Copper-clad steel wire
By using a combination of austenitic stainless steel core wire and nickel-copper cladding in copper-clad steel wire, and combining wire drawing processing to form a martensite surface layer, the problem of cladding peeling is solved and the corrosion resistance of copper-clad steel wire is achieved , balance strength and conductivity and connection stability.
Patent Information
- Application Number
- CN202380028134.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-30
- Filing Date
- 2023-01-16
- Publication Date
- 2024-11-01
AI Technical Summary
The existing copper-clad steel wires are prone to peeling the cladding layer when connecting the crimp terminals, resulting in reduced connection strength and corrosion of the core wire, making it difficult to take into account both corrosion resistance, strength and conductivity.
Austenitic stainless steel is used as the core wire, and martensite structure is formed as the surface layer by drawing, and a first cladding layer composed of nickel and a second cladding layer composed of copper or copper alloy is ensured to ensure consistency of the crystal structure to suppress cladding. The cladding is peeled off and the cladding thickness and core outer diameter are optimized for improved adhesion.
The peeling of the cladding layer is effectively suppressed, and the corrosion resistance, strength and conductivity of the copper-clad steel wire are achieved, and the stability of the connection with the crimp terminal is improved.
Smart Images

Figure CN118891687A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to copper clad steel wire.
[0002] This application claims the benefit of priority based on Japanese Application No. 2022-87545 filed on May 30, 2022, and all the contents described in the above Japanese Application are incorporated herein by reference. Background Art
[0003] When both strength and conductivity are required in an electric wire, a copper-clad steel wire including a core wire made of steel and a coating layer made of copper (Cu) or a copper alloy is sometimes used (for example, see Japanese Patent Application Laid-Open No. 1-289021 (Patent Document 1), Japanese Patent Application Laid-Open No. 2002-270039 (Patent Document 2), and Japanese Patent Application Laid-Open No. 2020-021620 (Patent Document 3)). The core wire made of steel contributes to improved strength, and the coating layer made of copper or a copper alloy is responsible for high conductivity.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 1-289021
[0007] Patent Document 2: Japanese Patent Application Publication No. 2002-270039
[0008] Patent Document 3: Japanese Patent Application Publication No. 2020-021620 Summary of the invention
[0009] The copper-clad steel wire according to the present disclosure comprises: a core wire including austenitic stainless steel; a first coating layer covering the outer peripheral surface of the core wire and composed of Ni; and a second coating layer covering the outer peripheral surface of the first coating layer and composed of copper or a copper alloy. The core wire comprises: an austenite layer arranged so as to constitute the outer peripheral surface of the core wire and having a thickness of 1 μm or more and 10 μm or less, in which the volume fraction of the austenite structure is 80% or more; and a martensite layer arranged on the inner peripheral side of the austenite layer, in which the volume fraction of the martensite structure is 80% or more. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 It is a schematic diagram showing the structure of a copper-clad steel wire.
[0011] Figure 2 It is a schematic cross-sectional view showing the structure of a copper-clad steel wire.
[0012] Figure 3 This is a flowchart schematically showing a method for producing a copper-clad steel wire.
[0013] Figure 4 This is a photograph showing an example of a cross section of a sample in which no peeling occurred in a compression test.
[0014] Figure 5 This is a photograph showing an example of a cross section of a sample in which peeling occurred during a compression test. DETAILED DESCRIPTION
[0015] [Technical Problems to be Solved by the Present Disclosure]
[0016] Depending on the use environment of the above-mentioned copper-clad steel wire, corrosion resistance is sometimes required. In this case, as the steel constituting the core wire, austenitic stainless steel with excellent corrosion resistance can be used. At this time, a first coating layer composed of nickel (Ni) is formed on the surface of the core wire, and a second coating layer composed of copper or a copper alloy is formed on the first coating layer. The surface of the core wire including austenitic stainless steel is covered with a passivation film. Therefore, if a coating layer composed of copper or a copper alloy is directly formed on the surface of the core wire, sufficient adhesion between the core wire and the coating layer cannot be obtained. By adopting a first coating layer composed of nickel that can be tightly bonded to both the core wire including austenitic stainless steel and the second coating layer composed of copper or a copper alloy, it is possible to prevent the coating layer from peeling off from the core wire.
