Method for producing cellulose-based substrate coated with barrier layer, laminated packaging material and packaging container comprising cellulose-based substrate produced thereby
By using high-linear speed conveying paper substrates with high-speed production conditions and combining roller coating and vapor deposition technology, a paper or cellulose-based substrate with high-efficiency oxygen barrier and recyclability is produced, solving the problem of The high-speed production and recyclability problems that are difficult to achieve in the prior art are suitable for packaging oxygen-sensitive products.
Patent Information
- Application Number
- CN202380028107.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-14
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to efficiently and robustly manufacture paper or cellulose-based substrates with good gas barrier properties and recyclability on an industrial scale for packaging oxygen-sensitive products, especially under high-speed production conditions. .
The paper-based or cellulose-based substrate is transported using a linear velocity of 300m/min or higher, and the aqueous solution of gas-barrier polymer is applied by roller coating method, combined with the physical vapor-deposited metal and/or metal oxide nano-thick layers to form a uniform And the barrier coating with few defects ensures oxygen barrier properties and recyclability.
It achieves efficient oxygen barrier properties and improved recyclability under high-speed production conditions, and is suitable for liquid, semi-liquid or viscous food packaging that is stored for a long time, reducing material costs and complexity.
Smart Images

Figure CN118891413A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an industrial process for producing a paper or cellulose-based substrate coated with a barrier layer for packaging oxygen-sensitive products, such as foods. The present invention also relates to a laminated packaging material comprising the paper or cellulose-based substrate coated with a barrier layer produced thereby, which is used for packaging oxygen-sensitive products, such as foods, such as liquid or semi-liquid foods, and to a packaging container comprising the laminated packaging material. Background Art
[0002] Disposable type packaging containers for single use of liquid foods are usually made of packaging laminates based on paperboard or cardboard. One such common packaging container is Tetra Brik The packaging containers are sold under the trademark of ANTI-FORMAT and are mainly used for aseptic packaging of liquid foodstuffs (e.g. milk, juice, etc.) that are sold for long-term ambient storage. The packaging material in such known packaging containers is usually a laminate material comprising a main body or core layer of paper, paperboard or other cellulose-based material and an outer liquid-tight layer of thermoplastic. In order to make the packaging container airtight, in particular oxygen-tight, for example for the purpose of aseptic packaging and packaging milk or juice, the laminate material in these packaging containers usually comprises at least one additional layer, most usually comprising an aluminum foil.
[0003] On the inside of the laminate, i.e. on the side intended to face the filled food content of the container produced from the laminate, there is an innermost layer applied to the aluminum foil, which innermost inner layer may consist of one or several partial layers, comprising a heat-sealable thermoplastic polymer, such as an adhesive polymer and / or a polyolefin. Likewise on the outside of the bulk layer, there is an outermost heat-sealable polymer layer.
[0004] Packaging containers are usually produced by modern high-speed packaging machines, which form packaging from packaging material coils or packaging material preforms, and fill and seal them. Therefore, packaging containers can be produced in the following manner: by welding the innermost and outermost heat-sealable thermoplastic polymer layers together, the two longitudinal edges of the coil are combined with each other at the overlap joint, and the laminated packaging material coil is transformed into a tube. The tube is filled with the expected liquid food, and then the tube is divided into each individual package by each repeated transversal seal of the tube, which is below the horizontal plane of the contents in the tube and at a predetermined distance from each other. The packaging is separated from the tube by the incision along the transversal seal, and the desired geometric configuration is obtained by folding and forming along the fold line prepared in the packaging material, and the desired geometric configuration is generally a parallelepiped. Before or after the container is filled, formed and sealed, each package can be equipped with an opening device, such as a screw plug.
[0005] The main advantage of this continuous tube forming, filling and sealing packaging process concept is that the web can be sterilized continuously before tube forming, thereby providing the possibility of an aseptic packaging process, i.e. a process in which the liquid contents to be filled as well as the packaging material itself are germ-reduced and the filled packaging containers are produced under clean conditions so that the filled packages can be stored for long periods of time even at ambient temperature without the risk of microbial growth in the filled product. As mentioned above, Tetra Another important advantage of the type packaging method is the possibility of continuous high-speed packaging, which has a considerable impact on cost efficiency.
[0006] Packaging containers for sensitive liquid foods (e.g. milk or juice) can also be made from sheet blanks or preformed blanks of the laminated packaging material of the present invention. The packaging is produced using a tubular blank of the packaging laminate folded into a plane by first erecting the blank to form an open tubular container capsule, one open end of which is closed by folding and heat-sealing integral end panels. The container capsule so closed is filled with the relevant food (e.g. juice) through its open end, which is then closed by further folding and heat-sealing the corresponding integral end panels. An example of a packaging container made from sheet and tubular blanks is the traditional so-called gable top package. There are also packages of this type with a molded top and / or a screw cap made of plastic.
[0007] The aluminum foil layer in the packaging laminate provides superior gas barrier properties to most other gas barrier materials. Traditional aluminum foil based packaging laminates for aseptic packaging of liquid foods also have inherent barrier properties to water vapor, light, aroma, taste and acidic substances and remain the most cost effective packaging material currently available in the market at its performance level. In addition, aluminum foil can be heat sealed and heated by induction in the aluminum foil.
[0008] Any other material comparable to aluminum foil-based materials must be cost-effective in terms of raw materials, have comparable food preservation properties, and have comparable low complexity in converting the material into a finished packaging laminate.
[0009] In the efforts to develop non-aluminum foil materials for liquid food carton packaging, there is also a motivation to develop prefabricated films or sheets with high barrier functions and multiple barrier functions, which can replace the aluminum foil barrier material in traditional laminated packaging materials, or be combined with other barrier layers in the laminated materials, and adapt them to conventional lamination and manufacturing processes.
[0010] A preferred type of such an alternative, more environmentally sustainable barrier material is a barrier coated paper substrate made by aqueous dispersion coating or vapor deposition coating on a thin paper carrier substrate. Various aqueous dispersion coating processes and vapor deposition coating processes and material formulations for achieving such coatings exist, but there is a need for a cost effective "non-foil" type (i.e. non-aluminum foil) barrier material having improved properties in terms of barrier properties, particularly against gases such as oxygen, for use in packaging laminates for liquid food packaging.
[0011] An earlier patent publication WO2011 / 003565A1 discloses a non-aluminium foil packaging material comprising a pre-coated and metallized kraft paper substrate for induction heat sealing purposes. It recommends a fairly thick coating and the inclusion of additional nanoclay particles in the pre-coating, and in order to obtain good gas barrier properties, a further barrier coating should also be applied in the packaging laminate, for example on the back side of the paper substrate or on the main paperboard layer.
[0012] Earlier patent publication WO2017 / 089508A1 discloses how to obtain further improved barrier properties from metallized paper in similar packaging laminates by selecting a paper substrate that provides the best performance. This metallized paper substrate not only provides improved barrier properties, but also shows that the metallized layer has better stability in induction heat sealing.
[0013] However, there is still a need for a robust and industrially viable coating process, operating at high coating line speeds, to provide optimal and reliable oxygen barrier properties over a selected optimal range of paper and cellulose based substrates. In general, there is also a need to improve the recyclability and sustainability of the materials used, in order to reduce the amount of materials used and the number of different types of materials. Summary of the invention
[0014] It is therefore a general object of the present invention to provide an industrially viable process for the high-speed, robust manufacture of paper or cellulose-based substrates coated with a barrier layer, suitable as gas barrier materials in the packaging of oxygen-sensitive products (e.g. foods, such as in particular liquid or semi-liquid or wet foods), and for the manufacture of future sustainable, non-aluminium foil-based ("non-foil") laminated packaging materials for packaging oxygen-sensitive products.
[0015] Another general object of the present invention is to provide an industrially viable process for the high-speed, robust manufacture of barrier-coated paper or cellulose-based substrates having good gas barrier properties as well as improved recyclability and sustainability characteristics (i.e., meeting future demands for sustainable packaging materials for packaging oxygen-sensitive products).
[0016] A more specific object is to provide an industrially feasible and robust method for manufacturing paper or cellulose based substrates coated with a barrier layer suitable for non-foil laminated packaging materials and packaging containers for liquid, semi-liquid or viscous foods for long term sterile storage under ambient conditions.
[0017] Another object is to provide a paper or paperboard based laminated packaging material which is cost effective and reliable relative to aluminum foil barrier materials, which has good gas barrier properties and optionally water vapor barrier properties, is easily recyclable and environmentally sustainable, for wrapping or packaging oxygen sensitive products (such as food).
[0018] Another object of the present invention is to provide a cost-effective, non-foil, paper or paperboard based, heat-sealable packaging laminate having reliable gas and water vapor barrier properties for use in making aseptic packaging containers for long-term storage of liquid, semi-liquid or viscous foods under ambient conditions and while maintaining nutritional quality.
[0019] Thus, according to the present invention, these objects are achieved by a method for producing a paper or cellulose based substrate coated with a barrier layer, a laminated packaging material and a packaging container as defined in the appended claims. Summary of the invention
[0020] According to a first aspect of the present invention, there is provided a method for manufacturing a barrier coated cellulose-based substrate for packaging oxygen sensitive products, the method comprising the steps of: conveying a web of a paper-based or cellulose-based substrate at a line speed of 300 m / min or more,
[0021] The web of cellulose-based substrate is selected to have a web weight of 30 to 70 g / m2 measured according to ISO 536:2012. 2 The grammage and the thickness of the fabric are 800 kg / m2 as measured according to ISO 534:2011. 3 Up to 1400kg / m 3 The surface of the top side of the paper-based or cellulose-based substrate exhibits a Bendtsen roughness value of less than 130 ml / min measured according to ISO 8791:4 and a roughness of less than 30 g / m2 measured according to ISO 535. 2 or lower Cobb 60,
[0022] Providing an aqueous solution of a gas barrier polymer selected from the group consisting of vinyl alcohol polymers, PVOH, ethylene vinyl alcohol copolymers, EVOH, and modified PVOH and EVOH polymers of this type, the aqueous solution having a solid content of 5 to 15 wt. % and a viscosity of 10 to 120 mPa*s, applying the aqueous solution of the gas barrier polymer to the surface of the top side of the web of the paper-based or cellulose-based substrate by a roll coating method to provide a dry weight of 0.5 to 2 g / m 2 The invention relates to a method of coating the web substrate with a uniform coating of at least one coating layer, drying the aqueous gas barrier polymer coating applied in the previous step while always maintaining the surface temperature of the web substrate below 60°C to 95°C, repeating the steps of applying the aqueous solution of the gas barrier polymer and subsequently drying the applied aqueous gas barrier polymer coating at least once, and optionally further coating the thus obtained, coated and dried web substrate with a nano-thick barrier deposited coating of metal and / or metal oxide by physical vapor deposition, thereby obtaining a paper-based or cellulose-based substrate coated with a barrier layer having minimal defects in the gas barrier coating and in the optional metal and / or metal oxide deposited coating.
[0023] In one embodiment, the roll coating process is a rotogravure coating process, such as a reverse rotogravure coating process.
[0024] The aqueous solution of PVOH or EVOH may have a solid content of 7 to 13 wt %, such as 9 to 13 wt %, such as 10 to 12.5 wt %.
[0025] The steps of applying an aqueous solution of a gas barrier polymer and then drying the applied aqueous gas barrier polymer coating may be repeated once so that the amount of the aqueous gas barrier polymer coating applied per coating step is 0.5 to 1 g / m 2 (dry weight). It has been found that this works best in high speed processing, i.e. applying a thin, uniform coating with few skips and defects to achieve adequate oxygen barrier properties, and being able to dry the coating carefully, but quickly enough to accommodate the high speed of the coating line, including avoiding the formation of defects in the coating during the drying step. At the same time, for the quality of paper substrate selected, a wet, thinly applied coating of the gas barrier polymer solution can even out the roughness of the substrate surface, while still maintaining the adhesion of the coating so that it is not disrupted or partially absorbed by the substrate surface before drying into a coherent, uniform barrier coating.
[0026] In a preferred embodiment, in each drying step, the surface temperature of the web substrate is always maintained below 85°C, such as below 80°C.
[0027] The optional vapor deposited coating may be an aluminum metallization coating or an aluminum oxide coating or a mixed coating of aluminum and aluminum oxide.
