temperature of the hydrogen generating tank 20 and the hydrogen detecting tank 21 is adjusted to 10°C using a temperature adjustment device such as a water bath. The thickness of the test steel plate 10 is 0.5 mm. In order to minimize the occurrence of reactions other than the oxidation reaction of hydrogen, palladium plating of about 100 nm is applied to the hydrogen detecting surface 12 of the test steel plate 10 in contact with the hydrogen detecting tank 21. A 0.1M NaOH aqueous solution degassed with nitrogen is filled in the hydrogen detecting tank 21 as an electrolyte. The potentiostat 30 is connected to the test steel plate 10 and the reference electrode 23 and the counter electrode 24 installed in the hydrogen detecting tank 21, and anodic polarization is started at a constant potential of 0 to 0.2 V vs SHE. The anode current decays to 0.1 μA / cm 2 After that, the hydrogen generation tank 20 is filled with a 5wt.% NaCl aqueous solution as a corrosion solution. The additive is contained in the NaCl aqueous solution in a concentration of 1g / L. The zinc plate 40 and the test steel plate 10 are connected by copper wire or the like to conduct, and the sacrificial anti-corrosion reaction is started. After the sacrificial anti-corrosion reaction starts, when the current is sufficiently stable, that is, after 48h from the start of the sacrificial anti-corrosion reaction, the hydrogen permeation current density iH is evaluated. t 、iH0。

[0067] Figure 3 This figure shows an example of the measurement result of hydrogen permeation current density. Figure 3 In the example of FIG. 1 , a diamine salt of fumaric acid and monooctylamine is used as an additive. Under the same conditions, the hydrogen permeation current density iH0 when the solution in the hydrogen generation tank 20 does not contain the additive and the hydrogen permeation current density iH0 when the solution in the hydrogen generation tank 20 contains the additive are measured. t Repeat twice each and find the average value. Figure 3 In the figure, the first measurement result is represented as N1, and the second measurement result is represented as N2. The hydrogen permeation current density iH0 when the solution in the hydrogen generation tank 20 does not contain an additive is 0.35 μA / cm 2 , when the solution in the hydrogen generating tank 20 contains an additive, iH t 0.07μA / cm 2 .

[0068] Table 1 shows the iH of various additives t / iH0. Examples of the additive satisfying the formula (1) include X1 to 60, 62 to 68, 70 to 76, 78 to 84, 86 to 92, 94 to 100, 102 to 108, 110 to 116, 118 to 124, and 126 to 149 in Table 1.

[0069] The film contains 10% to 50% by mass of the above-mentioned additives in terms of solid content. In order to make the film fully exhibit delayed fracture resistance under a corrosive environment, the content of the additives in the film (the ratio relative to the mass of the film) is set to 10% by mass or more. It is believed that as the content of the additives in the film increases, the area where the components alkylamine and cycloalkylamine with amide groups are adsorbed on the surface of the steel plate also increases, and the delayed fracture resistance performance is improved. On the other hand, if the content exceeds 50% by mass, there is a risk of reducing the strength of the film itself, so the content of the additives is 50% by mass or less. The film preferably contains 15% or more of the additives in terms of solid content, and more preferably contains 20% or more. In addition, the film preferably contains 40% or less of the additives in terms of solid content, and more preferably contains 30% or less. It should be noted that when the film is composed of multiple layers, the total content of the additives contained in the multiple layers is set to 10% to 50% by mass in terms of solid content.

[0070] Next, the components other than the above-mentioned additives contained in the film are described. The film may contain an organic resin. As the organic resin, it is preferred to use one or more selected from epoxy resins, acrylic resins, polyurethane resins, vinyl resins, phenolic resins, polyester resins, fluororesins, polyolefin resins and epoxy ester resins. This is because these organic resins serve as a barrier layer to protect the steel plate from corrosion factors, inhibit corrosion associated with hydrogen generation reactions, and have the function of preventing the galvanized layer from peeling off during processing. The above-mentioned organic resins may also be used in combination of two or more. It is also possible to use two or more resins from the above-mentioned organic resins to form a film consisting of multiple layers.