[0017] However, even when the first coating layer made of nickel is used, the coating layer may be peeled off from the core wire when the copper-clad steel wire is compressed by the crimping terminal. As a simple connection method, connection with the crimping terminal is important for the copper-clad steel wire. When the coating layer is peeled off, there are concerns about reduced strength of the connection portion with the crimping terminal and gap corrosion of the core wire.
[0018] Therefore, one of the objects of the present disclosure is to provide a copper-clad steel wire that has corrosion resistance, achieves a balance between strength and conductivity, and can suppress peeling of the coating layer when connected to a crimping terminal.
[0019] [Effects of the present disclosure]
[0020] According to the copper-clad steel wire described above, it is possible to provide a copper-clad steel wire that has corrosion resistance, achieves a balance between strength and conductivity, and can suppress peeling of the coating layer when connected to a crimping terminal.
[0021] [Description of Embodiments of the Present Disclosure]
[0022] First, the implementation aspects of the present disclosure are listed for explanation. The copper-clad steel wire of the present disclosure comprises: a core wire including austenitic stainless steel; a first coating layer covering the outer peripheral surface of the core wire and composed of Ni; and a second coating layer covering the outer peripheral surface of the first coating layer and composed of copper or a copper alloy. The core wire comprises: an austenite layer configured in a manner constituting the outer peripheral surface of the core wire and having a thickness of 1 μm or more and 10 μm or less, in which the volume fraction of the austenite structure is 80% or more; and a martensite layer configured on the inner peripheral side of the austenite layer, in which the volume fraction of the martensite structure is 80% or more.
[0023] The inventors of the present invention have studied a scheme for suppressing the peeling of the coating layer when connected to a crimping terminal. As a result, it was found that the peeling of the coating layer can be suppressed by making the surface part of the core wire, which is usually a structure composed mainly of martensite structure (process-induced martensite structure) through wire drawing, a structure composed mainly of austenite structure. This can be considered to be based on the following reasons. Usually, through wire drawing, the surface part of the core wire becomes a structure composed mainly of process-induced martensite structure. The crystal structure of the process-induced martensite structure is a body-centered tetragonal lattice with a lattice constant of 0.284 to 0.296 nm. In contrast, the crystal structure of Ni constituting the first coating layer is a face-centered cubic lattice with a lattice constant of 0.352 nm. Thus, the crystal structure is different between the surface layer of the core wire and the first coating layer, and the difference in lattice constant is also large, which is considered to be the cause of the peeling of the coating layer when connected to the crimping terminal. On the other hand, the crystal structure of the austenite structure is a face-centered cubic lattice with a lattice constant of 0.364nm. By making the surface layer of the core wire mainly composed of austenite, the crystal structure between the surface layer of the core wire and the first coating layer is consistent and the difference in lattice constant is small, thereby suppressing peeling of the coating layer when connected to the crimping terminal.
[0024] In the copper-clad steel wire of the present invention, excellent corrosion resistance is ensured by adopting austenitic stainless steel as the steel constituting the core wire. In addition, the steel core wire, especially the high-strength martensite layer, contributes to improving the strength. Furthermore, the second coating layer composed of copper or a copper alloy is responsible for high conductivity. In addition, an austenite layer having a thickness of 1 μm or more and 10 μm or less and a volume fraction of an austenite structure of 80% or more is arranged in a manner constituting the outer peripheral surface of the core wire. As a result, peeling of the coating layer when connected to the crimping terminal is suppressed. In this way, according to the copper-clad steel wire of the present invention, it has corrosion resistance, achieves a balance between strength and conductivity, and can suppress peeling of the coating layer when connected to the crimping terminal.