[0028] According to a second aspect of the present invention, there is provided a laminated packaging material comprising a cellulose-based substrate coated with a barrier layer produced by the method of the first aspect, and further comprising a first outermost protective material layer and a second innermost liquid-tight heat-sealable material layer, wherein the laminated packaging material exhibits an oxygen transmission rate value of 0.5 cm2 at 50% RH, 24 h, 0.2 atm oxygen as measured according to ASTM F1927-14. 3 / m 2 or lower, whereby the oxygen barrier properties measured are provided only by the coating material in the first aspect.
[0029] The first outermost protective material layer may be a thin polymer layer, the purpose of which is to protect the paper-based or paperboard-based laminate packaging material from dirt and moisture in the environment outside the closed packaging container, ie on the side facing the outside of the packaging container made of the packaging laminate.
[0030] The second innermost liquid-tight heat-sealable material layer may comprise a thermoplastic polymer layer which can be easily heat-sealed by available heat-sealing methods (e.g. induction heat sealing or ultrasonic heat sealing, or just contact heat sealing) and is located on the barrier-coated side of the barrier-coated paper-based or cellulose-based substrate which will face the interior of the packaging container made of the packaging laminate, i.e. in direct contact with the packaged food.
[0031] The second innermost layer of liquid-tight heat-sealable material may comprise a polyolefin polymer, such as a lower density range polyethylene, for example selected from the group consisting of LDPE, LLDPE, m-LLDPE and any mixture of two or more thereof.
[0032] According to one embodiment, both the first outermost protective material layer and the second innermost liquid-tight heat-sealable material layer may comprise a polyolefin polymer, such as the same or different types of polyethylene polymers.
[0033] For carton packaging of oxygen-sensitive products, such as liquid or semi-liquid or viscous foods, the laminated packaging material may further include a main body layer of paper or paperboard or other cellulose-based materials, and the cellulose-based substrate coated with the barrier layer is arranged on the inner side of the main body layer of paper or paperboard, between the main body layer and the second innermost liquid-tight heat-sealable material layer. The main body layer may contribute to the bending stiffness of the laminated packaging material and to the dimensional stability of the folding-molded packaging container made therefrom to withstand the strong forces generated by the movement of the package contents (such as liquid and viscous oxygen-sensitive products) during distribution and handling.
[0034] In one embodiment, to achieve such a liquid carton packaging, the second innermost liquid-tight heat-sealable polyolefin layer is a preformed polyolefin film, such as a preformed polyethylene film, such as a cast biaxially oriented polyethylene film, which includes at least one layer having a majority of LLDPE polymer to improve the robustness of the mechanical properties of the laminated packaging material.
[0035] A third aspect of the invention provides a packaging container comprising the laminated packaging material of the second aspect. According to one embodiment, the packaging container is at least partially made of the laminated packaging material of the invention, and according to another embodiment, it is entirely made of the laminated packaging material.
[0036] While it has been assumed until now that improved gas barrier properties of such barrier-coated cellulose-based substrates should be achieved by sourcing better papers or substrates or by coating more polymers with inherent gas barrier properties in thicker layers, which papers or substrates themselves inherently provide gas barrier properties when further laminated to the polymer layer, it is now better understood that the surface portion of the paper or cellulose-based substrate plays a key role for the optimal performance of the subsequently applied coating to bring about gas barrier properties, as well as for the optimized method of applying the barrier-coated layer with high and reliable quality (i.e. without defects and thickness variations) under industrially feasible conditions and with minimal consumption of barrier material. Industrially feasible conditions mean that a good barrier coating must be able to be applied at high speed and, therefore, at low or reasonable, balanced costs.
[0037] It has been seen that the barrier quality of the cellulose based substrate itself does not need to be very high and the amount of gas barrier polymer applied as a barrier pre-coat can be minimized under certain conditions to still produce a high quality barrier coated paper or cellulose based substrate in an economical manner.
[0038] Therefore, the use of a cellulose-based substrate coated with a barrier layer produced by the method of the present invention as described above can provide laminated packaging materials and packaging containers made therefrom with good gas barrier properties on an industrial scale, and can also impart improved repulpability and recycling properties, i.e., improved sustainability, due to the increased content of cellulose fibers that are easily repulpable.
[0039] In general, the use of cellulose-based substrates in laminates and packaging provides a greater proportion of fiber content that is both renewable, i.e., non-fossil-derived, and recyclable or biodegradable, thereby recycling old materials into the creation of new materials. In addition, the use of paper or cellulose-based substrates as "face layers" in sandwich structures supports the use of a body material that has a lower bending stiffness (and therefore lower fiber mass) and is cheaper, or has a lower density and therefore uses a lower amount of fiber, by laminating such face layers on each side of the body layer.
[0040] Therefore, the cellulose-based substrate coated with a gas barrier layer obtained by the method of the first aspect, and the material layer structure produced therefrom, provide improved barrier properties for the laminated packaging material containing it, and may further impart good recyclability and sustainability characteristics. Detailed Description
[0041] The term "long-term storage" used in conjunction with the present invention means that the packaging container should be able to maintain the quality (i.e. nutritional value, hygienic safety and taste) of the packaged food under ambient conditions for at least 1 or 2 months, for example at least 3 months, preferably longer, for example 6 months, for example 12 months, or longer.
[0042] The term "package integrity" generally refers to the seal of the package, that is, the resistance of the packaging container to leakage or damage. The term includes the resistance of the package to the intrusion of microorganisms (such as bacteria, dirt and other materials) that may spoil the filled food and shorten the expected shelf life of the package.
[0043] One major contribution of a laminated packaging material to the integrity of a package is provided by good internal adhesion between adjacent layers of the laminate. Another contribution comes from the material's resistance to defects (e.g. pinholes, tears etc. within each material layer itself), and yet another contribution comes from the strength of the sealing joints by which the materials are sealed together when forming a packaging container. Thus, for the laminated packaging material itself, the integrity performance focuses mainly on the adhesion of each laminate layer to its adjacent layers, as well as the quality of the individual material layers. With regard to the sealing of the package, the integrity focuses mainly on the quality of the sealing joints, which is ensured by good functional operation and a robust sealing operation in the filling machine, which in turn is ensured by the laminated packaging material's well-adapted heat-sealing properties.
[0044] The term "liquid, semi-liquid or viscous food" generally refers to a food with a flowable content, which may optionally also contain solid food pieces. Dairy products and milk, soy, rice, grain and seed beverages, fruit juices, nectars, non-carbonated beverages, energy drinks, sports drinks, coffee or tea beverages, coconut water, wine, soups, crushed tomatoes, sauces (such as pasta sauce), beans and olive oil are some non-limiting examples of contemplated food products.
[0045] Examples of other oxygen sensitive food products that may be packaged and protected with the laminated packaging material of the present disclosure are, for example, dry and / or fatty foods.
[0046] The term "sterility" in relation to packaging materials and packaging containers refers to conditions under which microorganisms are eliminated, inactivated or killed. Examples of microorganisms are bacteria and spores. When a product is aseptically packaged in a packaging container, an aseptic process is usually used. In order to achieve continuous sterility during the shelf life of the package, the integrity of the package is of course very important. In addition, in order to achieve a long shelf life of the filled food, it may also be important that the package has barrier properties to gases and vapors (e.g. to oxygen) in order to keep its original taste and nutritional value intact, such as its vitamin C content.
[0047] The term "body layer" generally refers to the thickest layer or the layer containing the most material in a multilayer laminate, i.e., the layer that contributes most to the mechanical properties and dimensional stability of the laminate (e.g., thick paper, paperboard, or cardboard) and the structural stability of a packaging container folded from the laminate. It may also refer to a layer that provides a greater thickness distance in a sandwich structure, which further interacts with a stabilizing surface layer having a higher Young's modulus on each side of the body layer to achieve sufficient such mechanical properties (e.g., bending stiffness) to achieve structural stability of a formed packaging container.
[0048] OTR was measured using an Oxtran 2 / 21 (Mocon) device based on a coulometric sensor according to ASTM F1927-14.
[0049] The method used to determine OTR determines the amount of oxygen per surface and time unit that passes through a material at a specific temperature, at a given atmospheric pressure, in a specific time (i.e., in an atmosphere of 20% or alternatively 100% oxygen at 0.2 or 1 atmosphere (oxygen) over a 24 hour period).
[0050] Substrates suitable for the method of the present invention are not limited to a certain type of paper or cellulose and also include other cellulose-based substrates, which are based on any type of natural cellulose, fiber cellulose or fibril cellulose. However, the present invention is not suitable for substrates made of plastics or polymers, such as films made of regenerated cellulose.
[0051] The paper or cellulose based substrate has a surface smoothness of 130 ml / min Bendtsen or less, such as 120 ml / min or less, such as 100 ml / min or less, such as 80 ml / min or less, such as 50 ml / min or less, such as 30 ml / min or less, such as 25 ml / min or less, measured according to ISO 8791:4, on its coated side ("top side" or "printing side"), and a Cobb 60 surface water absorption of 30 g / m2, measured according to ISO 535:2014. 2 or lower, plays a good role in the method for manufacturing a structure coated with a barrier layer according to the present invention, so that good such structures can be produced under industrially feasible conditions. It can be understood that the combination of method steps for coating and manufacturing a cellulose-based substrate coated with a barrier layer of the present invention, performed at a high coating line speed, can improve the barrier properties of different paper substrates, as long as the substrate meets a selected set of characteristic parameters. If the surface roughness (measured in Bendtsen values in ml / min) is too high, the surface of the cellulose-based material will have "valleys" and "peaks", so that the thinly applied wet coating of the gas barrier polymer aqueous solution will not be able to fill and smooth the "valleys" or cover the "peaks". Therefore, the applied and dried gas barrier polymer coating will not completely cover the surface, but will have defects that can be detected by dye coloring methods, and oxygen molecules can easily penetrate through the coating through these defects. Therefore, the contribution of such defective and insufficient barrier coating to the gas barrier properties will be significantly reduced. Rougher substrate surfaces naturally require more polymer coating to be applied, which can also be applied at a lower coating line speed. However, at high coating speeds, there are limits to how much aqueous coating can be applied, how much water can be evaporated in the drying operation, and how high the viscosity and solids content of the aqueous barrier polymer solution can be.
[0052] In one embodiment, a surface roughness of less than 120 ml / min Bendtsen is required, such as less than 100 ml / min, such as less than 80 ml / min, such as less than 50 ml / min, such as less than 30 ml / min, such as less than 25 ml / min. When less than 30 ml / min, the substrate surface is very smooth and 0.5 g / m can be applied. 2 A thin coating of PVOH and still completely covers and coats the surface.
[0053] The Cobb 60 method according to ISO 535:2014 measures the water absorption of a cellulose-based substrate under standard conditions and is, to some extent, a measure of the "coatability" of a cellulose-based substrate surface, i.e. the ability to be coated with an aqueous solution composition of a gas barrier polymer. If the surface is able to absorb too much solution before drying, a thinly applied wet coating will crack and fail to form a continuous coating of the gas barrier polymer. It is therefore important that the Cobb 60 value is below 30 g / m 2 , for example, less than 28g / m 2 , and preferably not higher than 25g / m 2 .
[0054] The surface of the top side of the cellulose-based substrate may exhibit a Bendtsen roughness value of less than 30 ml / min and a roughness value of less than 25 g / m 2 Or lower Cobb 60 absorption value.
[0055] To be suitable for the final barrier coating step by a vapour deposition coating process, the cellulose based substrate needs to be thin and have a thickness of 30 to 70 g / m2 as measured according to ISO 536:2012. 2 , for example 30 to 60 g / m 2 , for example 35 to 50 g / m 2 , for example 35 to 45 g / m 2 and has a grammage of 800 kg / m 3 Up to 1400kg / m 3 , for example 900 to 1400 kg / m 3 , for example 950 to 1400 kg / m 3 For reasons of efficiency and production economy, and to avoid blistering of the coating due to air being trapped in the fibrous porous cellulose-based substrate during coating and drying operations, a cellulose-based substrate having a high density and a relatively low weight and thickness is desired. On the other hand, a grammage of less than 30 g / m 2 Cellulose-based substrates may be too mechanically weak and / or have poor dimensional stability when coated with a wet dispersion and subsequently dried, thereby exhibiting shrinkage or curling problems.
[0056] Therefore, it is more preferred to use a grammage of 30 to 50 g / m 2 , for example, most preferably 35 to 45 g / m 2 , density is 900kg / m 3 Up to 1400kg / m 3 Cellulose-based substrate.