[0071] From the viewpoint of improving corrosion resistance, the film is preferably a film composed of two or more layers. In one example, the film is composed of two layers of a lower film provided on a galvanized steel sheet and an upper film provided on the lower film. Both the upper film and the lower film may contain additives, or only one of them may contain additives. From the viewpoint of taking into account both corrosion resistance and weldability, the lower film is preferably a film that does not reduce corrosion resistance and has excellent conductivity.

[0072] Specifically, the lower layer film is preferably obtained by applying a surface treatment liquid (A) to the surface of a galvanized steel sheet and drying it, wherein the surface treatment liquid (A) contains a water-soluble zirconium compound (a), a tetraalkoxysilane (b), a compound having an epoxy group (c), a chelating agent (d), a vanadic acid compound (e), and a metal compound (f) containing at least one selected from Ti, Al and Zn within the range satisfying the following conditions (I) to (IV), and the pH is set to 8 to 10.

[0073] (I) The mass ratio of the water-soluble zirconium compound (a) in terms of Zr (azr) to the tetraalkoxysilane (b) (azr / b): 1.0 to 6.0

[0074] When the mass ratio azr / b is 1.0 or more, a surface-treated galvanized steel sheet having more excellent corrosion resistance can be obtained. When the mass ratio azr / b is 6.0 or less, the conductivity of the surface-treated galvanized steel sheet is more suitable.

[0075] (II) Mass ratio of the solid content (cs) of the tetraalkoxysilane (b) to the compound (c) having an epoxy group: 0.1 to 1.6

[0076] When the mass ratio b / cs is 0.1 or more, a surface-treated galvanized steel sheet with better corrosion resistance can be obtained. When the mass ratio b / cs is 1.6 or less, the adhesion of the film is better.

[0077] (III) Mass ratio of the solid content (ds) of the tetraalkoxysilane (b) to the chelating agent (d) (b / ds): 0.3 to 2.0

[0078] When the mass ratio b / ds is 0.3 to 2.0, a surface-treated galvanized steel sheet having more excellent corrosion resistance can be obtained.

[0079] (IV) Mass ratio (ev / ds) of the V-converted mass (ev) of the vanadate compound (e) to the solid content (ds) of the chelating agent (d): 0.03 to 1.0

[0080] If the mass ratio ev / ds is 0.03 or more, a surface-treated galvanized steel sheet with better corrosion resistance can be obtained. In addition, if the mass ratio ev / ds is 1.0 or less, the vanadic acid compound (e) is more easily dissolved in the surface treatment liquid (A).

[0081] The film thickness of the film is not particularly limited. In order to better play the function as a barrier layer to the corrosive environment, the film thickness of the film is preferably 0.3 μm or more. On the other hand, in the case of automobile steel sheets, there is a process of assembling the steel sheets to each other by spot welding after being processed into a prescribed shape by stamping. At this time, if the film is too thick, sometimes the current during welding does not flow and the welding becomes poor. Therefore, in the case of using spot welding for the joining of steel plates, the film thickness of the film is preferably 4.0 μm or less. It should be noted that in a film composed of multiple layers, the total film thickness of the multiple layers is set as the film thickness of the film.

[0082] For the film thickness of the film, the cross section of the film is observed, and the thickness of the film (the thickness from the surface of the galvanized steel sheet to the surface of the film) is measured at multiple locations (3 locations) in any field of view, and the average value thereof is taken as the film thickness. The method of cross-section processing is not particularly limited, and examples thereof include FIB (Focused Ion Beam) processing and the like.

[0083] Next, the method for producing the surface-treated galvanized steel sheet disclosed in the present invention is described. A coating is formed by applying a surface treatment liquid containing the additive on at least one side of the galvanized steel sheet as the substrate and drying the surface treatment liquid. The surface treatment liquid contains the additive and the organic resin.

[0084] There is no particular limitation on the method of applying the surface treatment liquid on the surface of the galvanized steel sheet, and it can be any one of the coating method (rod coating), spraying method, and dipping method (and roller drawing). The heating and drying method after applying the surface treatment liquid is also not particularly limited, and an induction heater or the like can be used. The heating temperature is preferably a temperature below the decomposition temperature of the above-mentioned additive component. Specifically, the heating temperature after applying the surface treatment liquid is preferably below 180°C, more preferably below 160°C, and further preferably below 140°C. In addition, in the case of a film consisting of two or more layers, it is preferred to apply the surface treatment liquid and heat and dry it by the above method each time each layer is formed.