[0025] In the above-mentioned copper-clad steel wire, the outer diameter of the core wire may be greater than 0.05 mm and less than 1 mm. When the outer diameter of the core wire is less than 0.05 mm, the proportion of the austenite layer in the core wire becomes larger. As a result, it is difficult to ensure sufficient strength. On the other hand, when the outer diameter of the core wire exceeds 1 mm, it is difficult to set the manufacturing conditions such that the thickness of the austenite layer is greater than 1 μm and less than 10 μm. By setting the outer diameter of the core wire to greater than 0.05 mm and less than 1 mm, it is easy to manufacture the above-mentioned copper-clad steel wire with sufficient strength. It should be noted that in the present application, "wire diameter" refers to its diameter when the cross-section perpendicular to the length direction is circular. When the above-mentioned cross-section is other than the diameter of a circle, it refers to the diameter of the circle circumscribed to the cross-section.
[0026] In the above-mentioned copper-clad steel wire, the thickness of the first coating layer may also be greater than 0.001 μm and less than 50 μm. By setting the thickness of the first coating layer to be greater than 0.001 μm, it is possible to more reliably obtain adhesion with the second coating layer. On the other hand, with regard to the thickness of the first coating layer, even if it is thickened to more than 50 μm, the effect will be saturated. Therefore, the thickness of the first coating layer is preferably less than 50 μm, and may also be less than 30 μm. From the perspective of more reliably obtaining adhesion with the second coating layer, the thickness of the first coating layer is preferably greater than 0.015 μm.
[0027] The tensile strength of the copper-clad steel wire may be 600 MPa or more and 2500 MPa or less. By setting the tensile strength to 600 MPa or more, it is easy to obtain sufficient strength as a copper-clad steel wire, especially as a copper-clad steel wire used as an electric wire. By setting the tensile strength to 2500 MPa or less, it is easy to ensure sufficient toughness. The tensile strength of the copper-clad steel wire is preferably 900 MPa or more. The tensile strength of the copper-clad steel wire is preferably 2200 MPa or less.
[0028] The electrical conductivity of the copper-clad steel wire may be 20% IACS or more and 80% IACS or less. In this way, a copper-clad steel wire particularly suitable for use as an electric wire can be easily obtained.
[0029] In the copper-clad steel wire, the austenitic stainless steel constituting the core wire may be SUS301 (SUS301-CSP), SUS304 or SUS316 of JIS standard. From the viewpoint of strength and corrosion resistance, SUS301, SUS304 and SUS316 are preferred as the material constituting the core wire. It should be noted that in the present application, the austenitic stainless steel means steel having a component composition specified in JIS G4308 and JIS G4313 of JIS standard (Japan Industrial Standard).
[0030] [Details of the embodiments of the present disclosure]
[0031] Next, embodiments of the copper-clad steel wire according to the present disclosure will be described below with reference to the accompanying drawings. It should be noted that in the following drawings, the same or corresponding parts are denoted by the same reference numerals, and their description will not be repeated.
[0032] Figure 1 It is a schematic diagram showing the structure of a copper-clad steel wire. Figure 2 It is a schematic cross-sectional view showing the structure of a copper-clad steel wire. Figure 2 It is a cross-sectional view of the copper-clad steel wire taken along a plane perpendicular to the longitudinal direction, showing the vicinity of the first coating layer in an enlarged manner.
[0033] Reference Figure 1 and Figure 2 The copper-clad steel wire 1 in this embodiment includes a core wire 10, a first coating layer 30, and a second coating layer 20. The shape of the cross section of the copper-clad steel wire 1 perpendicular to the longitudinal direction is circular. The core wire 10 includes austenitic stainless steel. As the austenitic stainless steel constituting the core wire 10, for example, SUS301, SUS304, or SUS316 can be used. The outer diameter of the core wire 10 can be set to, for example, 0.05 mm or more and 1 mm or less. The shape of the cross section of the core wire 10 perpendicular to the longitudinal direction is circular.
