Magnetic body and magnetic element
By using soft magnetic powder and a resin cured product with imide bond in the magnetic body, combining an inorganic insulating layer and a thermosetting resin composition, the problem of the existing magnetic body reducing heat resistance and strength in a high temperature environment is solved, and the problem of realizing the reduction of heat resistance and strength of the existing magnetic body is achieved. Long-term heat resistance and insulation performance under 180°C.
Patent Information
- Application Number
- CN202380027039.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-03-07
- Publication Date
- 2024-11-01
AI Technical Summary
It is difficult for the existing magnetic bodies to maintain long-term heat resistance and strength under a high temperature environment of 180°C, especially under long-term vibration conditions, and there are problems of lowering strength and decomposition of resin cured substances.
Magnetic bodies containing soft magnetic powder and resin cured substances are used. The resin cured substance has an imide bond and a polyesterimide structure. The soft magnetic powder is a Fe-Si alloy, and an inorganic insulating layer is added. The thermosetting resin composition includes polyester. The relative ratio of the resin is 2 to 6 parts by mass, ensuring excellent performance in the radial collapse strength, strength retention rate and volume resistivity after 1000 hours in an environment of 180°C.
The radial crushing strength after 1000 hours in a high temperature environment of 180°C is achieved, and the strength retention rate is more than 50%, the volume resistivity is more than 106Ωcm, the weight change rate is less than 1%, and the average length of the resin cured substance is The average distance between the diameter and the soft magnetic powder is controlled within a suitable range, ensuring the long-term heat resistance and insulation of the magnetic body.
Smart Images

Figure CN118891691A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a magnetic body and a magnetic element. Background Art
[0002] In recent years, with the electrification of automobiles, the demand for in-vehicle electronic components has gradually increased. In addition, in order to ensure the space inside the car, electronic components are arranged near the engine and motor, so their heat resistance is required to be further improved. Magnetic components used in electronic components also require higher heat resistance. In addition, in order to ensure the function of the inductor for a long time, long-term heat resistance in a high temperature environment of 180°C and the strength of the components under long-term vibration are required.
[0003] As one of the magnetic bodies used for magnetic elements, there is a so-called plastic magnet. A plastic magnet is a magnet formed by molding a binder resin in which soft magnetic metal powder is dispersed into a predetermined shape by injection molding or the like. With a plastic magnet, a magnetic body of a desired shape can be obtained relatively easily.
[0004] As one of the methods for improving the heat resistance of magnetic bodies, the selection of a binder resin having excellent heat resistance has been studied. For example, Patent Document 1 discloses a magnetic core using a composite fluororesin including a perfluororesin having excellent heat resistance.
[0005] In addition, research is underway to manufacture integrated magnetic components in which a coil is embedded in a magnetic body using a plastic magnet. For example, Patent Document 2 discloses a method for manufacturing an inductor in which a coil is placed in a cavity and then the cavity is filled with a composition containing a thermoplastic element and magnetic powder. An integrated inductor has the advantage of suppressing leakage flux without shielding.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2017-188680;
[0009] Patent document 2: Japanese Patent Application Publication No. 2019-102713. Summary of the invention
[0010] Problem that the invention aims to solve
[0011] An object of the present invention is to provide a magnetic body and a magnetic element having excellent long-term heat resistance in a high-temperature environment of 180°C.
[0012] Solutions for solving problems
[0013] The magnetic body of the present invention comprises soft magnetic powder and a cured resin.
[0014] The magnetic body has a radial crushing strength of 30 MPa or more after being kept in an environment of 180° C. for 1000 hours.
[0015] In one embodiment of the magnetic body, the strength retention rate after being kept in an environment of 180° C. for 1000 hours is 50% or more.
[0016] In one embodiment of the magnetic body, the volume resistivity after being kept at 180° C. for 1000 hours is 10 6 Ωcm or more.
[0017] In one embodiment of the magnetic body, the radial crushing strength after being kept in an environment of 180° C. for 1000 hours is 50 MPa or more.
[0018] In one embodiment of the magnetic body, the weight change rate after being kept in an environment of 180° C. for 1000 hours is 1% or less.
[0019] In one embodiment of the magnetic body, the average major diameter of pores in the cured resin material after being kept in an environment of 180° C. for 1000 hours is 2 μm or less.
[0020] In one embodiment of the magnetic body, after being kept in an environment of 180° C. for 1000 hours, an average distance between the soft magnetic powder and the cured resin is 1 μm or less.
[0021] In one embodiment of the magnetic substance, the cured resin has an imide bond.
[0022] In one embodiment of the magnetic body, the cured resin includes polyester imide.
[0023] In one embodiment of the magnetic body, the ratio of the resin cured material is 2 to 6 parts by mass based on 100 parts by mass of the soft magnetic powder.
