Surface-treated copper foil, copper-clad laminate, and printed wiring board

By using the surface treatment layer of the surface-treated copper foil in the manufacturing of printed wiring boards, the wettability of the resin-made substrate is improved, and the problems of circuit machining properties and foreign matter are solved, thereby achieving excellent circuit machining properties and reducing transmission losses.

CN118891402APending Publication Date: 2024-11-01FURUKAWA ELECTRIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030520.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-30
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to achieve surface-treated copper foils with excellent circuit machining properties and are not prone to transmission losses and foreign matters in the manufacturing of printed wiring boards. Especially during the etching process, the tangent angle of the bottom end of the circuit is small, resulting in migration, and the resin-made substrate is made of base material. The low wettability makes it difficult for etching liquid and cleaning liquid to spread, resulting in foreign matter residues.

Method used

The surface-treated copper foil has a copper foil substrate and a surface treatment layer. The surface-treated layer is composed of a roughening treatment layer and an anti-rust treatment layer. The fine concave and convex shape is formed by capsule plating or etching concave and convex treatment, which improves the rotation of the resin-made substrate. The wettability of the printing surface ensures that the contact angle difference is above 5° and below 35°, and ensures the effective spread of etching liquid and cleaning liquid.

Benefits of technology

Excellent circuit machining performance is achieved, transmission loss and foreign matter generation are reduced, and high-frequency signal transmission performance of the printed wiring board and cleanliness of the manufacturing process are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891402A_ABST
    Figure CN118891402A_ABST
Patent Text Reader

Abstract

Provided is a surface-treated copper foil which has excellent circuit processability and is not susceptible to the occurrence of transmission loss and foreign matter. When the optical roughness of the surface (20a) of the surface treatment layer (20) of the surface-treated copper foil (30) is measured according to the method specified in ISO 25178, the arithmetic average roughness (Sa) is 0.04 [mu] m or more and 0.30 [mu] m or less. After a resin member (40) is bonded to a surface treatment layer (20) of a surface-treated copper foil (30), the surface-treated copper foil (30) is removed by etching, and a contact angle (theta 1) of distilled water is measured in accordance with a static drop method specified in JIS R3257: 1999 for a transfer surface (40a), which is the surface of the residual resin member (40) to which the surface-treated copper foil (30) is bonded. For a non-transfer surface, which is a surface to which the surface-treated copper foil (30) is to be attached after the surface-treated copper foil (30) of the resin member (40) before the surface-treated copper foil (30) is attached, the contact angle ([theta] 0) of distilled water is measured by a static drop method. The difference [theta] 0-[theta] 1 between the contact angles [theta] 0 and [theta] 1 is 5-35 degrees inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a surface-treated copper foil that can be suitably used in the production of a printed wiring board or the like, and a copper-clad laminate and a printed wiring board using the surface-treated copper foil. Background Art

[0002] In recent years, with the development of higher frequencies of signals, more and more high-frequency signals are transmitted to printed wiring boards mounted on electronic devices. Therefore, for surface-treated copper foil used as a material for printed wiring boards, in order to reduce the transmission loss of high-frequency signals, research has been conducted to make the surface roughness low (for example, see Patent Document 1).

[0003] In addition, with the high-density mounting and multifunctionalization of printed wiring boards, the circuit wiring is also developing. In order to form fine wiring, a surface-treated copper foil with good circuit processability is required. In order to improve the circuit processability, research has been conducted to make the surface low in roughness (for example, see Patent Document 2). In addition, in addition to this, the main reasons for the improvement of the metal used to treat the copper foil surface (for example, see Patent Document 3) and the improvement of the concave-convex shape transferred to the resin surface (for example, see Patent Documents 4 and 5) have also been studied.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Publication No. 2019-210521

[0007] Patent Document 2: Japanese Patent Publication No. 2017-20117

[0008] Patent Document 3: Japanese Patent Publication No. 2019-81913

[0009] Patent Document 4: Japanese Patent Gazette No. 6945523

[0010] Patent Document 5: International Publication No. 2020 / 105289 Summary of the invention

[0011] Technical problem to be solved by the invention

[0012] However, even if the surface roughness of the surface treated copper foil is reduced, the target fine wiring cannot be obtained sometimes. In the past, as an indicator of circuit processability, the etching factor obtained by the bottom width, top width and height of the circuit was widely used. In addition, it is known that the angle of the tangent at the bottom end of the circuit is also very important. That is, even if the etching factor is a good value evaluated in the past, if the angle of the tangent at the bottom end of the circuit is small (that is, the bottom width is larger than the top width of the circuit, and the cross-section of the circuit becomes a shape with a widened hem), migration sometimes occurs. It is expected that the reason is that the etching of the interface of the end of the circuit when observed from a microscopic viewpoint is poor, and there is a tendency that the smaller the angle of the tangent at the bottom end of the circuit, the easier it is to migrate.

[0013] In addition, in the research of the present inventors, the surface roughness of the surface-treated copper foil was reduced, and as a result, the following new technical problem was discovered: in the process of manufacturing a printed wiring board by stacking a resin substrate after etching away the surface-treated copper foil of a copper-clad laminate, foreign matter is easily generated between the resin substrate constituting the copper-clad laminate and the resin substrate stacked subsequently.

[0014] The technical problem of the present invention is to provide a surface-treated copper foil, a copper-clad laminate, and a printed wiring board which are excellent in circuit processability and are less likely to generate transmission loss and foreign matter.

[0015] Technical solutions for solving technical problems

[0016] The gist of a surface-treated copper foil according to one embodiment of the present invention is a surface-treated copper foil having a copper foil substrate and a surface-treated layer formed on at least one surface of the copper foil substrate, wherein the surface-treated layer is composed of one or both of a roughening treatment layer and a rust-proof treatment layer, and when the optical roughness of the surface of the surface-treated layer is measured according to the method specified in ISO25178, the arithmetic mean roughness Sa is 0.04 μm or more and 0.30 μm or less, and after a resin component is bonded to the surface-treated layer of the surface-treated copper foil, the surface-treated copper foil is removed by etching, and the contact angle θ1 of distilled water is measured according to the sessile drop method specified in JIS R3257:1999 for the surface of the remaining resin component to which the surface-treated copper foil is bonded, i.e., the transfer surface, and the contact angle θ0 of distilled water is measured according to the sessile drop method for the surface of the resin component before bonding the surface-treated copper foil, i.e., the non-transfer surface to which the surface-treated copper foil is bonded later, and in this case, the difference θ0-θ1 between the contact angle θ0 and the contact angle θ1 is 5° or more and 35° or less.

[0017] A copper-clad laminate according to another aspect of the present invention is gist of comprising the surface-treated copper foil according to the above-mentioned one aspect and a resin base material bonded to the surface-treated layer of the surface-treated copper foil.

[0018] A printed wiring board according to another aspect of the present invention is gist of including the surface-treated copper foil according to the above-mentioned other aspect.

[0019] Effects of the Invention

[0020] According to the present invention, circuit processability is excellent, and transmission loss and foreign matter are unlikely to occur. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a cross-sectional view illustrating the structure of a surface-treated copper foil according to one embodiment of the present invention.