[0057] The thickness of the cellulose-based substrate may be 35 to 65 μm, such as 35 to 60 μm, such as 35 to 50 μm, such as 35 to 45 μm. It has been found that for certain applications, such as for liquid-tight packaging of wet or liquid or viscous products, it is also advantageous to use a high-density paper substrate that is as thin as possible, because less polymer may be required in the adjacent liquid-tight or heat-sealable layer while maintaining the integrity of the packaging and its heat seal.
[0058] In one embodiment, the surface of the top side of the paper-based or cellulose-based substrate exhibits a Gurley porosity value of greater than 1000 s / dl, such as greater than 2000 s / dl, according to Tappi T460 om-2. The advantage of a surface with low porosity is that less of the aqueous solution of the gas barrier polymer will be absorbed into the cellulose-based substrate. Since each solution coating of the gas barrier solution is very thin, it is also important for the internal coherence of the coating and the ability of the coating to form a smooth and uniform surface to receive further coatings or layers thereon.
[0059] Therefore, in a cellulose-based substrate suitable for coating with a thin coating of an aqueous solution composition comprising an oxygen barrier polymer, the number and size of pores in the substrate material should preferably be significantly reduced. By extensive refining of the pulp used to make the substrate, the degree of fiber bonding will increase, thereby reducing the porosity. Grease-proof paper is produced by such extensive refining and has a sufficiently low porosity to provide a grease barrier. Therefore, grease-proof paper is regarded as a potential substrate or carrier for an additional gas barrier coating. However, the resulting pulp has a high resistance to dewatering, requires a long time for raw material dewatering, and the manufacturing process is costly and not conducive to repulping and recycling processes. This is also the case for parchment paper, during the manufacturing process, parchment paper is passed through a sulfuric acid bath to obtain gelatinized fibers, which makes the fibers difficult to dewater and repulp, and the parchment paper has an undesirable brittleness.
[0060] According to one embodiment, the cellulose-based substrate used in the present invention may be formed from cellulose fibers comprising at least 50% by dry weight of chemical pulp, such as kraft pulp or sulfite pulp. Sulfate or sulfite pulp is used to obtain a paper that is strong enough for downstream processes such as coating at high line speeds, as well as conversion lamination and final packaging use.
[0061] Sulfate / Kraft pulp may be preferred because it is widely produced in large quantities and facilitates improved repulping in recycling and general dewatering of the fiber. Sulfite fiber typically has a higher proportion of refined fiber, which may have a slightly opposite effect, depending on how high the proportion is and the degree of refining. According to one embodiment of the present invention, Kraft pulp may therefore be preferred.
[0062] The cellulose-based substrate may be formed from cellulose fibers comprising 35-100% (eg 35-80%, such as 40-70%) softwood pulp for forming high density paper by dry weight of pulp. The remainder of the pulp composition may include hardwood fibers and some minor amounts of other fibers.
[0063] The benefits of including softwood pulp are improved paper machine runnability and beneficial strength / toughness properties for the resulting paper. A relatively high proportion of softwood pulp promotes a cellulose-based substrate having a sufficiently high density without causing dewatering problems during substrate manufacturing and enabling repulping in recycling operations. The degree of refinement of the fiber components is further selected to promote dewatering and repulpability while forming a dense paper with relatively low porosity.
[0064] Therefore, although there are some substrate papers with inherently good oxygen barrier properties, these are less preferred for the final material for other reasons, such as low recyclability (repulpability), and a major contribution to the oxygen barrier properties needs to be provided by the coating material in order to coat and adhere well to and interact well with the substrate surface.
[0065] In order to have good coating mechanical properties at high coating line speeds above 300 m / min (e.g. above 400 m / min), the cellulose-based substrate should have a tensile strength of 3 to 6 KN / m in MD (machine direction) and 1.5 to 3.5 KN / m in CD (cross direction). In the present disclosure, tensile strength is measured according to ISO 1924-3:2005. Therefore, a higher tensile strength may indicate that the paper substrate can be used to withstand web handling forces during coating and lamination operations.
[0066] The cellulose-based substrate may also have a tensile strain in the machine direction of 1.4 to 3.5% and a tensile strain in the CD direction of 2.1 to 6.0%.
[0067] The cellulose-based substrate may also have a 35 to 90 J / m 2 The tensile energy in the CD direction is 37 to 140 J / m 2 of stretching energy.
[0068] In addition, the E modulus of the cellulose-based substrate may be 9500 to 12500 MPa in the MD direction and 4000 to 7000 MPa in the CD direction.
[0069] Preferably, beneficial barrier and recyclability properties are obtained without sacrificing tensile strength and other mechanical properties.
[0070] In order to provide good gas barrier properties from small amounts of barrier coating materials, it has therefore been previously discovered that to coat a vapor deposited coating of only nanometer thickness, a thin, defect-free gas barrier polymer pre-coat needs to first be applied to a paper or cellulose-based substrate to provide further barrier properties. Such barrier pre-coats that work best are selected from vinyl alcohol polymers and copolymers, which have inherent gas barrier properties and are food safe and environmentally sustainable, both in terms of recyclability and in terms of industrial coating and lamination processes. Such polymers are water dispersible and / or soluble in water and are applied by an aqueous "dispersion coating" process or a so-called "liquid film coating" process.
[0071] Industrially feasible (i.e. high speed) methods suitable for coating the aqueous gas barrier polymer solution composition of the present invention are generally any suitable wet roll coating method, such as rotogravure roll coating, smooth roll coating and reverse roll or gravure coating. In an advantageous embodiment of the method of the present invention, the aqueous solution composition of the gas barrier polymer is applied by reverse gravure coating. The reverse direction of the gravure coating process has been shown to be more conducive to smoothing the coating surface compared to forward gravure coating, which is more like a printing process that prints the gas barrier polymer onto a surface rather than a full coating process.
[0072] Thus, the gas barrier polymer of the aqueous coating composition can be a polymer or copolymer based on vinyl alcohol monomers, for example selected from polyvinyl alcohol (PVOH), ethylene vinyl alcohol copolymer (EVOH) and modified PVOH and EVOH copolymers that can form an aqueous solution. In some cases, such polymers are modified, for example, by adding carboxylic acid functional groups.
[0073] In one embodiment, the water soluble gas barrier polymer is PVOH, such as PVOH from Kuraray Type PVOH, which provides good film-forming properties, gas barrier properties, cost-effectiveness, food compatibility and odor barrier properties.
[0074] In another embodiment, the gas barrier polymer is a water-soluble EVOH having a low ethylene monomer content, such as EVOH from Kuraray. Type EVOH. The advantage of using EVOH polymer as a gas barrier material is that the ethylene content supports moisture resistance, so that the oxygen barrier properties are better maintained even at higher relative humidity (e.g. 80% RH). This is especially suitable for packaging of oxygen-sensitive liquids, such as paperboard laminate packaging for liquid foods.
[0075] Conventional EVOH polymers are usually used for extrusion and cannot be dispersed or dissolved in aqueous media to produce 4g / m 2 Barrier films coated with thin liquid films of 100 g / m2 or less are used. Water-soluble EVOH contains higher amounts of vinyl alcohol monomer units to be water dispersible and its properties are as close as possible to those of liquid film coating grades of PVOH. Therefore, on the other hand, an extruded EVOH layer is not a substitute for EVOH coated with liquid films because the properties of an extruded EVOH layer are inherently less similar to those of PVOH than those of EVOH grades used for dispersion / solution coating and because it cannot be melt extrusion coated or melt extrusion laminated at less than 4 g / m2. 2 The cost-effective amount comes applied as a single layer.
[0076] Gas barrier compositions based on PVOH perform best when the PVOH has a saponification degree of at least 98 mol % (e.g., at least 99 mol %), but PVOH with a lower degree of saponification will also provide oxygen barrier properties. The most advantageous PVOH quality and grade for the process of the present invention is 6-98.
[0077] In another embodiment, PVOH can be 15-99.
[0078] In yet another embodiment, the PVOH may be 6-96, although this grade may offer slightly lower oxygen barrier properties.
[0079] The EVOH grade suitable for coating in the method of the present invention can be 4104AQ, which has 6-98 similar coatability, and HR-3010, which has 15-99 Similar coatability.
[0080] The solid content of the water-soluble gas barrier polymer should be 5 to 15 wt % to be suitable for the roller coating application method, and can be adjusted to a suitable solid content according to the selection of EVOH or PVOH and the coating speed. The solid content in the method of the present invention is more preferably 7 to 13 wt %, such as 9 to 13 wt %, such as preferably 10 to 12.5 wt %. It has been shown that at a solid content of more than 10%, the best quality PVOH coating can be obtained by the reverse gravure coating method, i.e., the coating is uniform, smooth and substantially free of defects. More specifically, with PVOH grade When 6-98 is used in combination, better results are obtained at high coating line speeds above 300 m / min (e.g. above 400 m / min, such as above 600 m / min).
[0081] The viscosity of the aqueous solution of the gas barrier polymer to be coated should be from 10 to 120 mPa*s, for example from 50 to 100 mPa*s. This allows the gas barrier solution to be optimally picked up by the gravure roll and further transferred onto the substrate surface at high coating line speeds above 300 m / min, for example above 400 m / min, for example above 600 m / min.
[0082] The barrier pre-coat composition may also include a small amount (e.g., about 1 to about 10 weight percent based on the dry coating weight) of an inorganic laminar compound, such as calcium carbonate, CaCO 3 , talc or exfoliated nanoclay particles, such as bentonite. In this case, therefore, the barrier layer can include from about 99 to about 80 weight percent of the polymer based on the dry coating weight.
[0083] The gas barrier composition may further contain additives such as dispersion stabilizers, etc., preferably in an amount of no more than about 1 wt % based on the dry coating. The total dry content of the composition is preferably 5 to 15 wt %, more preferably 7 to 12 wt %.
[0084] Another possible additive in the barrier pre-coat composition may be a polymer or compound with functional carboxylic acid groups to improve the water vapor and oxygen barrier properties of the PVOH coating. Suitably, such polymers with functional carboxylic acid groups are selected from ethylene acrylic acid copolymers (EAA) and ethylene methacrylic acid copolymers (EMAA) or mixtures thereof. In one embodiment, such a barrier layer mixture may consist essentially of PVOH, EAA and an inorganic layered compound. The EAA copolymer may be included in the barrier layer in an amount of about 1-20 wt %, such as 1 to 15 wt %, such as 1 to 10 wt %, based on the dry coating weight.
[0085] It is believed that some of the further improved oxygen and water barrier properties may be due to the esterification reaction between PVOH and EAA at elevated drying temperatures, whereby the PVOH is cross-linked by the hydrophobic EAA polymer chains, which are thus built into the structure of the PVOH. Alternatively, cross-linking may be induced by the presence of multivalent compounds (e.g., metal compounds, such as metal oxides). However, such mixtures are more expensive due to the cost of the additives and may not be as preferred from a recyclability perspective.
[0086] Thus, while it is more preferred to use a barrier pre-coat made from a pure PVOH or EVOH composition, advantageous results may also be obtained with a gas barrier pre-coat containing other additives as described above.
[0087] In one embodiment, the aqueous solution of vinyl alcohol (co)polymer (eg, PVOH or EVOH) may, for example, contain a small amount of n-octanol as a defoaming additive, for example, in an amount of 0.01 to 0.1 wt %.
[0088] An aqueous solution of a gas barrier polymer is uniformly applied to the surface of the top side of a web of a paper or cellulose-based substrate by a roll coating method to provide a dry weight of 0.5 to 2 g / m 2 Coating. Less than 0.5g / m 2 When the gas barrier performance is higher than 2g / m 2 When the coating is applied to packaging laminates, it will not be cost-effective due to the high energy costs and the short time available for evaporation of the liquid (due to the high coating line speed). 2 and above to achieve a recognizable oxygen barrier level, and between 0.5 and 2 g / m 2 A good balance between barrier properties, coating quality and cost is achieved in a coating of the desired thickness. Typically, a thicker gas barrier polymer coating is required overall, so at least one further coating step is added after the drying of the first coating layer is complete.