[0024] In one embodiment of the magnetic body, the cured resin includes a cured product of a thermosetting resin composition, and the thermosetting resin composition includes a polyester-based resin, an epoxy-based resin, and a polyimide-based resin.
[0025] In one embodiment of the magnetic substance, the polyester-based resin has a carboxyl group.
[0026] In one embodiment of the magnetic body, the polyimide resin has olefinic double bonds.
[0027] In one embodiment of the magnetic body, the thermosetting resin composition further contains a peroxide.
[0028] In one embodiment of the magnetic body, the soft magnetic powder includes iron alloy powder.
[0029] In one embodiment of the magnetic body, the iron alloy powder includes a Fe—Si alloy.
[0030] In one embodiment of the magnetic body, the Fe—Si alloy contains 4 to 10 mass % of Si.
[0031] In one embodiment of the magnetic body, the iron alloy powder further includes one or more selected from Cr and Al.
[0032] In one embodiment of the magnetic body, the soft magnetic powder has an inorganic insulating layer on the surface.
[0033] In one embodiment of the magnetic body, the inorganic insulating layer includes one or more selected from phosphates and silicates.
[0034] In one embodiment of the magnetic body, the ratio of the inorganic insulating layer is 0.1 to 3 parts by mass based on 100 parts by mass of the soft magnetic powder.
[0035] In one embodiment of the magnetic body, the inorganic insulating layer has an average thickness of 10 to 100 nm.
[0036] In one embodiment of the magnetic body, the average particle size of the soft magnetic powder is 5 to 30 μm.
[0037] The magnetic element of the present invention comprises the magnetic body of the present invention and a coil embedded in the magnetic body.
[0038] Effects of the Invention
[0039] According to the present invention, a magnetic body and a magnetic element having excellent long-term heat resistance in a high-temperature environment of 180° C. can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a schematic cross-sectional view showing an example of a magnetic body.
[0041] Figure 2 is a schematic perspective view of a magnetic element according to one embodiment of the present invention.
[0042] Figure 3 To show Figure 2 Schematic cross-sectional view of section III-III.
[0043] Figure 4 This is a cross-sectional SEM image of the magnetic body of Example 5.
[0044] Figure 5This is a cross-sectional SEM image of the magnetic body of Example 6.
[0045] Figure 6 This is a cross-sectional SEM image of the magnetic body of Example 7.
[0046] Figure 7 This is a cross-sectional SEM image of the magnetic body of Example 8. DETAILED DESCRIPTION
[0047] Hereinafter, the present invention will be described based on the embodiments of the invention, but the invention of the claims is not limited to the following embodiments.
[0048] In order to make the description clear, the following description and drawings have been appropriately simplified. For the purpose of explanation, the scales of the components in the drawings are sometimes greatly different.
[0049] In addition, "to" indicating a numerical range includes the lower limit value and the upper limit value unless otherwise specified.
[0050] In the present invention, the "magnetic body immediately after production" includes a magnetic body stored at room temperature for about 24 hours after production of the magnetic body.
[0051] [Magnetic body]
[0052] Figure 1 This is a schematic cross-sectional view showing an example of a magnetic body. Figure 1 The magnetic body 10 of the example (hereinafter referred to as the present magnetic body) is a molded body having a soft magnetic powder 1 and a cured resin 2, wherein the soft magnetic powder 1 is dispersed in the cured resin 2.
[0053] The magnetic body is characterized in that the radial crushing strength after being kept at 180° C. for 1000 hours is 30 MPa or more, and the magnetic body is excellent in long-term heat resistance at a high temperature of 180° C. In the present embodiment, the radial crushing strength is a value obtained by the radial crushing strength test method of JIS Z2507.
[0054] The radial crushing strength of the magnetic body after being kept in an environment of 180° C. for 1000 hours is particularly preferably 40 MPa or more, more preferably 50 MPa or more.
[0055] The strength retention rate of the magnetic body after being kept in an environment of 180°C for 1000 hours is preferably 50% or more. Here, the strength retention rate is calculated based on the radial crushing strength K of the magnetic body just after production. 0 (MPa) and the radial crushing strength K (MPa) of the magnetic body after being kept in an environment of 180°C for 1000 hours are values calculated by the following formula (1).
[0056] Formula (1): Strength retention rate (%) = K / K0 ×100
[0057] From the viewpoint of heat resistance, the strength retention is particularly preferably 55% or more, preferably 60% or more. In addition, the radial crushing strength of the magnetic body immediately after production is preferably 60 MPa or more, more preferably 70 MPa or more, and even more preferably 80 MPa or more.
[0058] The present magnetic body preferably maintains insulation properties in a high temperature environment. From this point of view, the volume resistivity of the present magnetic body after being kept in an environment of 180°C for 1000 hours is preferably 10 6 Ωcm or more, more preferably 10 7 Ωcm or more.
[0059] In addition, the volume resistivity of the magnetic body just after production is preferably 10 6 Ωcm or more, more preferably 10 7 Ωcm or more, more preferably 10 8 Ωcm or more.