[0085] The surface-treated galvanized steel sheet has the following advantages: by forming a film containing specific components on its surface, it has excellent delayed fracture resistance that effectively suppresses delayed fracture, and this excellent delayed fracture resistance is independent of the composition of the base steel sheet and can be obtained even in a low-temperature environment. In addition, since the film on the surface of the surface-treated galvanized steel sheet does not use expensive materials such as bismuth, it can be manufactured at a low cost. Therefore, it can be applied to automobiles and building materials, and by using it for these purposes, the weight can be reduced.

[0086] The case of evaluating the tensile strength of the steel plate (base steel plate) of the surface-treated galvanized steel plate is supplemented. When evaluating the tensile strength of the steel plate (base steel plate) of the surface-treated galvanized steel plate, as described above, the galvanized layer and the film can be removed from the surface-treated galvanized steel plate to separate the single steel plate, and the tensile strength of the steel plate can be evaluated. The removal of the film and the galvanized layer can be performed, for example, by immersing the surface-treated galvanized steel plate in 10% by mass hydrochloric acid at 30°C for 60 seconds. The method of removing the galvanized layer and the film may be a method other than the above as long as it does not affect the tensile strength of the steel plate. It should be noted that, generally, the tensile strength of the steel plate, the tensile strength of the galvanized steel plate, and the tensile strength of the surface-treated galvanized steel plate are the same. In the present embodiment, the value of the tensile strength of the steel plate can be replaced by the tensile strength of the galvanized steel plate or the tensile strength of the surface-treated galvanized steel plate. That is, the tensile strength of the surface-treated galvanized steel plate disclosed in the present invention is above 1180MPa.

[0087] Example

[0088] [Example 1]

[0089] As the galvanized steel sheet, the following alloyed hot-dip galvanized steel sheet was used: the base steel sheet had a composition containing C: 0.22 mass%, Si: 1.2 mass%, Mn: 3.0 mass%, P: 0.007 mass%, S: 0.0005 mass%, and the remainder was composed of Fe and inevitable impurities, and the tensile strength was 1580 MPa, the plate thickness was 1.4 mm, and the steel sheet had an alloyed hot-dip galvanized layer on both the front and back surfaces. The coating adhesion of the alloyed hot-dip galvanized steel sheet was 44 g / m per single surface. 2 The Fe content of the alloyed galvannealed layer was 14% by mass. The alloyed hot-dip galvannealed steel sheet was immersed in toluene and ultrasonically cleaned for 5 minutes to remove the rust preventive oil, thereby preparing a test material.

[0090] Each carboxylic acid and amine were added to 1 kg of deionized water at the molar ratio shown in Table 1, and heated to 80° C. to dissolve to obtain a solution. Then, the solution was cooled to 20° C. to precipitate crystals of the additive.

[0091] The hydrogen permeation current density of each additive was measured by the above method. The evaluation results are shown in Tables 1-1 to 1-3.

[0092] Production of Surface-treated Galvanized Steel Sheets

[0093] The obtained crystals of the additive are filtered and dried, and then mixed with an organic resin in the mass ratio shown in Table 2 to obtain a surface treatment liquid. Using the following A1 to A4 as organic resins, a surface treatment liquid containing any organic resin and a specified additive (in part of the comparative example, a surface treatment liquid containing only an organic resin) is applied to the surface of the test material. The coating method of the surface treatment liquid is shown in Table 2. Then, the induction heater is used to heat the plate so that the plate temperature reaches 140°C, thereby forming a film on the test material to obtain a surface-treated galvanized steel sheet.

[0094] A1: Epoxy resin (manufactured by Japan Epoxy Resins Co., Ltd., trade name: jER1009)

[0095] A2: Acrylic resin (manufactured by DIC Corporation, trade name: 40-418EF)

[0096] A3: Polyurethane resin (manufactured by Dainippon Paint Co., Ltd., trade name: V Top RC Clear)

[0097] A4: Fluorine resin (manufactured by Asahi Glass Co., Ltd., trade name: LUMIFLON LF552)

[0098] The following properties were evaluated for each surface-treated galvanized steel sheet obtained as described above. The evaluation results are shown in Table 2. The film thickness of the film was measured by the above-mentioned method.