[0089] In the process of the invention, the gas barrier coating is applied as at least two partial layers in at least two consecutive steps with intermediate drying. When applied in two partial layers, each layer therefore suitably has a dry weight of 0.5 to 2 g / m 2 The amount applied is, for example, 0.5 to 1.5 g / m 2 , for example, preferably 0.5 to 1 g / m 2 The amount of PVOH applied is 0.5 to 1 g / m2 and allows a higher quality overall layer to be obtained from a smaller amount of liquid gas barrier composition. Most preferably, the two PVOH partial layers are applied at 0.5 to 1 g / m2 each. 2 amount applied.
[0090] The amount of wet coating applied is about ten times higher than the solid target coating applied and dried, so the amount of PVOH wet coating applied is about 5 to about 20 g / m 2 , for example 5 to about 10 g / m 2 , which therefore explains the considerable gram weight of water that needs to be evaporated during the drying step at high coating speeds. It is important not to leave too much moisture on the coated substrate or to allow it to be absorbed by the substrate, as this may interfere with any subsequent steps in the coating process and cause defects in the applied barrier coating, thus compromising the coating quality and ultimately reducing the oxygen barrier properties provided by the barrier-coated substrate.
[0091] The aqueous solution composition of the gas barrier polymer may be heated and applied at a temperature of 60 to 70 degrees C. By heating to such an elevated temperature, the risk of foam bubbles forming in the coating is reduced.
[0092] To further reduce bubble or foam formation in the aqueous gas barrier polymer solution, a defoaming additive may be added. A preferred defoaming agent is n-octanol, which is both food safe and has been shown to provide better results than other tested agents at low amounts (e.g., at low amounts of 0.01 to 0.1 wt % of the solution, such as at low amounts of about 0.05 wt % of the solution). It is noted that the other tested agents deteriorate the PVOH, such that they increase the OTR of the applied and dried PVOH coating.
[0093] According to the method of the invention, it is very important to continue drying only at low temperature, because the wet coating of the aqueous solution of the gas barrier polymer is very thin and may be damaged by applying too strong heat.
[0094] The drying step can be carried out by a hot air dryer, which also allows the water to evaporate and be blown away from the surface of the substrate by air convection. As the substrate passes through the dryer, the substrate temperature is kept constant at a temperature of 60° C. to below 95° C., such as 65° C. to below 90° C., such as 70° C. to below 90° C., such as 70° C. to 85° C., such as 70° C. to 80° C. If desired, at high line speeds, drying can be partially assisted by radiant heat from infrared IR lamps combined with hot air convection drying.
[0095] The more water is added to a wet applied coating, the more water evaporates in the dryer at high line speeds. How high a solids content is possible in a waterborne coating to achieve only 1-2 g / m 2 There is a balance between the drying of thin coatings and the length of the dryer section. The drying speed cannot be too fast, as there is a risk of skinning, nor too slow, as too high a paper absorption can lead to reduced surface film thickness and / or cracked (defective) coatings. Therefore, the evaporation of water should be controlled to avoid excessive substrate surface temperatures and skinning.
[0096] This balance setup may be unique for each coating line / paper / coating combination.
[0097] Preferably, the method of the present invention comprises the step of vapour depositing a barrier coating by physical vapour deposition (PVD) onto a first applied gas barrier pre-coating obtained from a dried aqueous solution of a gas barrier polymer.
[0098] The physical vapor deposition coating may be a material selected from metals, metal oxides and inorganic oxides.
[0099] In the method of the present invention, the barrier deposited coating is selected from aluminum metallization coating, aluminum oxide, AlO x , and aluminum and AlO x Preferably, it is an aluminum metallization coating.
[0100] Such thin vapor deposited coatings are of nanometer thickness, i.e., they have a thickness that is best measured in nanometers, e.g., 5 to 500 nm (50 to ), for example 5 to 200 nm, more for example 5 to 100 nm, for example 5 to 50 nm.
[0101] Typically, below 5 nm, the barrier properties may be too low to be useful, while above 200 nm, such as above 100 nm, such as above 50 nm, depending on the quality of the deposited coating, the barrier coating may be less flexible and therefore more susceptible to cracking when applied to a flexible substrate, and may also be more costly since the deposition coating speed must be lower.
[0102] In one embodiment, the barrier deposit coating is applied to a thickness of 10 to 80 nm, such as 10 to 50 nm, such as 10 to 45 nm.
[0103] The vapor deposited layer consisting essentially of aluminum metal may thus have a thickness of 5 to 50 nm, more preferably 5 to 40 nm, which corresponds to less than 1% of the aluminum metal material present in aluminum foil of conventional thickness for packaging (i.e. 6.3 μm). Although vapor deposited metal coatings require much less metal material, they can only provide low levels of oxygen barrier properties at best and need to be combined with other gas barrier materials in order to provide a final laminate with sufficient barrier properties. On the other hand, it can supplement gas barrier layers such as POVH or EVOH, which do not provide water vapor barrier properties and are quite sensitive to moisture.
[0104] Other examples of vapor deposited coatings are aluminum oxide (AlO x 、Al 2 O 3 ) and silicon oxide (SiO x) coating. Typically, such PVD coatings will be more brittle and less suitable for incorporation into packaging materials by lamination, whereas the metallized layer, although produced by PVD, does have mechanical properties that are more suitable for lamination.
[0105] Typically, due to the nature of the metallization coating process used, aluminum metallization layers inherently have a thin surface portion composed of aluminum oxide.
[0106] In order for the PVD coating process to work optimally, the moisture content in the paper-based or cellulose-based substrate should be maintained between 4% and 8%. If the paper substrate becomes too dry, it may cause its longitudinal edges to curl toward each other and cause coating and handling problems in the method of the present invention. On the other hand, if the moisture content becomes too high, the vapor deposition coating operation may not work properly to provide a high-quality coating.
[0107] In one embodiment, the aluminum metallization layer is applied to an optical density (OD) of 1.8 or higher, such as from 1.8 to 3.5, such as from 2.0 to 3.0, preferably from 2.1 to 2.6. At an optical density below 1.8, the barrier properties of the metallized film may be too low.
[0108] The optical density is measured in production by a densitometer, i.e. an instrument using the principle of diffuse light transmission (e.g. from Macbeth, Tobias or similar). This instrument is suitable for measuring the optical density values of metallized films coated with aluminum. The accuracy and precision of the measurement are very high, about + / - 0.2 OD and about + / - 0.01 OD, respectively, within the measuring range of 0 to 6.60 OD.
[0109] In laboratory measurements, a spectrophotometer can alternatively measure the light transmittance across the entire visible spectrum (380-800 nm). According to the formula OD = -log 10 (I 1 / I 0 ), the optical density is calculated based on the transmittance (T) value at 560nm, and the obtained value is equally accurate (+ / -0.2OD) and comparable to the transmittance densitometer value.
[0110] Typically, a thin coating of a metal or a mixture of a metal and a metal oxide provides barrier properties to water vapor and is used when the desired function is to prevent water vapor from migrating into and through a multilayer film or packaging laminate. Preferably, for the purpose of manufacturing food packaging materials, the metal in the metallized or inorganic metal coating is aluminum (Al).
[0111] The paper or cellulose based substrate coated with a barrier layer obtained according to the process of the present invention provides excellent low OTR and low WVTR and proves to be suitable for lamination into laminated packaging materials and further for folding, forming and sealing operations of forming such laminates into packages.
[0112] The high quality of the dispersion coating is also important and necessary for the resulting high quality of the subsequently applied vapor deposited coating. This is particularly important when the vapor deposited coating is a metallized coating also used for high frequency induction heat sealing, as the uniformity and substantial absence of defects in the coating are particularly important.
[0113] The laminated packaging material comprising a cellulose-based substrate coated with a barrier layer also includes a first outermost protective material layer and a second innermost liquid-tight heat-sealable material layer. The second innermost liquid-tight heat-sealable material layer may include a thermoplastic polymer, such as a polyolefin polymer or be made of a polyolefin polymer. The first outermost protective material layer may be transparent so that the printed decorative pattern outside the main body layer is visible. It may also include a thermoplastic polymer, such as a polyolefin polymer or be made of a polyolefin polymer.
[0114] The carton-based laminated packaging material for liquid food packaging may also include a main body layer of paper or paperboard, a first outermost protective material layer, a second innermost liquid-tight heat-sealable material layer, and the paper or cellulose-based substrate coated with a barrier layer, wherein the paper or cellulose-based substrate coated with a barrier layer is arranged on the inner side of the main body layer of paper or paperboard, toward the interior of a packaging container made of the packaging material, and between the main body layer and the second innermost liquid-tight heat-sealable material layer.
[0115] In one embodiment, the paperboard-based laminated packaging material may include a body layer of paper or paperboard, a first outermost liquid-tight heat-sealable polyolefin layer, a second innermost liquid-tight heat-sealable polyolefin layer, and the paper or cellulose-based substrate coated with a barrier layer, wherein the paper or cellulose-based substrate coated with the barrier layer is arranged on the inner side of the paper or paperboard body layer, toward the interior of a packaging container made of the packaging material and between the body layer and the innermost layer.
[0116] Thus, the barrier coated side of the barrier coated paper-based or cellulose-based substrate faces the second innermost liquid-tight heat sealable layer. Thus, any metallized barrier coating is adjacent to one or more second innermost liquid-tight heat sealable material layers.
[0117] The paper or paperboard main body layer used in the present invention generally has a thickness of about 100 μm to about 600 μm and a weight of about 100-500 g / m 2 , preferably about 200-300g / m 2 The surface weight of the packaging material may be conventional paper or paperboard of suitable packaging quality.
[0118] For low-cost aseptic, long-term packaging of liquid foods, thinner packaging laminates with thinner paper core layers can be used. Packaging containers made from such packaging laminates are not folded and are more like pillow-shaped soft bags. Paper suitable for pouch packaging typically has a density of about 50 to about 140 g / m 2 , preferably about 70 to about 120 g / m 2 , more preferably 70 to about 110 g / m 2 Since the barrier-coated paper-based or cellulose-based substrate of the method of the present invention itself can bring a certain stability to the laminated material, the paper layer corresponding to the "body" layer can be thinner and interact with the barrier-coated cellulose-based substrate through interlayer interaction, thereby still producing a laminated packaging material with full desired mechanical properties.
[0119] The paper or cellulose-based substrate coated with the barrier layer may be bonded to the bulk layer via an intermediate adhesive or thermoplastic polymer bonding layer, thereby bonding the uncoated surface of the paper coated with the barrier layer to the bulk layer. According to one embodiment, the bonding layer is a polyolefin layer comprising mainly ethylene monomer units, such as, in particular, a polyethylene-based polyolefin copolymer or blend layer. The bonding layer bonds the bulk layer to the paper or cellulose-based substrate coated with the barrier layer by melt extrusion laminating the bonding polymer layer between the bulk layer web and the cellulose-based substrate web, and simultaneously pressing the three layers together as they advance through the lamination roll nip, thereby providing a laminated structure by extrusion lamination.
[0120] In another embodiment, the cellulose-based substrate coated with the barrier layer can be bonded to the bulk layer by wet-applying an aqueous dispersion of a tacky composition containing a tacky polymer adhesive to one of the surfaces of the webs to be laminated and pressing the two paper webs together as they advance through the nip of the laminating rollers, thereby providing a laminated structure by wet lamination. During the subsequent lamination process, the moisture of the aqueous tacky composition is absorbed into the fibrous cellulose network of the two cellulose-based layers and partially evaporates over time. Therefore, no forced drying step is required.
[0121] The water-based tacky polymer binder may be selected from the group consisting of acrylic acid polymers and copolymers, starch, cellulose and polysaccharide derivatives, polymers and copolymers of vinyl acetate and vinyl alcohol. For best environmental and sustainability properties, tacky binders derived from plant or non-fossil sources are preferred.
[0122] Suitable thermoplastics for the outermost heat-sealable liquid-tight layer and the innermost heat-sealable liquid-tight layer are polyolefins, such as polyethylene and polypropylene homopolymers or copolymers, preferably polyethylene, more preferably polyethylene selected from low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), single-site catalyst metallocene polyethylene (m-LLDPE) and blends or copolymers thereof. According to one embodiment, the first outermost protective liquid-tight layer is LDPE, and the second innermost heat-sealable liquid-tight layer is a blended composition of m-LLDPE and LDPE to obtain optimal lamination and heat-sealing properties.