[0022] Figure 2 This is a diagram for explaining the wettability of the transfer surface of the resin substrate.

[0023] Figure 3 It is a figure explaining the manufacturing method of the copper-clad laminate and the printed wiring board which concern on one embodiment of this invention. DETAILED DESCRIPTION

[0024] One embodiment of the present invention will be described. It should be noted that the embodiment described below is an example of the present invention. In addition, various changes or improvements can be made to this embodiment, and the embodiment in which such changes or improvements are made is also included in the present invention.

[0025] In order to solve the above technical problems, the present inventors have conducted intensive research focusing on the wettability of the surface of a resin substrate used in the manufacture of a copper-clad laminate and a printed wiring board. Figure 1 , 2 , 3 are explained in detail.

[0026] The manufacturing process of the printed wiring board 60 includes a bonding process of bonding the surface treated copper foil 30 and the resin substrate 40 to manufacture the copper clad laminate 50 (see Figure 3 (b)), and an etching step of removing unnecessary portions of the surface treated copper foil 30 of the copper clad laminate 50 other than the portion to be the circuit 31 by etching with an etching solution (see Figure 3 (c)). In the laminating step, the resin substrate 40 is laminated on the surface treated layer 20 of the surface treated copper foil 30 (see Figure 3 (a)).

[0027] At this time, the shape of the surface 20a of the surface treatment layer 20 of the attached surface treatment copper foil 30 is transferred to the surface of the surface treatment copper foil 30 of the resin substrate 40 remaining after etching. That is, the surface of the resin substrate 40 to which the surface treatment copper foil 30 is attached becomes the transfer surface (replica) 40a of the surface of the attached surface treatment copper foil 30.

[0028] According to the research of the present inventors, as the surface roughness of the surface-treated copper foil 30 decreases, the surface roughness of the transfer surface 40a of the resin substrate 40 also decreases, and the wettability of the transfer surface 40a decreases. When the wettability of the surface of the resin substrate 40 is low, it is difficult for the etching liquid to spread to the end (the end in the wiring width direction of the circuit 31) of the circuit 31 (the surface-treated copper foil 30 remaining due to etching) on ​​the resin substrate 40 during etching, so it can be considered that the circuit processability is reduced. Whether the etching liquid spreads to the end of the circuit 31, especially to the bottom end 31b of the circuit 31 (the portion of the end of the circuit 31 adjacent to the resin substrate 40 (refer to Figure 2 ))'s processability becomes an important factor.

[0029] In addition, in the manufacturing process of the printed wiring board 60, after the etching process, there is a cleaning process of cleaning the resin substrate 40 having the circuit 31 with a cleaning liquid. However, if the wettability of the surface of the resin substrate 40 is low, it is difficult for the cleaning liquid to spread over the entire surface of the resin substrate 40, so that the foreign matter 100 existing on the resin substrate 40 and the circuit 31 may not be fully cleaned with the cleaning liquid (see Figure 3 Then, after the cleaning process, another resin substrate 41 is bonded to the surface of the resin substrate 40 having the circuit 31, where the circuit 31 is formed, to manufacture the printed wiring board 60. However, if the foreign matter 100 is not sufficiently cleaned in the cleaning process, the foreign matter 100 may remain between the two bonded resin substrates 40 and 41 (see Figure 3 (d)).

[0030] That is, the inventors' research has revealed that if the wettability of the surface of the resin substrate 40 is low, foreign matter 100 is easily generated on the printed wiring board 60. It should be noted that the foreign matter 100 includes attachments attached to the surface-treated copper foil 30 and the resin substrate 40 before lamination, and coagulated salts contained in the etching solution.

[0031] As described above, the present inventors have found that the wettability of the transfer surface 40a of the resin substrate 40 after the etching process is a very important factor in the manufacture of the printed wiring board 60. In addition, the present inventors have found that the wettability of the transfer surface 40a of the resin substrate 40 after the etching process can be evaluated by the contact angle of distilled water measured by the sessile drop method specified in JIS R3257:1999.

[0032] That is, the surface-treated copper foil 30 according to the present embodiment is a surface-treated copper foil 30 having a copper foil substrate 10 and a surface-treated layer 20 formed on at least one surface of the copper foil substrate 10, wherein the surface-treated layer 20 is composed of one or both of a roughening treatment layer 21 and a rust-proof treatment layer 22 (see Figure 1 ). It should be noted that Figure 1 An example of a surface-treated copper foil 30 is shown in which the surface-treated layer 20 is formed only on one surface of the copper foil base 10 and the surface-treated layer 20 is composed of both the roughening-treated layer 21 and the rust-proofing-treated layer 22 .

[0033] Moreover, when the optical roughness of the surface 20a of the surface-treated layer 20 of the surface-treated copper foil 30 was measured by the method specified in ISO25178, the arithmetic mean roughness Sa was 0.04 μm or more and 0.30 μm or less.

[0034] In addition, after the resin substrate 40 (corresponding to the "resin member" as a constituent element of the present invention) used when manufacturing the copper-clad laminate 50 and the printed wiring board 60 is laminated on the surface treated layer 20 of the surface treated copper foil 30, the surface treated copper foil 30 is removed by etching, and the contact angle θ1 of distilled water is measured on the transfer surface 40a of the remaining resin substrate 40 (hereinafter, sometimes referred to as "the contact angle θ1 of distilled water on the transfer surface after copper foil etching"). The transfer surface 40a of the resin substrate 40 is the surface of the resin substrate 40 to which the surface treated copper foil 30 is laminated.

[0035] In addition, the contact angle θ0 of distilled water was measured for the non-transferred surface of the resin substrate 40 before being bonded to the surface-treated copper foil 30 (hereinafter, sometimes referred to as "the contact angle θ0 of distilled water on the non-transferred surface before copper foil bonding"). The non-transferred surface of the resin substrate 40 is the surface of the resin substrate 40 before being bonded to the surface-treated copper foil 30, to which the surface-treated copper foil 30 is bonded later.

[0036] The contact angles θ0 and θ1 of distilled water are measured by the sessile drop method specified in JIS R3257: 1999. In this case, in the surface-treated copper foil 30 according to the present embodiment, the difference θ0-θ1 between the contact angle θ0 and the contact angle θ1 is 5° or more and 35° or less. The difference θ0-θ1 between the contact angle θ0 and the contact angle θ1 is a measure of how much the wettability of the resin surface has changed by laminating with the copper foil.

[0037] When the copper-clad laminate 50 and the printed wiring board 60 are manufactured using such a surface-treated copper foil 30, the wettability of the transfer surface 40a of the resin substrate 40 used in the manufacture of the copper-clad laminate 50 and the printed wiring board 60 becomes high. Therefore, the obtained copper-clad laminate 50 and the printed wiring board 60 are not only less likely to cause transmission loss, but also have excellent circuit processability, and foreign matter is less likely to be generated between the resin substrate 40 constituting the copper-clad laminate 50 and the other resin substrate 41 laminated thereafter for the manufacture of the printed wiring board 60.