[0099] (1) Evaluation of delayed fracture resistance (low temperature)

[0100] The galvanized steel sheets of the invention example and the comparative example were cut into sizes of 32 mm in width and 110 mm in length, and then ground to a width of 30 mm to remove residual stress during shearing to prepare test pieces. The test pieces were bent 90° with a bending radius of 10 mm using a 3-point bending tester. Figure 4 As shown in FIG. 1 , the shape of the test piece 1 is fixed in such a way that the inner spacing of the flange ends after being constrained by the bolts 2 and the nuts 3 (after the shape of the test piece is fixed by tightening with the bolts 2 and the nuts 3) is narrowed by 13.8 mm relative to the inner spacing of the flange ends before being constrained, thereby obtaining a test piece for evaluating delayed fracture resistance performance. The test piece for evaluating delayed fracture resistance performance thus prepared is subjected to corrosion simulating a low temperature environment. Figure 5 The dry-wet repetitive test of the cycle shown is carried out for a maximum of 28 days. In this cycle, the test temperature is constant (10°C), and the humidity cycle consists of a Dry step with a relative humidity of 30%, a Wet step with a relative humidity of 90%, and a humidity increase and decrease step, totaling four steps as one cycle. Each step is switched every 2 hours, and a cycle is repeated for 8 hours. In addition, twice a week, at the beginning of the Dry step, after cleaning with pure water, 27wt% (attached salt amount: 10000mg / m per single side) is added.2 ) is sprayed onto the delayed fracture resistance test piece to impart chloride. Here, twice a week means that the treatment is performed after 3 or 4 days of vacancy after the first treatment. For example, when the first treatment is performed on Monday, the second treatment is performed on Thursday and Friday. This is repeated thereafter.

[0101] At the beginning of the drying process of every three cycles (every day), the bending part of the test piece for delayed fracture resistance evaluation was visually confirmed to see if cracks occurred, and the number of days until cracks occurred (hereinafter referred to as "crack days") was investigated. In this test, three samples were tested for each galvanized steel sheet of the invention example and the comparative example, and the average value of the crack days was used to evaluate the delayed fracture resistance according to the following benchmark. It should be noted that the crack days in the table are 29 days, which means that no cracks occurred in the results of this embodiment. In the following description, the symbols ◎, ○, △ and × represent good to poor, respectively.

[0102] ◎: Crack days are more than 29 days

[0103] 0: Crack days are more than 20 days and less than 29 days

[0104] △: Crack days are more than 10 days and less than 20 days

[0105] ×: Crack days less than 10 days

[0106] (2) Evaluation of corrosion resistance after painting

[0107] The galvanized steel sheets of the invention examples and comparative examples were cut into sizes of 150 mm × 70 mm, respectively, and flat test pieces were made as test pieces for corrosion resistance evaluation. The test pieces for corrosion resistance evaluation used "PALBOND" manufactured by Japan Parkersei Co., Ltd., and were subjected to chemical conversion treatment by immersion under standard conditions (35°C, 120 seconds) to make chemical conversion treatment test pieces. Next, the chemical conversion treatment test pieces were subjected to electrodeposition coating and sintering treatment using the electrodeposition coating "GT-100" manufactured by Kansai Paint Co., Ltd. to make painted test pieces. The coating thickness of the electrodeposition coating was 15 μm, and the coating thickness was measured using a commercially available electromagnetic film thickness meter. For the painted test pieces, a cutting knife was used to form an X-cut (intersection angle 60° to 90°) that reached the film of the surface-treated galvanized steel sheet, and a salt spray test specified in JIS Z2371 was performed for 840 hours. The maximum rust width from the cross cut of the test piece after the test was measured to evaluate the corrosion resistance. The corrosion resistance was evaluated as follows by calculating the maximum rust width A of each test piece when the maximum rust width of the galvanized steel sheet without a coating was set to 1.