[0123] The same thermoplastic polyolefin-based materials (particularly polyethylene) listed for the first outermost layer and the second innermost layer are also suitable as adhesive layers inside the laminate, i.e., adhesive layers between the bulk or core layer (e.g., paper or paperboard) and the barrier film or sheet. In one embodiment, the thermoplastic internal adhesive layer can be a polyolefin layer, such as a polyethylene layer, such as a low-density polyethylene (LDPE) layer.
[0124] In another embodiment, the second innermost liquid-tight heat-sealable polyolefin layer is a preformed film comprising the same or similar polyolefin as described above, i.e. LDPE, LLDPE and / or m-LLDPE, such as a biaxially oriented film comprising at least one layer of predominantly LLDPE polymer to improve the robustness of the mechanical properties of the packaging material. Due to the manufacturing process in the film blowing and film casting operations, and the optional subsequent film orientation operation step, the polymer of such a film acquires different properties than a (co)extrusion coated polyolefin layer might acquire. Such a preformed, preferably oriented polymer film would contribute to the mechanical robustness of the laminated packaging material and the mechanical strength and packaging integrity of the packaging container formed and filled with the laminated packaging material.
[0125] According to an alternative embodiment, a suitable adhesive or tie layer inside the laminate (such as, for example, between the bulk layer or core layer and the cellulose-based substrate coated with a barrier layer or between the outer heat-sealable layer and the paper substrate coated with a barrier layer) is also a so-called adhesive thermoplastic polymer (such as a modified polyolefin), which is mainly based on LDPE or LLDPE copolymers or graft copolymers with monomer units containing functional groups (such as carboxyl or glycidyl functional groups) (such as (meth)acrylic acid monomers or maleic anhydride (MAH) monomers) (i.e. ethylene acrylic acid copolymer (EAA) or ethylene methacrylic acid copolymer (EMAA)), ethylene-glycidyl (meth)acrylate copolymer (EG(M)A) or MAH-grafted polyethylene (MAH-g-PE). Another example of such a modified polymer or adhesive polymer is a so-called ionomer or ionomer polymer. Preferably, the modified polyolefin is an ethylene acrylic acid copolymer (EAA) or an ethylene methacrylic acid copolymer (EMAA).
[0126] When the cellulose-based substrate coated with the gas barrier layer is further coated with a vapor deposited coating, the coating also adds water vapor barrier properties to the barrier layer coated substrate, so it is usually not necessary to add other gas or water vapor barrier material layers to the total laminate structure of the packaging material for liquid carton packaging.
[0127] However, in different embodiments, a cellulose-based substrate coated with a gas barrier layer (i.e., coated only with an aqueous gas barrier solution) can be laminated to another water vapor barrier material via an intermediate adhesive layer, rather than being directly coated with a water vapor barrier material. Thus, a paper substrate coated with a gas barrier layer can be bonded to a preformed polymer film having a vapor deposited coating of a metal or metal oxide via one side thereof coated with the barrier layer. Thus, the vapor deposited coating side of the preformed film is bonded to the paper substrate coated with the gas barrier layer. The adhesive layer can be a polymer or adhesive applied by melt extrusion lamination or wet bonding lamination as described above. The polymer matrix of the preformed film can also include a heat-sealable polymer layer on its opposite side, which can participate in the heat sealing operation of the laminated packaging material. Alternatively, or in addition, a separately applied heat-seal polymer can be applied to the inner side of the preformed film to form the second innermost liquid-tight heat-sealable layer of the laminated packaging material. Therefore, separately manufactured barrier-coated substrate paper and barrier-coated prefabricated polymer film can also be combined into a laminated packaging material to well protect oxygen-sensitive products from excessive exposure to oxygen under conditions of high moisture content (e.g., 80-90% relative humidity) in the laminate.
[0128] According to various specific embodiments, the laminated packaging material may have a preformed polymer film substrate laminated on the inside of a paper substrate coated with a barrier layer (i.e., on the side of the paper substrate opposite to the side laminated to the bulk layer), wherein the polymer composition of the preformed polymer film further comprises an inorganic layered compound to provide gas barrier properties to the preformed polymer film, rather than vapor depositing a metal or metal oxide coating. Such a filled polymer film may also protect the gas barrier coating on the paper coated with the barrier layer when the moisture content in the material is high (e.g., when packaging oxygen-sensitive liquid products).
[0129] However, in order for the thin barrier coating to provide the best possible oxygen and water vapour barrier properties, it is most advantageous and preferred if the gas barrier polymer coating is directly further coated by vapour deposition of the metal or metal oxide coating.
[0130] The laminated packaging material produced according to the above method provides good integrity when converted into filled packaging containers by good adhesion and interaction between adjacent layers within the laminate structure and by providing good quality gas barrier coatings and vapor deposited barrier coatings. Especially for the packaging of liquids and wet foods, an important conclusion is that the interlayer adhesion within the laminated packaging material as well as the oxygen barrier properties are maintained under wet packaging conditions.
[0131] According to a further embodiment, a packaging container formed from a laminated packaging material may be partially sealed, filled with a liquid or semi-liquid food and subsequently sealed by sealing the packaging material to itself (optionally in combination with a plastic opening or top portion of the package).
[0132] In summary, the barrier coated cellulose based substrate as defined in the present invention and the laminated packaging material comprising the barrier coated cellulose based substrate can achieve a robust and reliable packaging for liquid food packaging for long shelf life and storage due to the improved barrier properties provided. The laminated packaging material structure is more suitable for forming folded-to-form packaging, both because of the improved adhesion between the substrate and the barrier material coating and because of the improved contribution of the barrier coating substrate itself to the gas barrier properties, which may also be due to the improved bonding cohesion and adhesion of the barrier coating to the barrier coated cellulose based substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0133] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings, in which:
[0134] Figure 1a Schematically shows an example of a cross section of a cellulose-based substrate coated with a gas barrier layer produced by the method according to the present invention,
[0135] Figure 1b Another example of a cellulose-based substrate coated with a gas and water vapor barrier layer produced by the method according to the present invention is schematically shown,
[0136] Figure 2a A schematic cross-sectional view of a laminated packaging material is shown, the laminated packaging material comprising Figure 1a A cellulose-based substrate coated with a barrier layer,
[0137] Figure 2b A schematic cross-sectional view of a laminated packaging material is shown, comprising Figure 1b A cellulose-based substrate coated with a barrier layer,
[0138] Figure 2c Another laminated packaging material is shown, which comprises Figure 1b A cellulose-based substrate coated with a barrier layer,
[0139] Figure 3a A method for dispersing a gas barrier coating composition onto a cellulose-based substrate is schematically shown.
[0140] Figure 3b Schematically showing a method for melt (co)extrusion coating a thermoplastic heat-sealable and liquid-tight polymer layer onto a web substrate to form the innermost and outermost layers of the packaging laminate of the present invention,
[0141] Figure 4 A schematic diagram of an apparatus for physical vapor deposition (PVD) coating on a coil substrate using a solid metal evaporator is shown,
[0142] Figure 5a , 5b 5c and 5d show typical examples of packaging containers produced from the laminated packaging material according to the present invention,
[0143] Figure 6 shows the principles of how such packaging containers can be manufactured from packaging laminates in a continuous, roll-fed, form, fill and seal process, and
[0144] Figures 7a-7f Results obtained from comparative coating tests on the quality of wet applied aqueous gas barrier coatings are shown. DETAILED DESCRIPTION
[0145] In various cases, various paper substrates were coated with aqueous PVOH solutions at high line speeds of more than 300 m / min (e.g., 400 to 600 m / min) to verify whether a uniform and defect-free coating was achieved to provide additional, reliable oxygen barrier properties to the paper substrate under industrially viable manufacturing conditions. This was possible in previous pilot and laboratory scale coating experiments, but significant problems were encountered when scaling up to industrial speeds.
[0146] At industrial line speeds, two major interrelated issues arise. First, as the line speed through the hot air convection dryer during the drying step increases, there is insufficient time to evaporate the excessively high amount of water applied by the aqueous wet coating composition. As a result, the moisture content in the substrate coated with the gas barrier layer can become too high, for example, in excess of 8 weight percent, and cause problems in subsequent operations involving high temperatures, such as in vapor deposition coating processes or other heated lamination processes. Second, as the line speed through the dryer increases, the temperature of the drying operation also needs to be increased, which results in higher heat loads on the wet coated coating and higher temperatures of the paper substrate, which together promote the formation of defects in the coating, such as skinning, bubbles, pinholes, and inconsistent, non-uniform material in the coating. Therefore, it is important to be able to balance the effects of coating and manufacturing process variations and determine a set of robust settings and parameters that can be used for aqueous gas barrier coatings at high coating line speeds.
[0147] During the course of the experiments, a number of root causes for defect formation at high line speeds were identified. On the one hand, the applied wet coating must not be too thick and heavy, and on the other hand, the surface of the substrate must be well covered so that a uniform, defect-free dry coating can be formed. The surface properties of the paper substrate support or hinder the formation of oxygen-sealing dry polymer coatings of PVOH or EVOH from thinly applied aqueous polymer solutions. The desire to coat at high line speeds is hampered by the need to apply more wet coating due to the rough and highly absorbent substrate surface. The greater amount of water applied and the associated higher moisture content in the structure further have a negative impact on the ability of the paper substrate to be subsequently coated and / or laminated. The need for higher line speeds hinders drying operations and increases the need for more severe temperatures acting on the coated substrate. Higher temperatures have a negative impact on both the paper substrate and the coating. Therefore, it has been concluded that paper substrates with higher density and smoother surfaces are generally more suitable for high-speed coating. In addition, the grammage of the paper should be as low as possible, as long as the web has sufficient mechanical strength. The low paper substrate weight has positive effects on the subsequent vapour deposition coating step and further down the value chain, for example, by causing less strain on the laminate when folding into packaging. Example 1
[0148] Three different high-density paper substrates were coated with a PVOH gas barrier coating using different process parameters and compared with the results obtained by coating a similar paper (but with a lower density and a less smooth surface) in the same way. The coating was carried out on the top side of each paper substrate web at a speed of about 400 m / min. The coating was carried out by reverse gravure coating at a speed of about 8 g / m 2 Apply the first PVOH (measured by gravimetric method) 6-98 aqueous solution wet coating, the solid content of the solution is about 10% by weight, the viscosity is about 50mPa*s. The wet coated substrate is transferred to a drying station, where hot air acts on the wet substrate to evaporate its water, and the temperature of the drying tunnel and the air is carefully adjusted to keep the temperature of the substrate surface below 85-90 degrees Celsius. Thus, after drying, 0.8g / m 2 A second coating was applied in the same manner on the dried first coating in the same amount and then dried to provide 1.6 g / m PVOH together with the first coating. 2 Dry weight of full gas barrier PVOH coating.
[0149] The PVOH coatings in Table 1 were applied under optimized coating conditions, as defined in Claim 1 appended hereto.
[0150] The moisture content in the paper substrate is controlled simultaneously in the range of 4-8 wt% by drying to ensure that the next step of metallization coating with aluminum by physical vapor deposition does not fail and cause defects. For the papers tested, it can be seen that at a moisture content below 4 wt%, the paper substrate tends to "curl", i.e., to roll up in the transverse direction of the web, so that the web tends to form a paper tube in the machine direction.
[0151] The resulting uniformly smooth surface of the dried gas barrier coating in turn enables the application of further high quality vapor deposited coatings which are coherent, homogeneous and pinhole-free and which adhere well to the surface of the dried gas barrier coating.
[0152] Thus, a thin aluminum coating was applied to the surface of the second PVOH coating by passage through the PVD metallizer, with an optical density of about 2.5 (measured by an optical transmission densitometer) and a thickness of about 50 nm.
[0153] The barrier coated paper substrate was then laminated into the same packaging laminate structure as follows:
[0154] / / Outside 12g / m 2 LDPE / Duplex CLC 80mN, main paperboard layer / 20g / m 2 LDPE / paper substrate coated with barrier layer (as listed in Table 1) / 6g / m 2 EAA adhesive polymer / 13-20g / m 2 LDPE / 17gsm LLDPE film / / Table 1
[0155] Duplex CLC paperboard is a conventional type of clay-coated paperboard, the innermost liquidproof and heat-sealable layer being made of a preformed cast biaxially oriented film comprising at least one layer of mainly linear low-density polyethylene (LLDPE). The side of the paper substrate coated with the barrier layer is directed inwards in the laminated structure (corresponding to the interior of the packaging container made of the laminate). The paperboard body layer is laminated to the barrier-coated paper by melt extrusion lamination of the LDPE polymer between two webs of the paperboard body layer and the barrier-coated paper substrate to be joined in the nip of the cooled laminating rolls. The adhesive polymer EAA and the inner adjacent LDPE layer are coextrusion laminated together between the barrier-coated paper and the innermost preformed film comprising LLDPE. The outermost LDPE layer (which faces the outside of the laminate and the packaging made therefrom) is extrusion coated on the outside of the paperboard.