[0038] That is, by making the difference θ0-θ1 of the contact angle within the above numerical range, the wettability of the surface of the resin substrate 40 can be well maintained, so that during etching, the etching liquid easily spreads to the bottom end 31b of the circuit 31 on the resin substrate 40, and in the cleaning process after the etching process, the cleaning liquid easily spreads to the entire surface of the resin substrate 40. As a result, it is possible to manufacture a copper-clad laminate 50 and a printed wiring board 60 that have excellent circuit processability and foreign matter suppression and are less likely to cause transmission loss.

[0039] As described above, the surface-treated copper foil 30 according to the present embodiment can be suitably used for manufacturing copper-clad laminates, printed wiring boards, etc. That is, the copper-clad laminate 50 according to the present embodiment includes the surface-treated copper foil 30 according to the present embodiment and the resin substrate 40 attached to the surface-treated layer 20 of the surface-treated copper foil 30. In addition, the printed wiring board 60 according to the present embodiment includes the copper-clad laminate 50 according to the present embodiment.

[0040] Hereinafter, the surface-treated copper foil 30 , the copper-clad laminate 50 , and the printed wiring board 60 according to the present embodiment will be described in more detail.

[0041] (A) About surface treated copper foil

[0042] The copper foil substrate 10 as the raw material of the surface-treated copper foil 30 involved in this embodiment preferably has a ten-point average roughness Rzjis of 2 μm or less on both sides before the surface is subjected to a roughening treatment or the like. The ten-point average roughness Rzjis can be measured using a contact surface roughness measuring machine according to the method specified in JIS B0601: 2001. If the ten-point average roughness Rzjis of the surface is 2 μm or less, the adhesion with the resin substrate 40 is likely to be good.

[0043] The thickness of the copper foil base 10 before the roughening treatment or the like is determined by the target value of the thickness of the copper foil base 10 after the roughening treatment, but is preferably 5 μm or more and 40 μm or less.

[0044] Surface treatment is applied to at least one surface of the copper foil substrate 10 as a raw material to form a surface treatment layer 20, and the surface treated copper foil 30 involved in the present embodiment is manufactured. As the surface treatment, one or both of the roughening treatment and the rust-proof treatment are performed to roughen the surface. That is, the surface treatment layer 20 is composed of one or both of the roughening treatment layer 21 formed by the roughening treatment and the rust-proof treatment layer 22 formed by the rust-proof treatment. In the case where the surface treatment layer 20 is composed of both the roughening treatment layer 21 and the rust-proof treatment layer 22, the roughening treatment layer 21 is formed on the surface of the copper foil substrate 10, and the rust-proof treatment layer 22 is formed thereon. In addition, a chemical sealant treatment using a chemical sealant such as a silane coupling agent can also be implemented after the rust-proof treatment, and a chemical sealant layer such as a silane coupling agent layer is formed on the rust-proof treatment layer 22. These surface treatments will be described in detail later.

[0045] When manufacturing the surface-treated copper foil 30 involved in the present embodiment, for the purpose of improving the above-mentioned wettability, a concavo-convex forming treatment is performed on at least one surface of the copper foil substrate 10 before or after the general roughening treatment. Then, the roughening treatment layer 21 is formed by these general roughening treatments and concavo-convex forming treatments. The concavo-convex forming treatment is a treatment for forming fine concavo-convex shapes that do not affect the degree of transmission loss on the surface of the copper foil substrate 10. As examples of the concavo-convex forming treatment, capsule plating treatment and etching concavo-convex treatment can be cited.

[0046] First, an example of capsule plating treatment is described. The capsule plating treatment is performed before the general roughening treatment. By using a mesh-shaped cathode shielding plate, the surface of the copper foil substrate 10 is smoothly copper-plated (capsule plating), and a fine concavo-convex shape is formed on the surface of the copper foil substrate 10. By using a mesh-shaped cathode shielding plate, a concavo-convex shape with uniform deviation can be formed on the surface of the copper foil substrate 10.

[0047] At this time, by controlling the plating conditions such as the opening ratio of the grid-shaped cathode shielding plate, the current density, and the energizing time, a fine concavo-convex shape that does not affect the degree of transmission loss can be formed on the surface of the copper foil base 10. As a result, the wettability of the transfer surface 40a of the resin substrate 40 can be well controlled.

[0048] The plating solution can be a commonly used copper sulfate plating solution. The material for forming the cathode shielding plate is preferably a material with chemical resistance and insulation properties, such as resins such as vinyl chloride, polyethylene, and polybutylene terephthalate. The opening area of ​​the mesh portion is preferably 1 μm 2 Above and 100μm 2 Below, more preferably 10 μm 2 Above and 100μm 2In addition, the opening ratio of the mesh portion is preferably 5% or more and 15% or less. If the opening area and the opening ratio are within the above numerical ranges, a fine concavo-convex shape that does not affect the degree of transmission loss can be formed on the surface of the copper foil substrate 10, and the wettability of the transfer surface 40a of the resin substrate 40 becomes good.

[0049] Next, an example of etching unevenness treatment is described. Etching unevenness treatment is performed after general roughening treatment and before rust prevention treatment. After the roughening treatment, rust prevention metals such as nickel (Ni) and cobalt (Co) with chemical resistance are electrolytically deposited under conditions of high current density and extremely short time, and then the surface is immersed in an etching solution for a short time for etching, thereby forming a fine uneven shape on the surface of the copper foil substrate 10.

[0050] For nickel electrolysis, a general electrolytic bath containing nickel sulfate, nickel sulfamate, etc. can be used. In addition, the current density can be, for example, 1.0 A / dm 2 As described above, the energization time can be, for example, 0.5 seconds or more and 2.0 seconds or less.

[0051] By electrolyzing the rust-proof metal at a high current density and in a short time, the rust-proof metal is electrolyzed only on the tops of the roughened particles formed by the general roughening treatment. Therefore, the area other than the tops of the roughened particles on the surface of the copper foil substrate 10 is etched, and a fine concavo-convex shape is formed in the area other than the tops of the roughened particles on the surface of the copper foil substrate 10.

[0052] Furthermore, by controlling the conditions such as the immersion time in the etching solution, a fine concavo-convex shape that does not affect the degree of transmission loss can be formed on the surface of the copper foil base 10. As a result, the wettability of the transfer surface 40a of the resin base material 40 can be well controlled.

[0053] As the etching solution, for example, a mixed solution of sulfuric acid-hydrogen peroxide solution and a general copper etching solution such as hydrochloric acid can be used. The immersion time in the etching solution can be, for example, more than 2 seconds and less than 10 seconds. If the immersion time in the etching solution is within the above numerical range, a fine concavo-convex shape that does not affect the transmission loss can be formed on the surface of the copper foil substrate 10, and the wettability of the transfer surface 40a of the resin substrate 40 is good. In addition, in the subsequent rust-proofing treatment and chemical adhesive treatment steps, the surface of the copper foil substrate 10 can be uniformly treated, and good adhesion and corrosion resistance can be imparted.