[0034] The first coating layer 30 is arranged in a manner covering the entire area of the outer peripheral surface 10A of the core wire 10. The first coating layer 30 is in contact with the outer peripheral surface 10A of the core wire 10 at the inner peripheral surface 30A. The first coating layer 30 is composed of Ni. The thickness of the first coating layer 30 can be set to, for example, 0.001 μm or more and 50 μm or less. The first coating layer 30 can also be a plating layer formed by plating, for example. In the present embodiment, the second coating layer 20 is composed of pure Ni (composed of Ni and unavoidable impurities).
[0035] The second coating layer 20 is arranged in a manner covering the entire area of the outer peripheral surface 30B of the first coating layer 30. The second coating layer 20 is in contact with the outer peripheral surface 30B of the first coating layer 30 at the inner peripheral surface 20A. The second coating layer 20 is composed of Cu or a Cu alloy. The thickness of the second coating layer 20 can be set to, for example, 5 μm or more and 150 μm or less. The second coating layer 20 can also be a plated layer formed by plating, for example. The second coating layer 20 can also be a Cu-plated layer. That is, the second coating layer 20 can also be composed of pure copper (or copper and unavoidable impurities). In the present embodiment, the second coating layer 20 constitutes the surface (outer peripheral surface) of the copper-clad steel wire 1. In other embodiments, a surface layer composed of one or more metals selected from the group consisting of gold, silver, tin, palladium and nickel can also be formed to constitute the surface (outer peripheral surface) of the copper-clad steel wire 1.
[0036] Reference Figure 2 The core wire 10 includes an austenite layer 12 and a martensite layer 11. The austenite layer 12 is arranged so as to constitute the outer peripheral surface 10A of the core wire 10. The entire area of the outer peripheral surface 10A of the core wire 10 is composed of the austenite layer 12. The austenite layer 12 is a layer in which the volume ratio of the austenite structure is 80% or more. The thickness of the austenite layer 12 is 1 μm or more and 10 μm or less.
[0037] The martensite layer 11 is arranged on the inner side of the austenite layer 12. The martensite layer 11 is a layer in which the volume fraction of the martensite structure is more than 80%. Between the martensite layer 11 and the austenite layer 12, an intermediate layer in which the volume fraction of the martensite structure and the volume fraction of the austenite structure are both less than 80 volume % may also be formed. In the present embodiment, the martensite layer 11 constitutes the entire area of the inner side of the austenite layer 12 (or the inner side of the intermediate layer). The martensite layer 11 constitutes the core of the core wire 10. Preferably, the martensite layer 11 occupies more than 80 volume % in the core wire 10. It should be noted that the presence of the martensite layer 11 and the austenite layer 12 can be confirmed, for example, by performing an X-ray diffraction analysis on a cross section of the core wire 10 perpendicular to the length direction, based on the peaks corresponding to the austenite structure and the peaks corresponding to the martensite structure.
[0038] In the copper-clad steel wire 1 of the present embodiment, excellent corrosion resistance is ensured by adopting austenitic stainless steel as the steel constituting the core wire 10. In addition, the steel core wire 10, in particular, the high-strength martensite layer 11 contributes to improved strength. Furthermore, the second coating layer 20 composed of copper or a copper alloy is responsible for high conductivity. In addition, the austenite layer 12 is arranged so as to constitute the outer peripheral surface 10A of the core wire 10. Thus, peeling of the coating layers 20 and 30 when connected to the crimping terminal is suppressed. In this way, the copper-clad steel wire 1 of the present embodiment is a copper-clad steel wire that has corrosion resistance, achieves both strength and conductivity, and can suppress peeling of the coating layer when connected to the crimping terminal.