[0060] From the viewpoint of maintaining strength, the weight change rate of the magnetic body after being kept at 180°C for 1000 hours is preferably 1% or less, more preferably 0.9% or less, and further preferably 0.8% or less. Here, the weight change rate is calculated based on the weight W of the magnetic body just after production. 0 The weight W (g) of the magnetic body after being kept at 180°C for 1000 hours is calculated by the following formula (2).
[0061] Formula (2): Weight change rate (%) = |WW 0 | / W 0 ×100
[0062] Furthermore, from the viewpoint of maintaining strength, the present magnetic body preferably suppresses decomposition of the cured resin around the magnetic powder in a high temperature environment. Figure 5 This is a cross-sectional SEM image of the magnetic body of Example 6 below. Figure 5 As shown in FIG. 1 , the cured resin around the magnetic powder may decompose in a high temperature environment. In this case, the radial crushing strength tends to decrease significantly.
[0063] Specifically, from the viewpoint of maintaining strength, after the magnetic body is kept at 180°C for 1000 hours, the average distance between the soft magnetic powder and the cured resin is preferably 1 μm or less, more preferably 0.5 μm or less. Here, the average distance is the average value of the distance, taking the width of the gap between the magnetic body and the resin in the cross-sectional SEM image of the magnetic body as the distance.
[0064] In addition, from the viewpoint of maintaining strength, the magnetic body preferably suppresses the formation of large pores inside the resin cured product under high temperature environment. Specifically, from the viewpoint of maintaining strength, the average major diameter of the pores in the resin cured product after the magnetic body is kept at 180°C for 1000 hours is preferably 2 μm or less, more preferably 1.5 μm or less. When the average major diameter exceeds 2 μm, there is a tendency for the strength retention rate to decrease. Here, the above-mentioned average major diameter is the average value of the major diameters measured for each pore in the cross-sectional SEM image of the magnetic body.
[0065] The radial crushing strength of the magnetic body after being kept at 180° C. for 1000 hours is at least 30 MPa. The method for achieving the above-mentioned long-term heat resistance is not particularly limited, and it can be achieved by, for example, selecting the soft magnetic powder or resin cured product constituting the magnetic body.
[0066] Hereinafter, each component that can be contained in the present magnetic substance will be described.
[0067] <Soft magnetic powder>
[0068] Soft magnetic powder can be appropriately selected and used from materials showing soft magnetic properties. From the aspect of magnetic properties, it is preferred to include a material containing iron, which can be a single substance of iron or an alloy containing iron and other elements. As soft magnetic powder, it is preferred to include iron alloy powders such as carbonyl iron, Fe-Si alloy, Fe-Ni alloy, Fe-Si-Cr alloy, Fe-Si-Al alloy, Fe-based amorphous alloy powder containing at least Fe-B, and Fe-based nanocrystalline alloy containing at least Fe-BP-Cu. Here, the above-mentioned Fe-based amorphous alloy refers to an amorphous (amorphous) alloy that does not have a crystalline structure in the Fe-based alloy. In addition, the Fe-based nanocrystalline alloy refers to an alloy in which the above-mentioned Fe-based amorphous alloy is subjected to heat treatment and fine α-Fe crystals are precipitated in the amorphous phase. The soft magnetic powder can be used alone or in combination of two or more.
[0069] The iron alloy powder preferably contains Fe-Si alloy in order to suppress the oxidation of iron in the soft magnetic powder under high temperature environment and suppress the catalytic effect of iron generated at the contact surface between iron and resin cured product to suppress the thermal oxidation decomposition of resin cured product. In addition, by using Fe-Si alloy, a magnetic body with high magnetic permeability and low iron loss can be obtained.
[0070] The proportion of Si in the Fe-Si alloy is preferably 4 to 10% by mass relative to the total amount of the Fe-Si alloy. Furthermore, from the perspective of heat resistance of the magnetic body, the proportion of Si is preferably 4.5% by mass or more, and more preferably 5% by mass or more. On the other hand, from the perspective of being able to suppress the reduction of magnetic properties and suppress the hardness and brittleness of the Fe-Si alloy, the proportion of Si is preferably 10% by mass or less, preferably 8% by mass or less, and more preferably 7% by mass or less.
[0071] In addition, the Fe-Si alloy may also contain other elements such as Cr, Al, Mn, Ni, C, O, N, S, P, B, Cu, etc. From the aspect of heat resistance, it is preferred that the Fe-Si alloy powder contains one or more selected from Cr and Al. Cr and Al form a passivation layer on the surface of the Fe-Si alloy powder, so that the oxidation of the soft magnetic powder can be suppressed under high temperature environment, and the contact between the resin cured product and iron can be suppressed to suppress the oxidation of the resin cured product.