[0054] By the above-mentioned concavo-convex forming treatment, it is possible to obtain a copper foil substrate 10 having a surface with good wettability to the transfer surface 40a of the bonded resin substrate 40. As described above, the wettability of the transfer surface 40a of the resin substrate 40 can be evaluated by the contact angle of distilled water measured by the sessile drop method, and the difference θ0-θ1 between the distilled water contact angle θ0 of the non-transfer surface before copper foil bonding and the distilled water contact angle θ1 of the transfer surface 40a after copper foil etching needs to be 5° or more and 35° or less.

[0055] When the optical roughness of the transfer surface 40a is measured according to the method specified in ISO 25178, it is preferred that the arithmetic mean roughness Sa is 0.020 μm or more and 0.070 μm or less, and the volume Vvc of the space in the core is 0.030 mL / m 2 Above and 0.110mL / m 2 If the arithmetic mean roughness Sa of the transfer surface 40a and the volume Vvc of the space of the core are within the above numerical ranges, even if the surface roughness of the surface treatment layer 20 of the surface-treated copper foil 30 is small, the wettability of the transfer surface 40a becomes better, and in addition, the processed shape of the circuit can be further well maintained. The reason is not clear, but it is considered that it is because the etching amount of the resin-copper foil interface can be well controlled.

[0056] When the optical roughness of the transfer surface 40a is measured according to the method specified in ISO 25178, it is more preferable that the arithmetic mean roughness Sa is 0.020 μm or more and 0.051 μm or less, and the volume Vvc of the space in the core is 0.030 mL / m 2 Above 0.071mL / m 2 If the arithmetic mean roughness Sa of the transfer surface 40a and the volume Vvc of the space in the core are within the above numerical ranges, the generation of foreign matter can be further suppressed. The reason is not clear, but it is considered that this is because the gap into which foreign matter can enter can be limited.

[0057] As described above, by subjecting at least one surface of the copper foil substrate 10 to a concavo-convex forming treatment and a general roughening treatment for the purpose of improving wettability, the surface treated copper foil 30 involved in the present embodiment can be obtained. The surface roughness of the surface treated layer 20 of the obtained surface treated copper foil 30 needs to be as follows. That is, when the optical roughness of the surface 20a of the surface treated layer 20 is measured according to the method specified in ISO25178, the arithmetic mean roughness Sa needs to be greater than 0.04 μm and less than 0.30 μm. In order to further reduce the transmission loss, the arithmetic mean roughness Sa of the surface 20a of the surface treated layer 20 is preferably greater than 0.04 μm and less than 0.20 μm, and more preferably greater than 0.04 μm and less than 0.150 μm.

[0058] Next, the manufacturing method of the surface-treated copper foil 30 involved in the present embodiment is described. The surface-treated copper foil 30 involved in the present embodiment can be manufactured by performing the following steps (1) to (5) in the order described. When manufacturing the surface-treated copper foil 30, a concave-convex forming treatment is performed for the purpose of improving wettability. As the concave-convex forming treatment, two specific examples are cited for description, an example using a capsule plating treatment and an example using an etching concave-convex treatment.

[0059] [Example of using capsule plating]

[0060] (1) Manufacturing of copper foil substrate

[0061] In the manufacture of the surface-treated copper foil 30 according to the present embodiment, it is preferred to use an electrolytic copper foil or a rolled copper foil having a smooth and glossy surface without coarse irregularities as the copper foil substrate 10. Among them, from the viewpoint of productivity and cost, it is preferred to use an electrolytic copper foil, and it is particularly preferred to use an electrolytic copper foil having smooth surfaces on both sides, which is generally called "double-sided glossy foil".

[0062] In a conventional electrolytic copper foil, a smooth and glossy surface is a glossy surface (S surface). In a double-sided glossy foil, a smooth and glossy surface is both a glossy surface and a rough surface (M surface), and the smoother and glossier surface is the rougher surface. In the present embodiment, when any type of electrolytic copper foil is used, it is preferred that the smoother and glossier surface be subjected to a roughening treatment described later.

[0063] (2) Capsule plating treatment

[0064] The capsule plating treatment is performed to improve wettability and form fine irregularities on at least one surface of the copper foil substrate 10. Contents of the capsule plating treatment As described above, copper plating (capsule plating) can be performed locally on the surface of the copper foil substrate 10 by using a mesh cathode shielding plate.

[0065] Specific examples of the composition of the plating solution and the plating conditions are as follows. By appropriately setting the current density, only the openings of the mesh portion are subjected to smooth copper plating (capsule plating). As a result, fine concavities and convexities can be formed without changing the surface roughness of the entire surface of the copper foil.

[0066] <Composition of plating solution>

[0067] The concentration of copper sulfate pentahydrate is 50~65g / L in terms of copper (atoms).

[0068] Sulfuric acid concentration…80~170g / L

[0069] <Conditions of plating treatment>

[0070] Processing speed…5~18m / min

[0071] Current density…1~5A / dm 2

[0072] (3) Formation of roughening layer

[0073] As the roughening treatment, for example, it is preferable to perform the following two-stage plating treatment. It should be noted that, if necessary, the second-stage fixing plating treatment may not be performed.

[0074] The first stage of the roughening plating treatment is a treatment for forming roughening particles on the surface of the copper foil substrate 10 subjected to the capsule plating treatment. The first stage of the roughening plating treatment can be performed by plating treatment using a copper sulfate bath, for example. Specific examples of the composition of the plating solution and the plating conditions are as follows.

[0075] In order to prevent the roughened particles from falling off, i.e., "powder falling off", additives containing molybdenum (Mo), arsenic (As), antimony (Sb), bismuth (Bi), selenium (Se), tellurium (Te), tungsten (W), etc. can be added to the copper sulfate bath, and it is particularly preferred to add additives containing molybdenum.

[0076] <Composition of plating solution>

[0077] The concentration of copper sulfate pentahydrate is 5~15g / L in terms of copper (atoms).

[0078] Sulfuric acid concentration…120~250g / L

[0079] The concentration of ammonium molybdate is 500~1000mg / L in terms of molybdenum (atoms).

[0080] <Conditions of plating treatment>

[0081] Processing speed…8~22m / min

[0082] Current density 15~55A / dm 2

[0083] Processing time…0.5~5.0 seconds

[0084] Bath temperature…8~20℃

[0085] The second stage of fixed plating is a process of applying smooth cover plating to the copper foil substrate 10 subjected to the first stage of roughening plating. Thus, a roughening treatment layer 21 is formed on the surface of the copper foil substrate 10. The second stage of fixed plating can be performed by plating using a copper sulfate bath, for example. Specific examples of the composition of the plating solution and the plating conditions are as follows.

[0086] Generally, the fixed plating treatment is performed to prevent the roughened particles from falling off, that is, to fix the roughened particles. For example, in the manufacture of a copper-clad laminate, when a flexible substrate made of a hard resin such as a polyimide resin and the surface-treated copper foil 30 of the present embodiment are combined, the roughened surface can be fixedly plated to prevent the roughened particles from falling off.

[0087] <Composition of plating solution>

[0088] The concentration of copper sulfate pentahydrate is 50~65g / L in terms of copper (atoms).