[0039] The tensile strength of the copper-clad steel wire 1 is preferably 600 MPa or more and 2500 MPa or less. By setting the tensile strength to 600 MPa or more, it is easy to obtain sufficient strength as a copper-clad steel wire, especially as a copper-clad steel wire used as an electric wire. By setting the tensile strength to 2500 MPa or less, it is easy to ensure sufficient toughness.
[0040] The electrical conductivity of the copper-clad steel wire 1 is preferably 20% IACS or more and 80% IACS or less. In this way, the copper-clad steel wire 1 can be made particularly suitable for use as an electric wire.
[0041] Then, mainly based on Figure 3 An example of a method for producing the copper-clad steel wire 1 will be described. Figure 3In the method for manufacturing the copper-clad steel wire 1 of the present embodiment, first, as step S10, a raw steel wire preparation step is performed. In this step S10, a raw steel wire to be the core wire 10 is prepared. Specifically, for example, a steel wire having a component composition corresponding to JIS standard SUS301, SUS304, or SUS316 is prepared. The outer diameter of the raw steel wire can be set to, for example, 0.1 mm or more and 2 mm or less.
[0042] Next, as step S20, a wire drawing step is performed. In this step S20, the raw steel wire prepared in step S10 is subjected to wire drawing (drawing). The processing degree (cross-sectional reduction ratio) in the wire drawing of step S20 can be set to, for example, 90% or more and 98% or less. The wire drawing process can also be performed in multiple times.
[0043] In this step S20, a martensite layer 11 and an austenite layer 12 are formed. The raw steel wire prepared in step S10 has a structure mainly composed of austenite in the entire region. As described above, by setting the cross-sectional reduction rate in step S20 to a high value, the region including the core portion can be made into a martensite layer 11. On the other hand, in order to form the austenite layer 12, in step S20, it is necessary to make the surface of the raw steel wire higher than usual, specifically, 200°C or more, so as to suppress the processing-induced martensite transformation in the surface portion. In order to make the surface of the raw steel wire 200°C or more, for example, it is possible to adjust the processing conditions such as increasing the cross-sectional reduction rate each time when the wire drawing process is performed in multiple times, increasing the die half angle of the die used for wire drawing within the processable range, and increasing the wire drawing speed within the processable range. In addition, the surface temperature of the raw steel wire can also be adjusted by a heating unit prepared separately. By performing step S20 as described above, the core wire 10 including the martensite layer 11 and the austenite layer 12 can be obtained.
[0044] Next, a first coating layer forming step is performed as step S30. In step S30, a first coating layer 30 made of Ni is formed to cover the surface of the core wire 10 obtained in step S20. Specifically, for example, the first coating layer 30 having a desired thickness can be formed by Ni impact plating.
[0045] Next, as step S40, a second coating layer forming step is performed. In this step S40, the second coating layer 20 composed of Cu or a Cu alloy is formed so as to cover the surface of the first coating layer 30 formed in step S30. Specifically, for example, by performing Cu plating, the second coating layer 20 having a desired thickness can be formed. Through the above process, the copper-clad steel wire 1 of this embodiment can be easily manufactured.
[0046] Example
[0047] An experiment was conducted to confirm whether the coating layer of the copper-clad steel wire disclosed in the present invention peeled off during processing that assumes connection with a crimping terminal. The experimental procedure is as follows.
[0048] First, a copper-clad steel wire 1 was produced by the same steps as those in the above-mentioned embodiment. As a raw steel wire, a steel wire made of JIS standard SUS304 was prepared. As the second coating layer 20, a pure Cu layer was formed by plating. A plurality of samples (embodiments) were produced in which the outer diameter of the core wire 10 and the thickness of the second coating layer 20 were changed. On the other hand, the conditions of the wire drawing process in step S20 were changed, and a sample (comparative example) in which an austenite layer 12 having a volume fraction of an austenite structure of 80% or more was not present was also produced. Then, the electrical conductivity, tensile strength, and the proportion of the austenite structure at a depth of 5 μm from the outer peripheral surface 10A of the core wire 10 of each sample were confirmed, and a compression test of the copper-clad steel wire 1 was carried out. The compression test was carried out under the condition that the copper-clad steel wire 1 was compressed in the radial direction and the load was released at a time point when the height became 40% of the original outer diameter. Then, the peeling of the coating layers 30 and 20 after the compression test was observed.