[0072] From the perspective of heat resistance and rust prevention, the ratio of Cr or Al in the Fe-Si alloy is preferably 0.5 to 10 parts by mass, more preferably 3 to 8 parts by mass in 100 parts by mass of the Fe-Si alloy powder. In addition, when both Cr and Al are contained, the total mass is preferably within the above range.
[0073] From the viewpoint of heat resistance and magnetic properties, the total content of elements other than Cr and Al is preferably 1 part by mass or less, and more preferably 0.5 part by mass or less, in 100 parts by mass of the soft magnetic powder.
[0074] The shape of the soft magnetic powder may be spherical, ellipsoidal, needle-like, rod-like, plate-like, etc., and spherical is preferred from the viewpoints of filling the mold during molding of the magnetic body and reducing the contact area with the cured resin.
[0075] Furthermore, from the viewpoint of heat resistance, the average particle size of the soft magnetic powder is preferably 1 to 100 μm, more preferably 3 to 60 μm, and further preferably 5 to 30 μm from the viewpoint of skin effect when used in a frequency band of 1 MHz or more.
[0076] The method for producing the soft magnetic powder is not particularly limited, and may be appropriately selected from known methods such as atomization, melt spinning, rotary electrode method, mechanical alloying, and chemical deposition based on reduction. From the aspect that spherical particles can be appropriately obtained, atomization is preferred. As atomization, for example, gas atomization, water atomization, centrifugal atomization, plasma atomization, etc. may be cited. From the viewpoint of mass production stability and productivity, gas atomization or water atomization is preferred, and from the aspect that powders below 30 μm are easily obtained, water atomization is preferred.
[0077] (Inorganic insulating layer)
[0078] The soft magnetic powder may further include an inorganic insulating layer. By including the inorganic insulating layer, it is possible to suppress the contact between the soft magnetic powders and ensure insulation, while suppressing the contact between the soft magnetic powders and the resin cured product and thus suppressing the thermal decomposition of the resin cured product. In addition, by using the inorganic insulating layer, the heat resistance of the insulating layer itself is further improved.
[0079] Examples of the insulating material of the inorganic insulating layer include SiO 2 (Silicic acid), Al 2 O 3 (aluminum oxide), ZrO 2 Inorganic oxides such as Si 3 N 4 , BN and other nitrides; glass materials such as silicate glass, boric acid glass, borosilicate glass, phosphate glass, bismuth glass, etc.; minerals such as mica and clay, especially preferably containing phosphates and silicates. The insulating material in the inorganic insulating layer can be used alone or in combination of two or more.
[0080] From the perspective of ensuring insulation resistance and suppressing oxidation of the cured resin, the inorganic insulating layer is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and further preferably 0.5 parts by mass or more, relative to 100 parts by mass of the soft magnetic powder. The inorganic insulating layer may be 3 parts by mass or less relative to 100 parts by mass of the soft magnetic powder, and from the perspective of magnetic properties, it is preferably 2.5 parts by mass or less, and more preferably 2.0 parts by mass or less.
[0081] From the viewpoint of ensuring insulation resistance and suppressing oxidation of the cured resin, the average thickness of the inorganic insulating layer is preferably 10 to 100 nm, more preferably 10 to 60 nm.
[0082] In addition, the thickness of the inorganic insulating layer can be obtained by observing the surface of the soft magnetic powder using a transmission electron microscope (TEM). In addition, for simplicity, it is possible to assume that the soft magnetic powder is a spherical particle of a single particle size, and use the specific surface area of the soft magnetic powder and the specific gravity of the insulating material to calculate the average thickness of the inorganic insulating layer according to the following formulas (3) and (4).
[0083] Formula (3): Specific surface area of soft magnetic powder (m 2 / g) = 6 / [specific gravity of soft magnetic powder (g / m 3 )×particle size of soft magnetic powder (m)]
[0084] Formula (4): Inorganic insulating layer thickness (m) = mass of insulating material (g) / [mass of soft magnetic powder (g) × specific surface area of soft magnetic powder (m 2 / g)×specific gravity of coating powder (g / m 3 )]
[0085] The method for providing the inorganic insulating layer on the soft magnetic powder can be appropriately selected from a powder mixing method, an impregnation method, a sol-gel method, a CVD method, a PVD method, or various known methods other than the above.
[0086] <Resin Cured Product>
[0087] The present magnetic body includes a cured resin. A cured resin is a cured resin used as a binder component. The resin only needs to be curable by a single component or multiple components, and examples thereof include thermosetting resins and photocurable resins. From the perspective of both processability during heat molding and heat resistance after manufacturing, the curable resin in the present magnetic body is preferably a thermosetting resin. In addition, in the present invention, a cured resin refers to a cured resin in which at least a portion of the curable resin undergoes a cross-linking reaction. Examples of the cured resin include cured epoxy resins, polyimides, polyamide-imides, and the like.