[0156] Oxygen transmission measurements were performed at 23°C, 50% and 80% RH (relative humidity) using an Oxtran Mocon 2 / 21 device (a coulometric sensor based device) and the measured values were expressed as cc / m2 over a 24 hour period at an oxygen concentration of 0.2 atm (i.e. 1 atm air). 2 Report to the unit.
[0157] Paper A is a high-density calendered paper with a smooth surface and a grammage of about 40g / m 2 In addition, the Cobb 60 absorption value is quite low, at 22g / m 2 , so it also has good paintability.
[0158] Paper B is a significantly denser and less porous paper, with a measured density of 1055 and a grammage of approximately 45. It also has a smooth, non-absorbent surface, making it ideal for coating with aqueous polymer solutions.
[0159] Paper C is a less smooth paper with a similar density to Paper A but much less porosity. This paper contains highly refined fiber components and fibrils so that the pores between the longer fibers are filled with smaller cellulose components, which unfortunately also makes the paper brittle and less suitable for flexible lamination for folding carton packaging. Despite the density of Paper C substrate, its Cobb 60 absorption is higher and its top side surface is not as smooth as Papers A and B.
[0160] All paper substrates AC are calendered to provide higher density and surface smoothness.
[0161] For comparison, a coating treatment was applied to Paper D, which is a more porous and less dense paper substrate, but still has a fairly smooth surface of the glassine type, and therefore also involves some finer cellulose fibers and fibrils to "close" its top surface.
[0162] From the above coating and lamination tests, it can be concluded that for paper substrates with higher surface roughness, such as paper C, more coatings need to be applied to form a defect-free and uniformly thick gas barrier coating from the PVOH aqueous solution to further reduce the oxygen permeability. Therefore, in this test, it can be seen that the OTR does not significantly improve the oxygen barrier properties. On the other hand, paper C has very high inherent oxygen barrier properties, that is, when laminated in the same way into the same laminate structure, the OTR is lower without the barrier layer. Paper C has inherent barrier properties due to the content of cellulose fibrils and fines that fill its fiber structure, and the paper is super calendered, so the paper is very dense and has a very low porosity. Early pilot laboratory tests have found that paper C can be coated to very low total gas barrier values, such as 0.2cc / m 2 , 24 hours (23 ° C, 0.2atm, 50% RH), but it was also found in industrial tests that it is impossible to achieve such low values at industrial speeds (i.e. 400 or 600m / min), and in order to achieve the lowest possible OTR, it is necessary to pre-coat starch and then apply PVOH gas barrier coating. Therefore, these tests concluded that the surface of paper C is too rough and requires further smooth pre-coating. Therefore, this example shows that only 1.6g / m 2 The thin coating of PVOH did not allow for a robust, reliable and defect-free coating, so the oxygen transmission rate remained at the same level as the uncoated paper C. In any case, paper C was not selected due to other disadvantages, such as less suitable mechanical properties and recycling properties (deriving from the higher content of highly refined cellulose components). It was also concluded previously that for paper substrates to be coated with a high surface roughness, it is best to first smooth the surface by pre-coating with a smoothing substance such as starch, which has much lower or no inherent gas barrier properties.
[0163] Early trials have concluded that when measuring a good barrier coated paper at 50% RH, the OTR values of laminates with only PVOH coated paper are only less than 2 times higher compared to further metallized PVOH coated paper. It has also been found that when OTR measurements are made on laminated samples including a metallized coating at 80% relative humidity, the effects of the different contributions of the different paper grades tend to balance out and the oxygen barrier results appear to be at the same high level (i.e. about the same low OTR values), provided that the coating quality is good. On the other hand, if the OTR of the same packaging laminate with only PVOH coated paper substrate is measured at 50% RH and 80% RH, the OTR will increase by 4 to 10 times at 80% RH (0.2atm oxygen and 23 degrees Celsius) due to the moisture sensitivity of the gas barrier polymers (PVOH, EVOH, starch, etc.).
[0164] Table 1 further shows how the quality of the gas barrier polymer coating of different papers is ranked after the second aqueous coating and the subsequent drying step, based on an internal test method for detecting defects in the coated barrier layer. A substantially defect-free polymer barrier coating ensures a further defect-free or low-defect aluminum metallization coating by a subsequent optional physical vapor deposition coating step. The quality of the aluminum metallization coating is evaluated partly by observing its surface under a SEM microscope and partly by measuring the final oxygen transmission rate OTR value in the laminate obtained therefrom. Example 2
[0165] FIG. 7 shows an evaluation of the effects of the method steps and coating conditions in the coating method of the present invention. The parameters compared in this example are the maximum temperature of the surface of the cellulose-based substrate during the drying operation and the solid content of the aqueous gas barrier solution composition. Defects in the PVOH coating are visualized by applying a solvent-based (non-aqueous) colorant composition to indicate incomplete defects in the PVOH coating, so that the color solution penetrates the pores of the PVOH coating and reaches the surface of the paperboard and is colored with dots or spots, so it is clearly visible to the naked eye. The colorant composition includes a solvent, a non-ionic surfactant, and an oil-soluble organic red dye. The test sample is dry, clean and does not contain interfering substances (fats, greases, etc.). The colorant solution is applied to the coating surface of the paper substrate, completely covering the sample area, and is left on the surface for about 10 minutes, and then the excess is wiped off with dry paper or a dry cloth. Subsequently, inspection and counting / evaluation of the coloring traces of any defects are performed.
[0166] FIG7 shows an example of a series of comparative coating tests evaluated at a coating line speed set at 400 m / min, firstly, in which the drying maximum temperature of the substrate surface was varied and secondly, in which only the solids content of the PVOH aqueous solution was varied, in order to illustrate the influence of these characteristics on the quality of the applied PVOH coating. 6-98) after coating (PVOH solution concentration is 0.8g / m 2 ), and then after each coating step drying at the highest different surface temperatures, the tested paper substrate samples are photographed. Typically, the highest surface temperature will be reached at the end of each drying operation, i.e. for each given drying area, the highest surface temperature is reached at the end of the drying step.
[0167] Therefore, in Figure 7a In the coating process, the temperature of the substrate surface did not exceed 60 degrees Celsius in any case, and the solid content of PVOH was set at 10% by weight. The result was a good coated surface, and the colorant test produced only a few colored spots, indicating small holes in the dried coating, through which the colorant solution entered to color the coated paperboard surface, such as Figure 7a However, the moisture content of the coated paper substrate is rather high and is at the limit of suitability for an optional next metallization step by PVD coating.
[0168] Similarly, for Figure 7b-7e The resulting coated paper shown in FIG. 1 is a coating method performed with an increase in the maximum drying temperature of the substrate surface, wherein the PVOH solution has the same composition and solid content, while the Figure 7e Compared with the coating operation in Figure 7f The solid content increases while the maximum temperature remains constant.
[0169] Therefore, in Figure 7b In the case of , the drying temperature instead had a maximum drying temperature at 70 degrees Celsius and it can be seen how the moisture content is reduced, while the number of defect signs remains low. Figure 7c In the method, the maximum temperature was kept below 80 degrees Celsius, defect signs remained minimal, and the moisture content of the paper substrate was reduced to a more suitable 4.5%.
[0170] In addition, in Figure 7d In the related process, the maximum temperature of the paper substrate surface was increased to 90 degrees Celsius and the number of defects was also very low. Due to the increase in drying temperature, the moisture content of the paper was reduced to 3.9% by weight, however, this is the lower limit, where a tendency of the paper substrate to curl, i.e. to roll up in the machine direction (MD), can be seen.
[0171] In with Figure 7e and 7f In the related process, the temperature was instead maintained at an excessively high surface temperature of just below 115 degrees Celsius, and a sharp increase in defects was observed in both coated samples. The worst coated sample was obtained in 7f, where the solids content of the PVOH coating solution was also higher, i.e., 12.5%, while coated sample 7e was slightly better, but still not a gas barrier coating. In addition, in samples 7e and 7f, the paper substrate dried out and began to curl.
[0172] It can therefore be seen that the maximum temperature should not exceed 95 degrees Celsius in order to maintain equilibrium with the moisture content of the barrier coated paper substrate and if such drying conditions can be maintained very few defects are obtained. A maximum drying temperature slightly below 80-90 degrees Celsius appears to be optimal to provide as few defects as possible and a low but balanced moisture content in the substrate. Figure 7a , 7b All coated samples in 7c and 7d had very few defects, i.e., less than 10 color dots per square dm. Figure 7e and 7fIn the above examples, the moisture content of the resulting coated paper was too low and paper curling was observed. Compared to the ranking in Table 1, Figure 7e and 7f The results obtained with the method were considered to fail, with a rating of 4 being “very poor”.
[0173] It should generally be noted that any few or many dots or flaws seen are signs of a poor oxygen barrier coating regardless of the material used, i.e., each colored dot or spot represents a point of oxygen penetration through the coating and the cellulose-based substrate to which the barrier is applied.
[0174] Table 1 further shows the ranking of paper substrates in terms of recyclability, i.e. the ranking of repulpability of paper substrates. The repulpability was tested by the Valmet repulping method in a Valmet pulper model HD400, which involves repulping 0.5 kg of air-dried paper base (cut into 0.04×0.10 m chips) with 15 liters of 42 degrees Celsius water in a Valmet pulper at 50 Hz for 7.5 minutes. The dewatering ability of the pulp samples and the appearance and feel of the remaining cellulose in the filter were studied. The repulpability was evaluated based on the visual appearance of the pulp as well as the handsheets.
[0175] Paper A repulped in a good manner, with only a few pieces of paper seen in the pulp as well as in the handsheet. Fiber flocculation was seen in the handsheet, which is a sign of long fibers. Long fibers are good from a recyclability point of view.
[0176] Paper C was completely repulped. The pulp was thicker than the other variants and no larger pieces of paper were seen in the pulp. From the beginning, the amount of short fibers was higher, which resulted in very fine fibers after repulping. The fine fibers and / or tiny fibers clogged the filters in the paper machine, so the process of making handsheets was very slow.
[0177] Paper D shows relatively poor repulping results. Sheets are seen in both pulp and hand paper. More short fibers are seen in hand paper compared to other papers.
[0178] Internal relative ratings between the samples were assigned in the order of 1-4, with 1 indicating good "repulpability". Thus, Papers C and D proved not to be as good as expected, although they were selected with this property in mind.
[0179] Laminated packaging materials, such as those produced as described above in connection with the configurations described in Table 1, were further evaluated in limited filling machine trials for forming and filling and sealing into filled packages. No major issues with package integrity (i.e., package sealing in relation to the surrounding environment) and sealing were found during the trials and were therefore considered successful.
[0180] Furthermore, it was concluded that a laminate structure having a prefabricated heat-sealable film on the inner side of a paper substrate coated with a barrier layer is beneficial to the mechanical robustness of the laminated packaging material and the packaging container made therefrom by heat sealing.