[0108] ◎:A≤0.8

[0109] ○:0.8<A≤0.95

[0110] △: 0.95<A≤1.2

[0111] ×: 1.2<A

[0112] In Table 2, No. 1 (comparative example) is a plated steel sheet without a film formed thereon (comparative example of a galvanized steel sheet state), and it is found that cracks are generated at an early stage and the delayed fracture resistance is low.

[0113] Steel plates No. 3 to No. 161 are examples of coating the surface of alloyed hot-dip galvanized steel plates by applying a surface treatment liquid mixed with additives and epoxy resin (A1) to the surface of the steel plates using a coating method (rod coating). In addition, steel plate No. 2 is an example of forming a coating by similarly applying a surface treatment liquid of epoxy resin (A1) without additives. Among them, steel plates No. 4 to 164 with additive contents within the range disclosed in the present invention can all obtain excellent delayed fracture resistance, and the corrosion resistance after coating is also good.

[0114] In contrast, the delayed fracture resistance of the steel sheet No. 2 without additives and the steel sheet No. 3 with additive content below the range disclosed in the present invention slightly improved compared with the steel sheet No. 1 without film, but was inferior to the delayed fracture resistance of the steel sheets No. 4 to 163 as inventive examples. The steel sheets No. 162 and No. 163 are inventive examples in which the film forming method of the film is changed compared with the steel sheet No. 5, and both can obtain excellent delayed fracture resistance and have good corrosion resistance after painting.

[0115] Steel sheets No. 164 to No. 167 are inventive examples in which the type of organic resin is changed. All of them can obtain excellent delayed fracture resistance and also have good corrosion resistance after painting.

[0116] [Table 1-

[0117]

[0118] [Table 1-2]

[0119]

[0120] [Table 1-3]

[0121]

[0122] Table 2-

[0123]

[0124] The underline indicates that the invention is outside the applicable range.

[0125] [Table 22--2]

[0126]

[0127] [Table 2-3]

[0128]

[0129] [Example 2]

[0130] In the same manner as in Example 1, alloyed hot-dip galvanized steel sheets were prepared as test materials.

[0131] Production of Surface-treated Galvanized Steel Sheets

[0132] <Film formation of lower layer>

[0133] The crystals of the additive obtained by the method described in Example 1 were filtered and dried, and then mixed with a surface treatment liquid B having the following composition at the mass ratio shown in Table 3 to obtain a surface treatment liquid mixed with the additive. It should be noted that for component (d), the mixing ratio (mass %) of 1-hydroxymethane-1,1-diphosphonic acid and tartaric acid is 9:1. After applying the surface treatment liquid to the surface of the test material by rod coating, it was heated by an induction heater in such a way that the plate temperature reached 140°C, thereby forming a lower film on the test material. It should be noted that the lower film is a film (base film) that becomes the base of the upper film described later.

[0134] Surface treatment liquid B:

[0135]

[0136] <Film formation of the upper layer>

[0137] The crystals of the additive obtained by the method described in Example 1 were filtered and dried, and then mixed with an organic resin in the mass ratio shown in Table 3 to obtain a surface treatment liquid. Using the following A1 or A5 as an organic resin, a surface treatment liquid containing any organic resin and a specified additive (in part of the comparative example, a surface treatment liquid containing only an organic resin) was applied to the surface of the test material after the lower film was formed by rod coating. Then, the upper film was formed on the test material after the lower film was formed by heating with an induction heater in such a way that the plate temperature reached 140°C, thereby obtaining a surface treated galvanized steel sheet having two layers of film.

[0138] A1: Epoxy resin (manufactured by Japan Epoxy Resins Co., Ltd., trade name: jER1009)

[0139] A5: Epoxy ester resin (DIC Corporation, trade name: WATERSOL EFD-5560)

[0140] The galvanized steel sheets obtained as described above were evaluated for delayed fracture resistance and corrosion resistance after coating by the same methods as in Example 1. The evaluation results are shown in Table 3 together with the composition of the coating. The film thickness of the coating was also measured in the same manner as in Example 1 and is shown in Table 3.

[0141] In Table 3, No. 1 (comparative example) is a plated steel sheet without a film formed thereon (comparative example of an alloyed hot-dip galvanized steel sheet state), and it is found that cracks are generated at an early stage and the delayed fracture resistance is low.