[0088] In view of excellent long-term heat resistance in a high-temperature environment, in the present magnetic body, the cured resin preferably has an imide bond (-C(=O)-NR-C(=O)-; wherein R is a hydrogen atom or an organic group). The cured resin having an imide bond can suppress the decomposition of the imide bond even in a high-temperature environment, is less likely to form voids, is less likely to reduce strength after long-term storage, and can maintain insulation properties.
[0089] From the perspective of further improving heat resistance, the cured resin preferably has polyesterimide. In the present invention, polyesterimide refers to a polyesterimide having two or more ester bonds and two or more imide bonds in the molecule. The cured resin having polyesterimide has a three-dimensional structure formed by cross-linking multiple polymer chains, and the cured resin has multiple ester bonds and imide bonds, respectively, thereby stabilizing the structure and further inhibiting thermal decomposition in a high temperature environment of 180°C.
[0090] The thermosetting resin as a precursor of the cured resin preferably forms a cured product containing a polyesterimide structure after curing. Among them, from the aspect of easy molding of the magnetic body at low temperature, a thermosetting resin composition containing a polyester resin, an epoxy resin and a polyimide resin is preferred. By using this thermosetting resin composition, the heating temperature during molding can be set to, for example, about 180°C.
[0091] The polyester resin can be appropriately selected from polymers of polycarboxylic acids and polyols and used. Among them, polyester resins having a carboxyl group are preferred from the viewpoint of reactivity with epoxy resins.
[0092] The polycarboxylic acid can be appropriately selected from compounds having two or more carboxylic acids in one molecule, and dicarboxylic acids having two carboxylic acids in one molecule or anhydrides thereof are particularly preferred.
[0093] Specific examples of dicarboxylic acids include terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid, succinic acid, adipic acid, maleic acid, etc., and one or more of them can be used alone or in combination. In the present invention, the polycarboxylic acid preferably contains one or more selected from isophthalic acid and maleic acid.
[0094] The polyol can be appropriately selected from compounds having two or more hydroxyl groups in one molecule. Specific examples of the polyol include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, diethylene glycol, dipropylene glycol, neopentyl glycol, 1,3-butanediol, trimethylolpropane, glycerol, 1,4-cyclohexanediol, cyclohexanedimethanol, bisphenol A, bisphenol F, etc., and these can be used alone or in combination of two or more.
[0095] The polyester resin is obtained by subjecting the above-mentioned polycarboxylic acid and polyol to a dehydration condensation reaction by a known method. In addition, a commercially available product having a desired structure may also be used.
[0096] The epoxy resin can be appropriately selected from compounds having one or more epoxy groups in one molecule. Preferred specific examples of epoxy resins include: Epi-Bis epoxy resins obtained by condensation reaction of bisphenol A, bisphenol F and their oxyalkylene modified products with epichlorohydrin; novolac epoxy resins obtained by condensation reaction of epichlorohydrin with phenolic resin; alkyl glycidyl ethers such as methyl glycidyl ether and butyl glycidyl ether, etc., which can be used alone or in combination of two or more.
[0097] The polyimide resin can be appropriately selected from compounds having two or more imide bonds in one molecule. Among them, from the aspect of crosslinking with other resins, a resin having an olefinic double bond is preferred, preferably N,N'-(4,4'-diphenylmethane) diallylnadiimide and N,N'-(m-xylylene) diallylnadiimide. The polyimide resin can be used alone or in combination of two or more.
[0098] From the viewpoint of heat resistance and mechanical strength of the obtained cured resin, the mixing ratio of the thermosetting resin composition is preferably 20 to 50 parts by mass of the polyester resin, 1 to 25 parts by mass of the epoxy resin, and 1 to 15 parts by mass of the polyimide resin.
[0099] The thermosetting resin composition may further contain other components, such as vinyl monomers, epoxy acrylates, curing agents, catalysts, and the like.
[0100] Examples of the vinyl monomer include monomers having a vinyl group, a (meth)acryloyl group, and the like, such as vinyl monomers such as vinyl acetate and styrene, and acrylic monomers such as methyl (meth)acrylate. In addition, a (meth)acryloyl group refers to an acryloyl group or a methacryloyl group, and the same applies to (meth)acrylate.
[0101] Examples of epoxy acrylates include compounds obtained by reacting a carboxyl group of (meth)acrylic acid with an epoxy group of various epoxy resins.
[0102] As a curing agent for accelerating the curing reaction of the thermosetting resin composition, peroxide is preferred. Specific examples of peroxides include dicumyl peroxide, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, 2,2-bis(tert-butyldioxy)octane, tert-butyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, α,α'-bis(tert-butylperoxy-m-isopropyl)benzene, tert-butyl-cumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane-3, etc.
[0103] Examples of the reaction catalyst between a carboxyl group and an epoxy group include imidazole and tertiary amines.