[0089] Sulfuric acid concentration…90~160g / L

[0090] <Conditions of plating treatment>

[0091] Processing speed…5~20m / min

[0092] Current density 1~7A / dm 2

[0093] (4) Formation of anti-rust treatment layer

[0094] A silane coupling agent layer may be further formed directly or via an intermediate layer on the roughening treatment layer 21. Examples of the intermediate layer include a base layer containing nickel, a heat-resistant treatment layer containing zinc (Zn), and a rust-proof treatment layer 22 containing chromium (Cr). It should be noted that since the thickness of the intermediate layer and the silane coupling agent layer is very thin, the particle shape of the roughening particles on the roughening surface of the surface-treated copper foil 30 is not affected. The particle shape of the roughening particles on the roughening surface of the surface-treated copper foil 30 is substantially determined by the particle shape of the roughening particles on the surface of the roughening treatment layer 21 corresponding to the roughening surface.

[0095] For example, when copper (Cu) in the copper foil substrate 10 and the roughening treatment layer 21 diffuses toward the resin substrate 40 side and copper damage occurs, and the adhesion is reduced, the base layer is preferably formed between the roughening treatment layer 21 and the silane coupling agent layer. The base layer is preferably formed of at least one selected from nickel, nickel-phosphorus (P), nickel-zinc, and nickel-molybdenum.

[0096] The heat-resistant treatment layer is preferably formed when it is necessary to improve the heat resistance of the surface-treated copper foil 30. The heat-resistant treatment layer is preferably formed of zinc or an alloy containing zinc, for example. As the alloy containing zinc, zinc-tin (Sn) alloy, zinc-nickel alloy, zinc-cobalt alloy, zinc-copper alloy, zinc-molybdenum alloy, zinc-chromium alloy, zinc-vanadium (V) alloy can be listed.

[0097] The rust-proofing layer 22 is preferably formed when it is necessary to further improve the corrosion resistance. Examples of the rust-proofing layer 22 include a chromium layer formed by chromium plating and a chromate layer formed by chromate treatment.

[0098] When all three layers of the base layer, the heat-resistant treatment layer and the rust-proof treatment layer 22 are formed, they are preferably formed in this order on the roughening treatment layer 21. In addition, depending on the application and target characteristics, only one or two of the base layer, the heat-resistant treatment layer and the rust-proof treatment layer 22 may be formed.

[0099] (5) Formation of silane coupling agent layer

[0100] As a method for forming the silane coupling agent layer, for example, a method of applying a silane coupling agent solution directly or via an intermediate layer on the concavo-convex surface of the roughening treatment layer 21 of the surface-treated copper foil 30, followed by air drying (natural drying) or heat drying can be cited. If water in the applied coupling agent solution evaporates, a silane coupling agent layer is formed. If heat drying is performed at a temperature of 50 to 180° C., the reaction between the silane coupling agent and the copper foil can be promoted, so it is preferred.

[0101] The silane coupling agent layer preferably contains at least one of an epoxy silane coupling agent, an amino silane coupling agent, a vinyl silane coupling agent, a methacrylic silane coupling agent, an acrylic silane coupling agent, an azole silane coupling agent, a styryl silane coupling agent, a ureide silane coupling agent, a mercapto silane coupling agent, a sulfide silane coupling agent, and an isocyanate silane coupling agent.

[0102] [Example of using etching roughness treatment]

[0103] (1) Manufacturing of copper foil substrate

[0104] This is the same as the case where the capsule plating process is used.

[0105] (2) Formation of roughening layer

[0106] This is the same as the case where the capsule plating process is used.

[0107] (3) Etching concave-convex treatment

[0108] The etching process is performed for the purpose of improving wettability, and a fine concavo-convex shape is formed on the surface of the copper foil substrate 10. The content of the etching process is as described above, and the process conditions are further described in detail. An electrolytic bath containing nickel sulfate and a nickel concentration of 30 to 150 g / L is used at a current density of 1.0 to 4.0 A / dm 2 , electrolysis is performed under the condition of a power-on time of 0.5 to 2.0 seconds, and then etching is performed by immersing in an etching solution for a short time, thereby forming a fine concave-convex shape on the surface of the copper foil substrate 10 that does not affect the degree of transmission loss.

[0109] By this etching unevenness treatment, unevenness is formed on the surface of the roughened particles formed by the roughening treatment. As other etching methods, immersion treatment in a solution containing an inorganic acid such as hydrochloric acid, sulfuric acid, phosphoric acid, etc. can be cited. By immersing the copper foil substrate 10 in an inorganic acid aqueous solution of a specified concentration for several seconds to tens of seconds, fine unevenness is formed on the surface of the roughened particles. For example, when hydrochloric acid is used, fine unevenness is formed on the surface of the roughened particles by immersing in hydrochloric acid with a concentration of 5 to 20 volume % for more than 2 seconds.

[0110] In addition, as other etching methods, in addition to the above-mentioned immersion treatment in a solution containing an inorganic acid, immersion treatment in a solution containing an organic acid such as acetic acid or formic acid, immersion treatment in a solution containing ferric chloride or cupric chloride, and electrolytic etching treatment using anodization can also be used. These methods can be combined with two or more.

[0111] (4) Formation of anti-rust treatment layer

[0112] This is the same as the case where the capsule plating process is used.

[0113] (5) Formation of silane coupling agent layer

[0114] This is the same as the case where the capsule plating process is used.

[0115] (B) Regarding the wettability of the transfer surface

[0116] Next, the evaluation method of the wettability of the transfer surface 40a is described. When manufacturing the copper-clad laminate 50 and the printed wiring board 60, the wettability of the transfer surface 40a of the resin substrate 40 bonded to the surface-treated copper foil 30 can be evaluated by the contact angle of distilled water measured by the sessile drop method specified in JIS R3257:1999.

[0117] The contact angle θ0 of distilled water was measured by the above-mentioned sessile drop method for the surface of the resin substrate 40 before being bonded to the surface-treated copper foil 30. The surface on which the contact angle θ0 of distilled water of the non-transferred surface before the copper foil is bonded is measured is the non-transferred surface to which the surface shape of the surface-treated copper foil 30 is not transferred.

[0118] In addition, after the resin substrate 40 is laminated on the surface treated layer 20 of the surface treated copper foil 30, the surface treated copper foil 30 is removed by etching, and the contact angle θ1 of distilled water is measured according to the above-mentioned sessile drop method for the surface of the remaining resin substrate 40 on which the surface treated copper foil 30 is laminated. The surface on which the contact angle θ1 of distilled water of the transferred surface after copper foil etching is measured is the transferred surface 40a to which the shape of the surface of the laminated surface treated copper foil 30 is transferred.

[0119] Then, the wettability of the transfer surface 40a of the resin substrate 40 is evaluated by the difference θ0-θ1 between the contact angles θ0 and θ1. If the difference θ0-θ1 between the contact angles θ0 and θ1 is 5° or more and 35° or less, the wettability of the transfer surface 40a is good.