[0142] Steel sheets No. 2 to No. 35 are examples of surface treated galvanized steel sheets with lower and upper films formed on hot dip galvanized steel sheets. Steel sheets No. 5 to 35 with additive contents within the range disclosed herein all have excellent delayed fracture resistance and good corrosion resistance after painting.

[0143] In contrast, the delayed fracture resistance of the steel sheet No. 2 without additives and the steel sheets No. 3 and No. 4 having additive contents below the range disclosed in the present invention are slightly improved compared with the steel sheet No. 1 without a film, but are inferior to the delayed fracture resistance of the steel sheets No. 5 to 35 as inventive examples.

[0144]

[0145] Explanation of symbols

[0146] 100 Hydrogen intrusion measurement device

[0147] 10 Test piece

[0148] 11 Hydrogen intrusion surface

[0149] 12 Hydrogen detection surface

[0150] 20 Hydrogen generation tank

[0151] 21 Hydrogen detection tank

[0152] 23. Reference electrode

[0153] 24 pairs of electrodes

[0154] 30 Potentiostat

[0155] 40 zinc plate

[0156] 50 Palladium coating

[0157] 1 Test piece

[0158] 2 Bolts

[0159] 3 Nut

Claims

1. A surface-treated galvanized steel sheet having: Steel plates with a tensile strength of 1180 MPa or more, A galvanized layer formed on at least one surface of the steel sheet, and The film formed on the zinc plating layer, The film contains 10% to 50% by mass of additives in terms of solid content. Here, the additive is at least one selected from the group consisting of salts of aliphatic dicarboxylic acids having 2 to 8 carbon atoms and alkylamines having 6 to 18 carbon atoms, salts of aliphatic dicarboxylic acids having 2 to 8 carbon atoms and cycloalkylamines having 6 to 18 carbon atoms, and salts of aromatic monocarboxylic acids having 7 to 12 carbon atoms and alkylamines having 6 to 18 carbon atoms.

2. The surface-treated galvanized steel sheet according to claim 1, wherein: The aliphatic dicarboxylic acid having 2 to 8 carbon atoms is at least one selected from oxalic acid, maleic acid, fumaric acid, malonic acid, succinic acid, glutaric acid and adipic acid, The aromatic monocarboxylic acid having 7 to 12 carbon atoms is at least one selected from benzoic acid, m-aminobenzoic acid, p-aminobenzoic acid, p-nitrobenzoic acid, salicylic acid, p-hydroxybenzoic acid, toluic acid, p-tert-butylbenzoic acid and β-hydroxynaphthoic acid, The alkylamine having 6 to 18 carbon atoms is at least one selected from octadecylamine, dodecylamine, decylamine, monooctylamine, monohexylamine, monodecylamine, monododecylamine and mono-2-ethylhexylamine. The cycloalkylamines having 6 to 18 carbon atoms are cyclohexylamine, dicyclohexylamine and tricyclohexylamine.

3. The surface-treated galvanized steel sheet according to claim 1 or 2, wherein: The hydrogen permeation current density iH was measured by adding 1 g / L of the additive to a solution simulating a corrosive environment. t The hydrogen permeation current density iH0 measured without adding the additive to the solution satisfies the following formula (1), them t / iH0≤0.50···(1) Here, the hydrogen permeation current density iH is measured as follows: a zinc plate and a test steel plate are brought into electrical connection, one surface of the zinc plate and the test steel plate is exposed to the solution and the one surface is used as a hydrogen intrusion surface, The other surface of the test steel plate is used as a hydrogen detection surface having a palladium-plated film. The measurement is performed using an electrochemical cell provided on the hydrogen detection surface.

4. The surface-treated galvanized steel sheet according to any one of claims 1 to 3, wherein A base film is provided between the zinc plating layer and the film.

5. The surface-treated galvanized steel sheet according to any one of claims 1 to 4, wherein The film includes one or more selected from epoxy resins, acrylic resins, polyurethane resins, vinyl resins, phenolic resins, polyester resins, fluororesins, polyolefin resins, and epoxy ester resins.