[0104] When a vinyl monomer or epoxy acrylate is added to the thermosetting resin composition, it is preferably added in such a ratio that the total of the polyester resin, epoxy resin and polyimide resin to the total of the vinyl monomer and epoxy acrylate is 1:3 to 3:1 in terms of mass ratio.
[0105] The present magnetic body can be obtained by, for example, dispersing soft magnetic powder in the above-mentioned thermosetting resin composition, filling it into a mold of a desired shape and heating it. The heating conditions also depend on the reactivity of the above-mentioned thermosetting resin composition, but by, for example, heating at 150 to 200° C. for about 0.5 to 12 hours, the crosslinking reaction can be fully carried out.
[0106] From the cured resin obtained by curing the thermosetting resin composition, ester bonds and imide bonds were detected, and in addition, hydroxyl groups derived from the reaction between epoxy groups and carboxyl groups were detected.
[0107] The mixing ratio of the thermosetting resin composition and the soft magnetic powder can be appropriately adjusted according to the purpose, for example, preferably 1 to 10 parts by mass, more preferably 2 to 6 parts by mass relative to 100 parts by mass of the soft magnetic powder. If it is above the above lower limit, the mechanical strength of the magnetic body is improved. On the other hand, if it is below the above upper limit, the magnetic properties are excellent.
[0108] The magnetic body can be used in known applications using magnetic bodies. Since the magnetic body has excellent long-term heat resistance in a high temperature environment of 180°C, it can be suitably used as a core material for inductors for automotive applications that require heat resistance, especially those arranged near engines.
[0109] Furthermore, when the thermosetting resin composition is used, the heat treatment temperature during molding can be set to a relatively low temperature of about 180° C., and thus it can be suitably used for coil-embedded magnetic element applications described later.
[0110] [Magnetic components]
[0111] Reference Figure 2 and Figure 3 An example of the magnetic element of the present invention (also referred to as the present magnetic element) will be described. Figure 2 is a schematic top perspective view of a magnetic element, Figure 3 for Figure 2 Schematic III-III cross-sectional view of. In addition, Figure 2 The terminal portion 12 is Figure 3 The terminal 12 is affixed to the magnetic body 10 using an adhesive member 13. The magnetic element comprises a magnetic body 10 and a coil 11 embedded in the magnetic body 10, and the magnetic body 10 is the magnetic body of the present invention described above. The magnetic element only needs to have at least the winding portion of the coil 11 embedded in the magnetic body 10, and a portion of the coil 11 may be exposed from the magnetic body 10. From the perspective of wettability of solder such as lead-free solder, the terminal portion 12 may include, for example, copper plated with Sn or the like. The copper of the terminal portion 12 may be joined to the coil 11 or may be integral.
[0112] The shape of the coil 11 is appropriately selected from coils known as coils used in magnetic elements, and generally has a winding portion and a terminal portion connected to a circuit, etc. The material of the coil 11 is not particularly limited, and can be, for example, a copper wire, etc., and the copper wire preferably has an insulating film. From the aspect of heat resistance, polyamide-imide film, polyimide film, etc. are preferred as the insulating film.
[0113] When manufacturing a coil-embedded magnetic element, in the above-mentioned method for manufacturing a magnetic body, the coil may be arranged in the mold before or when the mold is filled with the magnetic body.
[0114] Although not shown in the drawings, a magnetic element produced by winding a coil around the present magnetic body described above also has excellent long-term heat resistance in a high-temperature environment of 180°C.
[0115] The magnetic element can be suitably used as an inductor for a power inductor, a choke coil, a transformer, and the like.
[0116] Example
[0117] Hereinafter, the present invention will be specifically described with reference to Examples and Comparative Examples, but these descriptions do not limit the present invention.
[0118] (Example 1)
[0119] As the soft magnetic powder, a Fe-Si-Cr alloy containing 4.5 to 7 mass % of Si and 3 to 8 mass % of Cr and having an average particle size of 10 μm was prepared.
[0120] The soft magnetic powder is coated with a phosphoric acid-based inorganic insulating material in an amount equivalent to 0.5 parts by mass relative to 100 parts by mass of the soft magnetic powder to form an insulating layer (the thickness of the insulating layer is about 10 nm). The following thermosetting resin composition (1) is added to the soft magnetic powder having the insulating layer in an amount equivalent to 5 parts by mass relative to 100 parts by mass of the soft magnetic powder and kneaded to obtain an iron alloy powder coated with the thermosetting resin composition (1).
[0121] Thermosetting resin composition (1): a composition comprising a polyester resin, an epoxy resin and a polyimide resin.
[0122] The soft magnetic powder after the above treatment was passed through a 500 μm metal mesh to adjust the particle size so that it can be easily filled into the mold, and then granulated. The granulated powder was filled into a ring-shaped mold with an outer diameter of 13 mm and an inner diameter of 8 mm at a pressure of 5 tons / cm 2 The obtained ring-shaped sample was heat-cured at a temperature of 180° C. for 2 hours or more in a thermostatic chamber to obtain a magnetic body including a cured resin containing polyester imide.