[0120] The resin component used when measuring the contact angle θ0 and the contact angle θ1 may be the same type of component as the resin substrate 40 used when manufacturing the copper-clad laminate 50 and the printed wiring board 60 as described above, or a different component may be used to measure the contact angle θ0 and the contact angle θ1. That is, a component having a different type, shape, size, etc. of resin from the resin substrate 40 used when manufacturing the copper-clad laminate 50 and the printed wiring board 60 may be used as the resin component.

[0121] The type of resin forming the resin component used in measuring the contact angle θ0 and the contact angle θ1 may be a curable resin such as a thermosetting resin, or a thermoplastic resin. In the case of a curable resin, the contact angle θ0 and the contact angle θ1 are measured after the resin component is cured. That is, in the case of the contact angle θ1, the resin component before curing is attached to the surface treatment layer 20 of the surface treatment copper foil 30, and after the resin component is cured, the surface treatment copper foil 30 is removed by etching. Then, for the transfer surface on the surface of the resin component, the contact angle θ1 of distilled water is measured according to the above-mentioned sessile drop method.

[0122] (C) About copper-clad laminates

[0123] The structure of the copper-clad laminate 50 according to the present embodiment is not particularly limited, and includes a surface-treated copper foil 30 and a resin substrate 40. The resin substrate 40 is bonded to the surface-treated layer 20 of the surface-treated copper foil 30. The copper-clad laminate 50 can be used to manufacture a printed wiring board 60, for example.

[0124] Examples of the resin forming the resin substrate 40 include epoxy resin, polyphenylene ether, phenolic resin, bis(phenoxyphenoxy)benzene, polyimide, liquid crystal polymer, and fluororesin (eg, polytetrafluoroethylene).

[0125] (D) About printed wiring boards

[0126] The structure of the printed wiring board 60 according to the present embodiment is not particularly limited, and includes the copper-clad laminate 50 according to the present embodiment. For example, after etching the surface-treated copper foil 30 of the copper-clad laminate 50 to form the circuit 31, another resin substrate 41 is attached to cover the circuit 31, and the printed wiring board 60 can be obtained (see Figure 3 (d)). The resin base material 41 bonded to cover the circuit 31 may be of the same type as the resin base material 40 of the copper-clad laminate 50 or may be of a different type.

[0127] [Example]

[0128] The present invention will be described in more detail below by showing examples and comparative examples. First, the surface-treated copper foil of comparative example 7 is manufactured by the manufacturing method described in patent document 1. Similarly, the surface-treated copper foil of comparative example 8 is manufactured by the manufacturing method described in patent document 2, the surface-treated copper foil of comparative example 9 is manufactured by the manufacturing method described in patent document 3, the surface-treated copper foil of comparative example 10 is manufactured by the manufacturing method described in patent document 4, and the surface-treated copper foil of comparative example 11 is manufactured by the manufacturing method described in patent document 5.

[0129] Next, the surface-treated copper foils of Examples 1 to 23 and Comparative Examples 1 to 6 and 12 to 14 were produced according to the procedure described below.

[0130] (1) Copper foil substrate

[0131] As the raw material, i.e., copper foil substrate, for manufacturing the surface-treated copper foil of Examples 1 to 23 and Comparative Examples 1 to 6 and 12 to 14, a roll-shaped electrolytic copper foil (glossy foil on both sides) with a thickness of 18 μm was prepared. The cathode used in the preparation of the electrolytic copper foil was a titanium rotating drum whose surface roughness was adjusted by polishing with #1000 to #2000, and the anode was a dimensional stability anode DSA (registered trademark). The composition of the electrolyte and the electrolysis conditions are as follows.

[0132] <Electrolyte composition>

[0133] Copper: 75g / L

[0134] Sulfuric acid: 65g / L

[0135] Chlorine: 20mg / L

[0136] Sodium 3-mercapto-1-propane sulfonate: 2 mg / L

[0137] Hydroxyethyl cellulose: 10 mg / L

[0138] Low molecular weight glue (molecular weight 3000): 50mg / L

[0139] <Electrolysis conditions>

[0140] Bath temperature: 50°C

[0141] Current density: 45A / dm 2

[0142] Next, the copper foil substrate prepared as described above was subjected to the above-mentioned general roughening treatment and the concave-convex forming treatment for the purpose of improving wettability. For Examples 1 to 8, 17 to 23 and Comparative Examples 2, 3, and 6, after the copper foil substrate was subjected to the concave-convex forming treatment for the purpose of improving wettability, i.e., capsule plating treatment, a general roughening treatment was performed. For Examples 9 to 16 and Comparative Examples 4 and 5, after the copper foil substrate was subjected to the general roughening treatment, a concave-convex forming treatment for the purpose of improving wettability, i.e., etching concave-convex treatment, was performed. The general roughening treatment, capsule plating treatment, and etching concave-convex treatment are described below.

[0143] (2) General roughening treatment

[0144] The rough surface of the copper foil substrate was subjected to a roughening treatment in a roll-to-roll manner. The roughening treatment was a two-stage electroplating treatment. The composition of the plating solution and the plating conditions of the first-stage electroplating treatment were as follows. In addition, the composition of the plating solution and the plating conditions of the two-stage electroplating treatment (fixed plating treatment) were as follows. As shown in Tables 1 and 2, by changing the current density and the power-on time of the first-stage electroplating treatment, roughened particles with different heights and shapes were formed on the surface of the copper foil.

[0145] <Composition of plating solution in the first stage of electroplating treatment>

[0146] The concentration of copper sulfate pentahydrate is calculated as 10 g / L in terms of copper (atoms).

[0147] Sulfuric acid concentration…150g / L

[0148] The concentration of ammonium molybdate is 600 mg / L in terms of molybdenum (atoms).

[0149] <Conditions of the first-stage plating treatment>

[0150] Processing speed…15m / min

[0151] Current density…15~55A / dm 2

[0152] Bath temperature…15℃

[0153] Power-on time…4~6 seconds

[0154] <Composition of plating solution in the second-stage electroplating treatment>

[0155] The concentration of copper sulfate pentahydrate is 55 g / L in terms of copper (atoms).

[0156] Sulfuric acid concentration…120g / L

[0157] <Conditions of the second-stage plating treatment>

[0158] Processing speed…15m / min

[0159] Current density…2A / dm 2

[0160] Power-on time…3 seconds

[0161] (3) Capsule plating treatment

[0162] The copper foil substrate was subjected to capsule plating as a concavo-convex forming treatment by a roll-to-roll method. 2 A grid-shaped cathode shielding plate with an opening ratio of 5 to 15% was placed near the copper foil substrate in the electrolytic bath, and electroplating was performed under the following plating conditions using the following plating solution. As shown in Tables 1 and 2, copper foil substrates with different surface irregularities were prepared by changing the opening ratio of the cathode shielding plate, the electroplating current density, and the energization time.

[0163] <Composition of plating solution>

[0164] The concentration of copper sulfate pentahydrate is 60 g / L in terms of copper (atoms).