[0181] In addition, regarding the attached drawings:
[0182] exist Figure 1a In FIG. 1 , an example of a cellulose-based substrate 10a coated with a barrier layer produced by the method of the present invention is shown in cross section. The cellulose-based substrate 11 is a cellulose-based substrate having a density greater than 900 kg / m 3 , weight is about 40g / m 2 , the top roughness Bendtsen value is less than 30ml / min and the Cobb 60 value is less than 25g / m 2 of paper and has a PVOH (from Kurary 6-98), the first gas barrier coating 12a is applied by reverse gravure coating in the form of an aqueous solution, and then heated and dried at 80 to 85 degrees Celsius to evaporate the water in the wet coating. The dry weight of the resulting PVOH coated with a gas barrier layer is about 0.8 g / m 2 In addition, the paper substrate has a second gas barrier coating 12b made of the same PVOH solution (from Kuraray 6-98) and applied to the dried surface of the first gas barrier layer 12a. The gas barrier layer 12b has been applied and dried in the same manner, and the dry weight of the second PVOH gas barrier layer is also about 0.8g / m 2 . PVOH gas barrier coatings are sensitive to moisture, dirt and liquids, so at least one further layer or coating 13 of protective polymer is optionally applied over the second PVOH coating 12b. This further layer or coating 13 may be a thermoplastic polymer, such as a polyolefin, such as LPDE. Such a further layer is typically necessary for measuring the oxygen transmission rate of a cellulose-based substrate coated with a barrier layer in order to cover any defects, such as pinholes, in the first PVOH coating. The idea here is that there are no defects in the coating or the number of defects is negligible, so a further polymer layer over the barrier coating should not actually be necessary. In any case, the further polymer layer or further coating itself does not have inherent oxygen barrier properties and therefore does not further affect the measured oxygen transmission rate value. A further layer or coating 18 of protective polymer may also be optionally applied to the other side of the cellulose-based substrate, which further layer or coating 18 may be of the same or different type than the coating or layer 13. Thus, a simple laminate 10a is obtained by simply adding the outermost protective polymer layers 13 and 18 to the cellulose-based substrate coated with the barrier layer.
[0183] exist Figure 1b, another example of a cellulose-based substrate 10b coated with a barrier layer prepared by the method of the present invention is shown in cross-section. Figure 1a The first and second gas barrier coatings of the same PVOH are applied to the same cellulose-based substrate 11 in the same manner as in the above. In addition, such a cellulose-based substrate coated with a gas barrier layer is a vapor-deposited coating having an aluminum metallized coating 14 (i.e., an aluminum metallized layer) applied to the dried surface of the second gas barrier coating 12b by physical vapor deposition, with an optical density of about 2 and a thickness of about 40 nm. Figure 1a In the same manner as in the above, at least one further layer or coating 13 of protective polymer is optionally applied over the aluminum metallized coating layer 14. This further layer or coating 13 may be a thermoplastic polymer, such as a polyolefin, such as LPDE. A further layer or coating 18 of protective polymer may also be applied to the other side of the cellulose-based substrate (not shown), which further layer or coating 18 may be of the same or different type than the coating or layer 13. Thus, a simple laminate 10b is obtained by simply adding the outermost protective polymer layers 13 and 18 (not shown) to the cellulose-based substrate coated with the barrier layer.
[0184] exist Figure 2a , a laminated packaging material 20a for packaging oxygen-sensitive products (e.g., for liquid carton packaging) is shown, which includes a cellulose-based substrate 25a (coated with a barrier layer) manufactured by the method of the present invention. Figure 1b 10b) of the laminate includes a laminate having a bending force of 80 mN and about 200 g / m 2 The present invention relates to a paperboard main body layer 21a of paperboard having a grammage of paperboard, and also includes an outermost protective (e.g., liquid-tight and heat-sealable) polymer layer 22a applied to the outer side of the main body layer 21a, which side will face the outside of the packaging container made of the packaging laminate material. Layer 22a is transparent to show the printed decorative pattern 27a printed on the paper or paperboard main body layer to the outside. The printed pattern can thus inform the contents of the package, the packaging brand, and other information for consumers in retail facilities and food stores. The polymer of the outermost layer 22a can be a polyolefin, such as conventional low-density polyethylene (LDPE) of heat-sealable quality, but may also include other similar polymers, including LLDPE. Its application amount is about 12g / m 2. The innermost liquid-tight heat-sealable layer 23a is arranged on the opposite side of the main body layer 21a, which side will face the interior of the packaging container made of the packaging laminate material, that is, layer 23a will be in direct contact with the packaged product. Therefore, the innermost heat-sealable layer 23a will form a strong transverse heat-seal portion of the liquid packaging container made of the laminated packaging material, which includes a combination of one or more polyethylenes, and the polyethylene is selected from the group consisting of: LDPE, linear low-density polyethylene (LLDPE), and LLDPE prepared by polymerizing ethylene monomers with C4-C8 (more preferably C6-C8) α-olefin alkylene monomers in the presence of a metallocene catalyst (i.e., the so-called metallocene-LLDPE (m-LLDPE)). Its application amount is about 22g / m 2 .
[0185] The main body layer 21a is laminated to the Figure 1b The intermediate bonding layer 26a is formed by melt extrusion molding it as a thin polymer melt curtain between two paper webs, and thus laminating the main body layer and the paper substrate coated with the barrier layer to each other when all three layers pass through the cooled nip of the press rolls. The thickness of the intermediate bonding layer 26a is 12 to 18 μm, for example, 12-15 μm.
[0186] The innermost heat seal layer 23a may be composed of one or two or more layers of the same or different types of LDPE or LLDPE or their blends, and is well adhered to the metallized barrier deposit coating surface 14 of the barrier paper substrate 10b through an intermediate coextruded tie layer 24a made of, for example, ethylene acrylic acid copolymer (EAA), the tie layer 24a being several g / m 2 , for example 4 to 7 g / m 2 , thus, the innermost heat sealable layer is bonded to the barrier layer coated paper substrate 10b when the layers are applied together in a single melt coextrusion coating step.
[0187] exist Figure 2b , another embodiment of a laminated packaging material 20b is shown, which includes a cellulose-based substrate 25b coated with a barrier layer produced by the method of the present invention. The laminated material includes a flexural strength of 80 mN and a strength of about 200 g / m 2 The outer polyolefin layer 22b is a conventional low-density polyethylene (LDPE) of heat-sealable quality and has been coated at 12 g / m 2The amount of the heat sealable layer 23b is applied, but other similar polymers, including LLDPE, may be included. The innermost liquid-tight heat-sealable layer 23b is arranged on the opposite side of the main body layer 21b, which will face the interior of the packaging container made of the packaging laminate, that is, the layer 23b will directly contact the packaged product. Thus, the innermost heat-sealable layer 23b will form a strong heat seal portion of a liquid packaging container made of a laminated packaging material, which includes one or more polyethylenes selected from the group consisting of LDPE, linear low-density polyethylene (LLDPE), and LLDPE produced by polymerizing ethylene monomers with C4-C8 (more preferably C6-C8) α-olefin alkylene monomers in the presence of a metallocene catalyst (i.e., so-called metallocene-LLDPE (m-LLDPE)) One or more or combinations thereof.
[0188] The main body layer 21b is laminated to the paper substrate 25b (i.e., the paper substrate 25b) coated with the barrier layer by wet lamination using an intermediate adhesive layer 26b which is a thin layer of adhesive polymer. Figure 1b 10b) shown in FIG. 10b), this is achieved by applying an aqueous dispersion of polyvinyl acetate adhesive to one of the surfaces to be adhered to each other and then pressing them together in a roller gap. This lamination step is performed at industrial speed in an efficient cold lamination or ambient lamination step without any energy-consuming drying operation to accelerate the evaporation of water. The dry coating weight of the intermediate adhesive layer 26b is only 3 to 4 g / m 2 , which means that drying and evaporation are not required.
[0189] Therefore, with Figure 2a The amount of thermoplastic polymer in the laminate layer can be significantly reduced compared to the conventional melt extrusion laminated polyethylene adhesive layer 26a described in .
[0190] According to a preferred embodiment, the innermost heat-sealable and liquid-proof layer 23b consists of a pre-made oriented film comprising at least one partial layer of mostly linear low-density polyethylene (LLDPE). The film may also comprise some LDPE.
[0191] The preformed film is laminated to the barrier-coated paper substrate by intermediate melt extrusion lamination adhesive layer portion, laminated to the surface of its vapor deposited barrier coating (i.e., aluminum metallization layer), the adhesive layer portion including the EAA tie layer (also used for Figure 2a The laminated material) and / or LDPE adhesive layer 24b has a thickness of 12 to 20 μm, for example 12 to 18 μm.
[0192] In an alternative embodiment, the pre-film 23b' can be coated with 3 to 4 g / m 2 The content of the acrylic (co)polymer adhesive layer 24b' is laminated to the metallized coating by another wet lamination step using an aqueous adhesive.
[0193] Another embodiment is also disclosed herein, which has all of the above features and Figure 2a The melt extruded main layer laminate layer 26a, but it is combined with the characteristics of the innermost heat sealable film structure 23, 23b', and the innermost heat sealable layer structure 23b' is applied by melt extrusion lamination with layer 24b or by wet lamination of water-based adhesive 24b', such as combined Figure 2b described.
[0194] Yet another embodiment is also contemplated and thus disclosed, wherein Figure 2b A thin, wet, aqueous adhesive dispersion laminate layer 26b is combined with conventional melt coextrusion coated inner layers 24a and 23a.
[0195] exist Figure 2c , another embodiment of a laminated packaging material 20c is shown, which includes a cellulose-based substrate 25c coated with a barrier layer manufactured by the method of the present invention, namely Figure 1a 10a as described above. This cellulose-based substrate coated with a gas barrier layer (which is not further coated with a vapor-deposited water vapor barrier layer) can be supplemented in a laminated packaging material by laminating the cellulose-based substrate coated with a barrier layer on its inner side to the vapor-deposited coated preformed polymer film 28c. Thus, the laminated packaging material 20c has the same Figure 2a or Figure 2b The corresponding layers with respect to the paperboard body layer 21c, the outermost protective polymer layer 22c and the inner lamination layer 26c are of the same type and the same layers.
[0196] The preformed polymer film 28c comprises a polymer film substrate 28a and a vapor-deposited coating of aluminum metallization and / or aluminum oxide. The preformed vapor-deposited coating film 28c is laminated to a cellulose-based substrate 25c coated with a gas barrier layer through an intermediate adhesive layer 29c (e.g., a melt extrusion lamination layer). The preformed polymer film may include a heat-sealable layer for the innermost side of the laminate 20c. Alternatively, the inner layers 23c, 24c are further melt-coated and extruded onto the inner side of the preformed film 28c.
[0197] exist Figure 3a , a process for coating an aqueous dispersion 30a is shown, which can be used to apply an aqueous composition of a gas barrier polymer coating 12a and 12b. Figure 1a and 1bThe cellulose-based substrate 11 in the wet coating is conveyed to a dispersing coating station 32a, where an aqueous composition is applied to the top surface of the substrate by a roller. If the surfaces on both sides of the substrate are different, one side is usually more suitable for receiving a coating or printing a decorative pattern, so this is the surface to be coated in the present invention (this side is called the top surface or printing surface). Since the water content of the composition is 80-99% by weight, there will be a large amount of water on the wet coated substrate, which needs to be heated, dried and evaporated to form a uniform continuous coating and have uniform quality in terms of barrier properties and surface properties (i.e., uniformity and low defect incidence). Drying is performed by a hot air dryer 33a, which also allows moisture to evaporate and be removed from the surface of the substrate. When the substrate surface passes through the dryer, the temperature of the substrate surface is always maintained below 95°C, for example, maintained between 60 and 95°C, for example, maintained between 70 and 90°C, for example, maintained between 80 and 90°C, for example, maintained below a temperature of about 85°C.
[0198] The resulting paper substrate web 34a coated with a gas barrier layer is sent for cooling and wound on a reel for intermediate storage. In an optional subsequent or later stage, the web coated in this way can be sent for a further coating step to physically vapor deposit the gas barrier deposited coating 14 onto the paper coated with the gas barrier layer.
[0199] Figure 3b The main body layers 21a, 21b, and 21c are respectively shown. Figure 1a The cellulose-based substrate 10a (i.e. Figure 2a and 2b 25a or 25b) or Figure 1b After the barrier layer coated substrate 10b (25c) is prepared Figure 2a , 2b and 2c are the processes for the final lamination step in the packaging laminate 20a, 20b or 20c.
[0200] As combined Figure 2a and 2b As described above, the main body paperboard 21a; 21b can be laminated to the paper substrate 10a; 25a; 25b coated with the barrier layer by wet normal temperature aqueous adhesive lamination or by melt extrusion lamination. Figure 3a The wet laminating adhesive is applied as described in the dispersion coating of the present invention, and lamination is performed by simply pressing the surfaces to be joined together without forcing the adhesive composition to dry. The main methods of melt extrusion lamination are described below. Figure 3b shown.