[0123] (Example 2)
[0124] In Example 1, the magnetic body of Example 2 (the thickness of the insulating layer was about 50 nm) was obtained in the same manner as in Example 1 except that the amount of the phosphoric acid-based inorganic insulating material was changed to 1.5 parts by mass.
[0125] (Example 3)
[0126] A magnetic body of Example 3 was obtained in the same manner as in Example 1 except that the amount of the phosphoric acid-based inorganic insulating material was changed to 1.5 parts by mass and the amount of the thermosetting resin composition (1) was changed to 2 parts by mass relative to 100 parts by mass of the soft magnetic powder.
[0127] (Example 4)
[0128] In Example 1, the magnetic body of Example 4 was obtained in the same manner as in Example 1 except that the thermosetting resin composition was changed to a thermosetting phenolic resin.
[0129] (Example 5)
[0130] A magnetic body of Example 5 was obtained in the same manner as in Example 1 except that the insulating coating treatment was not performed.
[0131] (Example 6: Comparative Example)
[0132] In Example 5, the magnetic body of Example 6 was obtained in the same manner as in Example 5 except that the thermosetting resin composition was changed to a thermosetting phenolic resin.
[0133] (Example 7)
[0134] In Example 5, a magnetic body of Example 7 was obtained in the same manner as in Example 5 except that the thermosetting resin composition was changed to an epoxy resin having a glass transition temperature of 250° C. or higher (epoxy resin (1)).
[0135] (Example 8)
[0136] In Example 5, the magnetic body of Example 8 was obtained in the same manner as in Example 5 except that the thermosetting resin composition was changed to a bisphenol A type epoxy resin (epoxy resin (2)).
[0137] (Example 9)
[0138] In Example 1, the same procedures as in Example 1 were followed except that 0.5 parts by mass of the phosphoric acid-based inorganic insulating material was replaced with 1 part by mass of the silicate-based insulating material and the thermosetting resin composition was replaced with a thermosetting phenolic resin to obtain a magnetic body of Example 9 (the thickness of the insulating layer was about 30 nm).
[0139] (Example 10)
[0140] In Example 9, a magnetic body of Example 10 was obtained in the same manner as in Example 9 except that the soft magnetic powder was changed to a soft magnetic powder containing 6.5 mass % Si, 3 to 8 mass % Cr and having an average particle size of 10 μm.
[0141] (Example 11)
[0142] A magnetic body of Example 11 was obtained in the same manner as in Example 9 except that the soft magnetic powder was changed to a soft magnetic powder containing 0.5 mass % Si and 1 mass % Cr and having an average particle size of 10 μm.
[0143] <Evaluation of Magnetic Materials>
[0144] The magnetic body of each example was evaluated by the following method.
[0145] The volume resistivity of the magnetic body is calculated as follows: Using a resistance meter (B2985A) from Keysight, an electrode with a diameter of 1 mm is brought into contact with the top and bottom surfaces of a ring-shaped molded body with an outer diameter of 13 mm, an inner diameter of 8 mm, and a height of 5.0 mm to 6.0 mm, a voltage of 100 V is applied, and the insulation resistance is measured.
[0146] The radial crushing strength of the magnetic body was evaluated by performing a compression test in accordance with the radial crushing strength test method of JIS Z2507 and calculating it according to Formula (5).
[0147] Formula (5): K=[F×(De)] / (L×e 2 )
[0148] K: Radial crushing strength (MPa)
[0149] F: Maximum load at rupture (N)
[0150] L: Length of hollow cylinder (mm)
[0151] D: outer diameter of hollow cylinder (mm)
[0152] e: Wall thickness of hollow cylinder (mm)
[0153] (Heat resistance evaluation)
[0154] Heat resistance was evaluated as follows: After each magnetic body was stored in an atmosphere at 180°C for 1000 hours, the volume resistivity, radial crushing strength and weight were measured in the same manner as above. The results are shown in Table 1. In addition, when the value of the weight change rate is - (negative), it means that the weight has decreased.
[0155] In addition, the cross section of the magnetic body after storage at 180°C for 1000 hours was observed by SEM. The cross section SEM images of the magnetic bodies of Examples 5 to 8 are as follows: Figure 4 to Figure 7 shown.
[0156] [Table 1]
[0157]
[0158] Figure 5The cross-sectional SEM image of Example 6 is shown. It can be seen that when the magnetic body of Example 6, which is a combination of soft magnetic powder without an inorganic insulating layer and thermosetting phenolic resin, is stored at 180°C for 1000 hours, the resin around the soft magnetic powder is decomposed, and gaps are generated between the soft magnetic powder and the cured resin. As a result, the strength retention rate is particularly low.