[0165] Sulfuric acid concentration…150g / L

[0166] <Conditions of plating treatment>

[0167] Processing speed…18m / min

[0168] (4) Etching concave-convex treatment

[0169] The roughened surface of the copper foil substrate subjected to the roughening treatment was subjected to an etching roughening treatment as a roughening treatment. The etching roughening treatment is a treatment in which nickel is electrolyzed and then immersed in an etching solution for etching. The composition of the electrolyte used for the electrolysis, the electrolysis conditions, and the etching conditions are as follows. As shown in Tables 1 and 2, copper foil substrates with different surface roughnesses were prepared by changing the current density and power-on time of the electrolysis and the etching treatment time.

[0170] <Electrolyte composition>

[0171] Nickel concentration…60g / L

[0172] Concentration of boric acid (H3BO3)…15g / L

[0173] Bath temperature…20℃

[0174] pH…3.5

[0175] <Electrolysis Conditions>

[0176] Current density…1~2.5A / dm 2

[0177] Power-on time…1~3 seconds

[0178] <Etching conditions>

[0179] Etching solution: 10% by volume hydrochloric acid

[0180] Bath temperature…30℃

[0181] Processing time…0.5~2 seconds

[0182] (5) Anti-rust treatment

[0183] Next, the surface of the copper foil substrate subjected to the roughening treatment and the concavo-convex forming treatment as described above is subjected to rust-proof treatment to form a rust-proof treatment layer. The rust-proof treatment is a process of nickel plating, zinc plating, and chromium plating in this order. The conditions of nickel plating, zinc plating, and chromium plating are shown.

[0184] <Composition of nickel plating solution>

[0185] Nickel concentration…45g / L

[0186] Boric acid concentration...20g / L

[0187] Bath temperature…20℃

[0188] pH…3.5

[0189] <Nickel plating conditions>

[0190] Current density: 0.4A / dm 2

[0191] Processing time: 8 seconds

[0192] <Composition of zinc plating solution>

[0193] Zinc concentration…2.5g / L

[0194] The concentration of sodium hydroxide (NaOH) is 25 g / L.

[0195] Bath temperature…20℃

[0196] <Galvanizing conditions>

[0197] Current density: 0.7A / dm 2

[0198] Processing time: 4 seconds

[0199] <Composition of chrome plating solution>

[0200] Chromium concentration…8g / L

[0201] Bath temperature…30℃

[0202] pH…2.4

[0203] <Chrome plating conditions>

[0204] Current density: 5A / dm 2

[0205] Processing time: 4 seconds

[0206] (6) Silane coupling agent treatment

[0207] Finally, a silane coupling agent treatment was performed to form a silane coupling agent layer on the outermost chrome plating layer of the rust-proofing layer. The silane coupling agent layer was formed by applying a 0.2 mass % 3-aminopropyltrimethoxysilane aqueous solution and drying it at 100°C.

[0208] [Table 1]

[0209]

[0210] [Table 2]

[0211]

[0212] The surface treated copper foils of Examples 1 to 23 and Comparative Examples 1 to 14 obtained as described above were subjected to various evaluations. The evaluation items and evaluation methods are described below. The evaluation results are shown in Tables 1 and 2.

[0213] <Contact angle of distilled water>

[0214] A resin component was laminated on the surface treatment layer (i.e., silane coupling agent layer) of the surface treated copper foil to prepare a copper clad laminate. As the resin component, the following components were used. That is, for Examples 1 to 20 and Comparative Examples 1 to 11, as the resin component, a component obtained by laminating two low dielectric polyphenylene ether resin substrate films (super-low transmission loss-high heat-resistant multilayer substrate material MEGTRON7N manufactured by Panasonic Corporation, thickness 60 μm) was used.

[0215] In addition, ThunderClad3+ manufactured by Taiwan Union Corporation was used for Example 21 and Comparative Example 12, ESPANEX (registered trademark) manufactured by Nippon Steel Chemicals & Materials Co., Ltd. was used for Example 22 and Comparative Example 13, and Vecstar (registered trademark) liquid crystal polymer film manufactured by Kuraray Co., Ltd. was used for Example 23 and Comparative Example 14.

[0216] In addition, the bonding of the surface-treated copper foil and the resin member was performed under the conditions in accordance with the process guide of each resin.

[0217] The copper-clad laminate was etched using a mixture of cupric chloride and hydrochloric acid as an etching solution to remove all the surface-treated copper foil. After the remaining resin component was thoroughly washed with water, the contact angle θ1 of distilled water was measured for the surface of the resin component to which the surface-treated copper foil was attached (transferred surface) according to the sessile drop method specified in JIS R3257:1999.

[0218] On the other hand, a resin component of the same type as the resin component bonded to the surface treated layer of the surface treated copper foil was prepared separately, and the surface treated copper foil was not bonded to the other resin component. The same operation as the above-mentioned step in the case of preparing the copper clad laminate was performed, and the contact angle θ0 of distilled water was measured on the surface (non-transferred surface) by the above-mentioned sessile drop method. Then, the difference θ0-θ1 between the contact angle θ0 and the contact angle θ1 was calculated.

[0219] <Arithmetic mean roughness Sa of surface-treated copper foil, arithmetic mean roughness Sa of resin member, and volume Vvc of space in core>

[0220] Using confocal laser microscopes VK-X1050 and VK-X1000 manufactured by KEYENCE Co., Ltd., the arithmetic mean roughness Sa of the surface of the surface treated layer (i.e., the silane coupling agent layer) of the surface treated copper foil, the arithmetic mean roughness Sa of the transfer surface of the resin component at the distilled water contact angle θ1 of the transfer surface after etching the copper foil, and the volume Vvc of the space in the core were measured in accordance with ISO25178.

[0221] It should be noted that the magnification of the objective lens of the confocal laser microscope was 100 times, the scanning mode was laser confocal, the measurement size was 2048×1536, the measurement quality was High Precision, and the pitch was 0.08 μm.

[0222] The calculation of the arithmetic mean roughness Sa and the volume Vvc of the space in the core portion is performed under the filtering process and calculation conditions shown below.

[0223] Image processing: smoothing, 3×3, median

[0224] S filter: No

[0225] F-operation: plane tilt correction

[0226] L filter: 0.025μm

[0227] Calculation area: 100μm×100μm

[0228] Load area ratio in load curve: 10% and 90%

[0229] <Circuit processability>

[0230] On the surface treated copper foil of the same copper clad laminate produced to measure the distilled water contact angle θ1 of the transferred surface after copper foil etching, a resist pattern with L&S of 50 / 50 μm was formed by a subtractive method. Then, the surface treated copper foil was etched to form a circuit with a wiring pattern. A dry resist film was used as the resist, and a mixed solution containing cupric chloride and hydrochloric acid was used as the etching solution.

[0231] Then, the etching factor (Ef) of the obtained circuit was measured. The etching factor is a value represented by the formula Ef=2H / EB-T when the thickness of the copper foil is H, the bottom width of the formed circuit is B, and the top width of the formed circuit is T.

[0232] The copper-clad laminate on which the circuit was formed was cut to reveal a cross section perpendicular to the surface of the resin component, and the cross section of the circuit was observed using a scanning electron microscope. Figure 2 Angle X and angle Y on the cross section shown. Angle X is the angle formed by the straight line connecting the top end 31a and the bottom end 31b of the circuit 31 and the surface of the resin component. Angle Y is the angle formed by the tangent line of the bottom end 31b of the circuit 31 and the surface of the resin component.