[0049] Figure 4 This is a photograph showing an example of a cross section of a sample in which no peeling occurred in a compression test. Figure 5 This is a photograph showing an example of a cross section of a sample in which peeling occurred during a compression test. Figure 4 and Figure 5 , will be like Figure 4 The samples without a gap G formed between the core wire 10 and the second coating layer 20 were judged as having no peeling. Figure 5 The samples in which the gap G was formed were judged to have peeled. Table 1 shows the conditions and results of the experiment.
[0050] [Table 1]
[0051]
[0052] Referring to Table 1, samples A to I correspond to the embodiments of the present disclosure, and samples J to L correspond to comparative examples that do not satisfy the conditions of the present disclosure. Regarding the electrical conductivity, since the second coating layer 20 made of pure Cu is responsible for the electrical conductivity, it is confirmed that the electrical conductivity depends on the area ratio of the second coating layer 20 in the cross section perpendicular to the length direction of the copper-clad steel wire 1. In addition, regarding the tensile strength, since the core wire 10 is responsible for the tensile strength, it is confirmed that the tensile strength depends on the outer diameter of the core wire 10. In addition, regarding samples J to L in which the core wire 10 does not have an austenite layer 12, peeling occurred during the compression test. On the other hand, regarding samples A to I in which the core wire 10 has an austenite layer 12, peeling did not occur regardless of the wire diameter, electrical conductivity, and tensile strength. It is thus confirmed that according to the copper-clad steel wire of the present disclosure, by providing the core wire 10 with an austenite layer 12, peeling of the coating layer when connected to the crimping terminal can be suppressed.
[0053] It should be understood that the embodiments and examples disclosed herein are illustrative in all respects and are not restrictive in any respect. The scope of the present invention is defined not by the above description but by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims.
[0054] Description of Reference Numerals
[0055] 1 copper clad steel wire, 10 core wire, 10A outer peripheral surface, 11 martensite layer, 12 austenite layer, 20 second coating layer, 20A inner peripheral surface, 30 first coating layer, 30A inner peripheral surface, 30B outer peripheral surface, G gap.
Claims
1. A copper-clad steel wire having: Core wire, including austenitic stainless steel; a first coating layer covering the outer peripheral surface of the core wire and composed of Ni; and a second coating layer, covering the outer peripheral surface of the first coating layer and composed of copper or a copper alloy, The core wire comprises: an austenite layer configured to constitute the outer peripheral surface of the core wire and having a thickness of 1 μm to 10 μm, wherein the volume ratio of the austenite structure in the austenite layer is 80% or more; and The martensite layer is arranged on the inner peripheral side of the austenite layer, and in the martensite layer, the volume ratio of the martensite structure is 80% or more.
2. The copper-clad steel wire according to claim 1, wherein: The outer diameter of the core wire is greater than or equal to 0.05 mm and less than or equal to 1 mm.
3. The copper-clad steel wire according to claim 1 or 2, wherein: The thickness of the first coating layer is greater than or equal to 0.001 μm and less than or equal to 50 μm.
4. The copper-clad steel wire according to any one of claims 1 to 3, wherein: The copper-clad steel wire has a tensile strength of 600 MPa or more and 2500 MPa or less.
5. The copper-clad steel wire according to any one of claims 1 to 4, wherein: The electrical conductivity of the copper-clad steel wire is greater than or equal to 20% IACS and less than or equal to 80% IACS.