[0201] The resulting paper pre-laminate web 31b is delivered from an intermediate storage reel, or directly from a laminating station for laminating the pre-laminate of the bulk layer onto the cellulose based substrate coated with the barrier layer. The non-laminated side, i.e. the printed side thereof, of the bulk layer 21a; 21b is melt extrusion coated at a cooled nip 33 by engagement with a molten polymer curtain 32 of LDPE which will form the outermost layer 22a; 22b of the laminate, extruded from an extruder feed block and die 32b. Subsequently, the pre-laminated bulk paper web, now with the outermost layer 22a; 22b coated on its printed side (i.e. the outer side), passes through a second extruder feed block and die 34b and a laminating nip 35, where a molten polymer curtain 34 is engaged and coated on the other side of the pre-laminate, i.e. the barrier coated side of the paper substrate 10; 25a; 25b. Thus, the innermost heat sealable layer 23a (optionally together with a tie layer of an adhesive polymer having functional groups to increase its bonding ability to adjacent layers) is coextrusion coated onto the inside of the paper pre-laminated web to form the final laminated packaging material 20a; 36, which is ultimately wound onto a storage reel (not shown).
[0202] The two coextrusion steps at the lamination roll nips 33 and 35 may alternatively be performed as two consecutive steps in reverse order.
[0203] According to another embodiment, one or both of the outermost layers can be applied in a separate pre-lamination station, where the coextrusion coating is first applied to the outside of the (printed) body paperboard layer and to the metallized coating of the barrier-coated paper substrate, and then the two pre-laminated paper webs are finally laminated to each other as described above.
[0204] According to various embodiments, the innermost layer of heat-sealable liquid-tight thermoplastic layer is applied in the form of a pre-made film, which is laminated to the coating side of the paper substrate 10a; 10b; 25a, 25b coated with the barrier layer.
[0205] As combined Figure 2a and 2b As mentioned above, such innermost layer 23a; 23b, 23b' can be laminated to the paper substrate 10a coated with the barrier layer by melt extrusion lamination or wet normal temperature aqueous adhesive lamination.
[0206] Figure 4Schematic diagram of an example of an apparatus for physical vapor deposition (PVD) of, for example, aluminum metal coating onto a web substrate of the present invention. A barrier-coated paper substrate 44 is conveyed through a deposition chamber in which a continuous evaporative deposition 40 of evaporated aluminum is carried out on its barrier-coated side to form a metallized layer of aluminum, or alternatively a continuous evaporative deposition 40 of a mixture of oxygen and aluminum vapor is carried out to form a deposited aluminum oxide coating. The coating has a thickness of 5 to 100 nm, preferably 10 to 50 nm, thereby forming a barrier-coated paper 43 of the present invention. Aluminum vapor is formed by ion bombardment of an evaporation source of solid aluminum flakes 41. For the coating of aluminum oxide, some oxygen can also be injected into the plasma chamber via an inlet.
[0207] Figure 5a An embodiment of a packaging container 50a produced with a packaging laminate according to the present invention is shown. The packaging container is particularly suitable for beverages, sauces, soups, etc. Typically, such a package has a volume of about 100 to 1000 ml. It can be of any structure, but is preferably brick-shaped, with longitudinal and transverse seals 51a and 52a, respectively, and optionally with an opening device 53. In another embodiment not shown, the packaging container can be formed into a wedge shape. In order to obtain such a "wedge shape", only the bottom part of the package is folded into shape so that the transverse heat seal at the bottom is hidden under the triangular flap, which is folded and sealed to the bottom of the package. The top transverse seal remains in the unfolded state. In this way, the packaging container, which is only partially folded, is still easy to handle and is stable enough in size to be placed on a shelf in a food store or on any flat surface,
[0208] Figure 5b An alternative example of a packaging container 50b produced with an alternative packaging laminate according to the present invention is shown. The alternative packaging laminate is thinner due to the thinner paper body layer, so it is not dimensionally stable enough to form a parallelepiped or wedge-shaped packaging container and is not folded into shape after the transverse seal 52b. The packaging container will remain a pillow-shaped bag-like container and be distributed and sold in this form.
[0209] Figure 5c A mountain-top package 50c is shown which is formed from a pre-cut sheet or blank, folded from a laminated packaging material comprising a paperboard bulk layer and a barrier-coated paper substrate of the present invention. Flat-top packages may also be made from similar blanks.
[0210] Figure 5d A bottle-shaped package 50d is shown which is a combination of a sleeve 54 formed from a pre-cut blank of the laminated packaging material of the present invention and a top 55 formed from injection-moulded plastic combined with an opening device such as a screw plug or the like. This type of package is marketed for example under the trade name Tetra and Tetra These particular packages are formed by attaching a molded top 55 with an attached opening device in a closed position to a tubular sleeve 54 of laminated packaging material, sterilizing the bottle-top capsule thus formed, filling it with the food product, and finally folding-forming the bottom of the package and sealing it.
[0211] Figure 6 The principle described in the introduction of the present application is shown, i.e. a web of packaging material is formed into a tube 61 by overlapping the longitudinal edges 62, 62' of the web and heat-sealing them to each other to thereby form an overlapping joint 63. The tube is continuously filled 64 with the liquid food to be filled and is divided into individual filled packages by repeated double transverse seals 65 of the tube, which are below the level of the contents filled in the tube and at a predetermined distance from each other. The packages 66 are separated by cutting between the double transverse seals (top seal and bottom seal) and are finally formed into the desired geometric configuration by folding along prepared crease lines in the material.
[0212] As a final remark, the invention is not limited to the embodiments shown and described above, but may vary within the scope of the claims.
Claims
1. A method for producing a paper-based or cellulose-based substrate (10a; 10b) coated with a barrier layer for packaging oxygen-sensitive products, the method comprising the following steps: a) conveying a web of a paper-based or cellulose-based substrate at a line speed of 300 m / min or more, The paper-based or cellulose-based substrate web is selected to have a web weight of 30 to 70 g / m2 as measured according to ISO 536:2012. 2 The grammage and the thickness of the fabric are 800 kg / m2 as measured according to ISO 534:2011. 3 Up to 1400kg / m 3 The surface of the top side of the paper-based or cellulose-based substrate exhibits a Bendtsen roughness value of less than 130 ml / min measured according to ISO 8791:4 and a roughness of less than 30 g / m2 measured according to ISO 535. 2 Cobb 60, b) providing an aqueous solution of a gas barrier polymer selected from the group consisting of vinyl alcohol polymers, PVOH, ethylene vinyl alcohol copolymers, EVOH and modified such PVOH and EVOH polymers, the aqueous solution having a solids content of 5 to 15 wt. % and a viscosity of 10 to 120 mPa*s, c) applying the aqueous solution of the gas barrier polymer to the surface of the top side of the web of the paper-based or cellulose-based substrate by roll coating to provide a dry weight of 0.5 to 2 g / m 2 A uniform coating, d) drying the aqueous gas barrier polymer coating applied in step c) while maintaining the surface temperature of the web substrate at a constant level below 60° C. to 95° C., e) repeating steps c) and d) at least once, f) optionally, further coating the dried web substrate coated with the aqueous solution of the gas barrier polymer obtained in step e) with a nanometer thick barrier deposited coating of metal and / or metal oxide by means of physical vapor deposition, Thereby a barrier-coated paper-based or cellulose-based substrate is obtained which has minimal defects in the gas barrier coating as well as in the deposited coating of the metal and / or metal oxide.
2. The method according to claim 1, wherein the roll coating method is a rotogravure coating method, such as a reverse rotogravure coating method.
3. The method according to any one of claims 1-2, wherein the aqueous solution of PVOH or EVOH has a solid content of 7 to 13 wt. %, such as 9 to 13 wt. %, such as 10 to 12.5 wt. % solid content.
4. The method according to any one of the preceding claims, wherein the aqueous solution of PVOH or EVOH has a viscosity of 50 to 100 mPa*s.
5. The method according to any one of the preceding claims, wherein the surface of the top side of the paper-based or cellulose-based substrate exhibits a Bendtsen roughness value of less than 120 ml / min, such as less than 100 ml / min, such as less than 80 ml / min, such as less than 50 ml / min, such as less than 30 ml / min.
6. The method according to any one of the preceding claims, wherein the surface of the top side of the paper-based or cellulose-based substrate exhibits a Bendtsen roughness value of less than 30 ml / min and a roughness value of 25 g / m 2 Or lower Cobb 60 absorption value.
7. The method according to any one of the preceding claims, wherein steps c) and d) are repeated once in step e) and each coating step applies a dry weight of 0.5 to 1 g / m 2 coating.
8. The method according to any one of the preceding claims, wherein in each drying step d), the temperature of the surface of the web substrate is always kept below 65°C to 95°C, such as below 65°C to 90°C, such as below 70°C to 90°C, such as 70°C to 85°C, such as 70°C to 80°C.
9. A method according to any one of the preceding claims, wherein the barrier deposited coating (14) is an aluminium metallisation coating applied to an optical density OD of 1.8 or higher, such as 1.8 to 3.5, such as 2.0 to 3.0, preferably 2.1 to 2.6, measured as described herein.
10. The method according to any of the preceding claims, wherein said surface of said top side of said paper-based or cellulose-based substrate further exhibits a Gurley porosity value according to Tappi T460 om-2 of greater than 1000 s / dl, such as greater than 2000 s / dl.
11. The method according to any one of the preceding claims, wherein the web of paper-based or cellulose-based substrate has a g / m 2 Weight, for example 35 to 50 g / m 2 , for example 35 to 45 g / m 2 Weight.
12. A method according to any one of the preceding claims, wherein the barrier polymer is selected from the group consisting of PVOH of this type having a degree of saponification of at least 98 mol%, such as at least 99 mol%.
13. A laminated packaging material (10a; 10b; 20a; 20b; 20c) comprising a cellulose-based substrate (11-12; 11-12-14; 25a; 25b; 25c) coated with a barrier layer manufactured according to the method of any one of claims 1 to 12, further comprising a first outermost protective material layer (22a; 22b; 22c) and a second innermost liquid-tight heat-sealable material layer (23a; 23b; 23b'; 23c), wherein: Such a laminated packaging material has an oxygen transmission value of 0.5 cm2 at 50% RH, 24 h, and 0.2 atm oxygen as measured according to ASTM F1927-14. 3 / m 2 or lower, the oxygen barrier is provided by a paper-based or cellulose-based substrate coated with a barrier layer after lamination.
14. A laminated packaging material according to claim 13, wherein the second innermost liquid-tight heat-sealable material layer (23a; 23b; 23b'; 23c) comprises a thermoplastic polymer, such as a polyolefin polymer, such as a polyethylene from a lower density range, the thermoplastic polymer being for example selected from the group consisting of LDPE, LLDPE, m-LLDPE and any mixture of two or more thereof.
15. Laminated packaging material according to claim 13, wherein the first outermost protective material layer (22a; 22b; 22c) and the second innermost liquid-tight heat-sealable material layer (23a; 23b; 23b'; 23c) both comprise a thermoplastic polymer, such as a polyolefin polymer, such as polyethylene.
16. The laminated packaging material (20a; 20b; 20c) according to any one of claims 13 to 15, further comprising a main body layer (21a; 21b; 21c) of paper or paperboard or other cellulose-based material, and the cellulose-based substrate (10a; 10b; 25a; 25b; 25c) coated with a barrier layer is arranged on the inner side of the paper or paperboard main body layer, between the main body layer and the second innermost liquid-tight heat-sealable material layer (23a; 23b; 23b'; 23c).
17. A laminated packaging material (20a; 20b; 20c) according to claim 16, wherein the cellulose-based substrate (10a; 10b; 25a; 25b; 25c) coated with a barrier layer is bonded to the main layer (21a; 21b; 21c) via an intermediate adhesive layer (26a; 26b; 26c) comprising an adhesive from an aqueous composition, the aqueous composition comprising an adhesive selected from the group consisting of acrylic acid polymers and copolymers, starch, cellulose and polysaccharide derivatives, polymers and copolymers of vinyl acetate and / or vinyl alcohol.
18. A laminated packaging material (20a; 20b; 20c) according to any one of claims 14-17, wherein the second innermost liquid-tight heat-sealable polyolefin layer (23a; 23b; 23b'; 23c) is a prefabricated polyolefin film comprising at least one layer of a majority of LLDPE polymer, such as a biaxially oriented polyethylene film, for improving the robustness of the mechanical properties of the laminated packaging material.
19. Packaging container (50a; 50b; 50c; 50d) comprising a laminated packaging material as defined in any one of claims 13 to 18.
Citation Information
Cited By
Medical high-barrier easy-to-tear composite film and preparation method thereof
CN121403799A