[0233] The tangent line of the bottom end 31b of the circuit 31 is defined in more detail. A straight line parallel to the surface of the resin component is drawn at a height of 1.5 μm from the surface of the bottom side of the resin component, and a straight line connecting the intersection 31c of the straight line with the side surface of the circuit 31 and the bottom end 31b is defined as "the tangent line of the bottom end 31b of the circuit 31", and the angle formed by the tangent line and the surface of the resin component is defined as angle Y.

[0234] Observe 5 random cross sections of a circuit and measure angle X and angle Y respectively. Then, the average value of the 5 measured values ​​is calculated for angle X and angle Y. The results are shown in Tables 1 and 2. In Tables 1 and 2, the value where Ef is greater than 2.5 and angle Y is greater than angle X is represented as "A", the value where Ef is greater than 2.0 and less than 2.5 and angle Y is greater than angle X is represented as "B", and the other values ​​are represented as "C". It should be noted that Figure 2 (a) is a diagram showing an example of a circuit 31 in which the angle Y is smaller than the angle X. Figure 2 (b) is a diagram showing an example of the circuit 31 in which the angle Y is larger than the angle X.

[0235] <Transmission loss>

[0236] A printed wiring board with a strip line was prepared using the same copper-clad laminate as that prepared for measuring the distilled water contact angle θ1 of the transferred surface after copper foil etching, and the transmission characteristics were evaluated. The strip line formed on the printed wiring board had a circuit width of 140 μm and a circuit length of 76 mm.

[0237] A network analyzer N5291A manufactured by Keysight Technologies was used to transmit a high-frequency signal to the circuit formed on the printed wiring board, and the transmission loss was measured. The characteristic impedance is 50Ω. The measured value of the transmission loss means that the smaller the absolute value, the less the transmission loss (that is, the high-frequency signal can be transmitted well). The results are shown in Tables 1 and 2. In Tables 1 and 2, the absolute value of the transmission loss at 40GHz is less than 3.0dB / 76mm, and is represented as "A", and the absolute value of the transmission loss at 40GHz is less than 3.0dB / 76mm. It is represented as "B" when it is greater than 3.0dB / 76mm and less than 3.6dB / 76mm, and it is represented as "C" when it is greater than 3.6dB / 76mm.

[0238] <Generation of foreign matter>

[0239] A mixture of cupric chloride and hydrochloric acid was used as an etching solution to etch the copper-clad laminate that was produced to measure the distilled water contact angle θ1 of the transfer surface after copper foil etching, and the surface-treated copper foil was completely removed. After the remaining resin component was fully washed with water, a resin component of the same type as the material used in the production of the above-mentioned copper-clad laminate and a surface-treated copper foil were overlapped and laminated in sequence on the surface (transfer surface) of the resin component on which the surface-treated copper foil was laminated, and then etching was performed according to the same steps as above to completely remove the surface-treated copper foil. Thus, a resin sample formed by laminating two resin components was obtained.

[0240] Next, the obtained resin sample is cut into a square shape with a side of 5 cm. Then, the cut resin sample is magnified 35 times by a microscope for observation, and the number of black spots with a diameter of more than 1 mm is measured. The black spots are caused by foreign matter generated between the two bonded resin components. The observation under the microscope is carried out in the form of observing the transfer surface of the resin component that initially constitutes the copper-clad laminate from the side of the resin component bonded thereafter. The results are shown in Tables 1 and 2. In Tables 1 and 2, the case where the number of black spots per cut resin sample is 2 or less is represented as "A", the case where 3 or more and 5 or less is represented as "B", and the case where more than 5 are represented as "C".

[0241] As can be seen from Tables 1 and 2, although the surface treated copper foils of Examples 1 to 23 have the arithmetic mean roughness Sa of the surface of the surface treated layer controlled to be between 0.04 μm and 0.30 μm, the difference θ0-θ1 between the contact angle θ0 and the contact angle θ1 representing the wettability of the transfer surface of the resin substrate is well controlled, so the circuit processability is excellent and transmission loss and foreign matter are not easily generated.

[0242] Among them, the surface treated copper foils of Examples 1 to 4, 10 to 14, 17, 18, and 21 to 23 have better circuit processability and are less likely to generate foreign matter because the arithmetic mean roughness Sa of the transfer surface of the resin substrate and the volume Vvc of the space in the core are well controlled.

[0243] On the other hand, the surface-treated copper foils of Comparative Examples 1 to 14 had low wettability on the transfer surface of the resin substrate, and therefore were insufficient in any of circuit processability, transmission loss, and generation of foreign matter.

[0244] Description of Reference Numerals

[0245] 10: Copper foil substrate; 20: Surface treatment layer; 20a: Surface of surface treatment layer; 21: Roughening treatment layer; 22: Anti-rust treatment layer; 30: Surface treated copper foil; 31: Circuit; 31a: Top end; 31b: Bottom end; 40: Resin substrate (resin component); 40a: Transfer surface; 41: Resin substrate; 50: Copper clad laminate; 60: Printed wiring board; 100: Foreign matter.

Claims

1. A surface-treated copper foil comprising a copper foil substrate and a surface-treated layer formed on at least one surface of the copper foil substrate, The surface treatment layer is composed of one or both of a roughening treatment layer and an anti-rust treatment layer. When the optical roughness of the surface of the surface treatment layer is measured according to the method specified in ISO 25178, the arithmetic mean roughness Sa is 0.04 μm or more and 0.30 μm or less, After a resin component is laminated on the surface treated layer of the surface treated copper foil, the surface treated copper foil is removed by etching, and the contact angle θ1 of distilled water is measured for the surface of the remaining resin component on which the surface treated copper foil has been laminated, i.e., the transfer surface, according to the sessile drop method specified in JIS R3257:1999, and the contact angle θ0 of distilled water is measured for the surface of the resin component before being laminated on the surface treated copper foil, i.e., the non-transfer surface, according to the sessile drop method. In this case, the difference θ0-θ1 between the contact angle θ0 and the contact angle θ1 is greater than 5° and less than 35°.

2. The surface-treated copper foil according to claim 1, wherein When the optical roughness of the transfer surface is measured according to the method specified in ISO 25178, the arithmetic mean roughness Sa is 0.020 μm or more and 0.070 μm or less, and the volume Vvc of the space in the core is 0.030 mL / m 2 Above and 0.110mL / m 2 the following.

3. The surface-treated copper foil according to claim 1, wherein When the optical roughness of the transfer surface is measured according to the method specified in ISO 25178, the arithmetic mean roughness Sa is 0.020 μm or more and 0.051 μm or less, and the volume Vvc of the space in the core is 0.030 mL / m 2 Above 0.071mL / m 2 the following.

4. A copper-clad laminate, The surface-treated copper foil according to any one of claims 1 to 3 and a resin substrate bonded to the surface-treated layer of the surface-treated copper foil.

5. A printed wiring board, A copper-clad laminate according to claim 4.