[0159] Figure 6 and Figure 7 These are cross-sectional SEM images of Examples 7 and 8. It is shown that when the magnetic bodies of Examples 7 and 8 using epoxy resins were stored at 180°C for 1000 hours, voids were generated inside the cured resins. As a result, the strength retention rate was slightly reduced.
[0160] Figure 4 This is a cross-sectional SEM image of Example 5. It shows that when the magnetic body of Example 5 is stored at 180°C for 1000 hours, although pores are generated inside the cured resin, they do not expand and the mesh structure of polyesterimide is maintained. The magnetic body of Example 5 has a high strength retention rate after being stored at 180°C for 1000 hours, and also maintains insulation. The same results were obtained in Examples 1 to 3. Furthermore, Examples 1 to 3 having an inorganic insulating layer obtained higher volume resistivity and radial crushing strength after being stored at 180°C for 1000 hours than Example 5 without an inorganic insulating layer.
[0161] In addition, the magnetic bodies of Examples 9 and 10 in which the ratio of Si in the soft magnetic powder was within the range of 4 to 10 mass % were superior to those of Example 11 in which the ratio of Si in the soft magnetic powder was outside the range, and the decrease in volume resistivity after storage at 180°C for 1000 hours was suppressed. In addition, the radial crushing strength of Examples 9 and 10 after storage at 180°C for 1000 hours was 30 MPa or more.
[0162] This application claims the priority based on Japanese patent application No. 2022-48117 filed on March 24, 2022, and all the disclosed contents of this Japanese application are incorporated into the present invention.
[0163] Description of Reference Numerals
[0164] 1: Soft magnetic powder
[0165] 2: Resin cured product
[0166] 10: Magnetic body
[0167] 11: Coil
[0168] 12: Terminal
[0169] 13: Bonding components
Claims
1. A magnetic body comprising a soft magnetic powder and a cured resin, The magnetic body has a radial crushing strength of 30 MPa or more after being kept in an environment of 180° C. for 1000 hours.
2. The magnetic body according to claim 1, wherein The magnetic body has a strength retention rate of 50% or more after being kept in an environment of 180° C. for 1000 hours.
3. The magnetic body according to claim 1 or 2, wherein: The volume resistivity of the magnetic body after being kept at 180°C for 1000 hours is 10 6 Ωcm or more.
4. The magnetic substance according to any one of claims 1 to 3, wherein The magnetic body has a radial crushing strength of 50 MPa or more after being kept in an environment of 180° C. for 1000 hours.
5. The magnetic substance according to any one of claims 1 to 4, wherein The weight change rate of the magnetic body after being kept in an environment of 180° C. for 1000 hours is 1% or less.
6. The magnetic substance according to any one of claims 1 to 5, wherein After the magnetic body is kept in an environment of 180° C. for 1000 hours, the average major diameter of the pores in the cured resin is 2 μm or less.
7. The magnetic substance according to any one of claims 1 to 6, wherein After the magnetic body is kept in an environment of 180° C. for 1000 hours, an average distance between the soft magnetic powder and the cured resin is 1 μm or less.
8. The magnetic substance according to any one of claims 1 to 7, wherein The cured resin has an imide bond.
9. The magnetic substance according to any one of claims 1 to 8, wherein The cured resin includes polyester imide.
10. The magnetic substance according to any one of claims 1 to 9, wherein The ratio of the resin cured product is 2 to 6 parts by mass based on 100 parts by mass of the soft magnetic powder.
11. The magnetic substance according to any one of claims 1 to 10, wherein The resin cured product includes a cured product of a thermosetting resin composition, and the thermosetting resin composition includes a polyester resin, an epoxy resin, and a polyimide resin.
12. The magnetic body according to claim 11, wherein The polyester-based resin has a carboxyl group.
13. The magnetic body according to claim 11 or 12, wherein: The polyimide-based resin has ethylenic double bonds.
14. The magnetic substance according to any one of claims 11 to 13, wherein The thermosetting resin composition further comprises a peroxide.
15. The magnetic substance according to any one of claims 1 to 14, wherein The soft magnetic powder includes iron alloy powder.
16. The magnetic body according to claim 15, wherein: The iron alloy powder includes a Fe—Si alloy.
17. The magnetic body according to claim 16, wherein: The Fe-Si alloy contains 4 to 10 mass % of Si.
18. The magnetic substance according to any one of claims 15 to 17, wherein The iron alloy powder further includes one or more selected from Cr and Al.
19. The magnetic substance according to any one of claims 1 to 18, wherein The soft magnetic powder has an inorganic insulating layer on the surface.
20. The magnetic body according to claim 19, wherein The inorganic insulating layer includes at least one selected from phosphates and silicates.
21. The magnetic body according to claim 19 or 20, wherein: The ratio of the inorganic insulating layer is 0.1 to 3 parts by mass relative to 100 parts by mass of the soft magnetic powder.
22. The magnetic substance according to any one of claims 19 to 21, wherein The average thickness of the inorganic insulating layer is 10-100 nm.