Nerve sheathing canal based on electrostatic spinning membrane and preparation process of curled nerve sheathing canal
Curled nerve sheaths prepared by electrospinning membrane solve the adhesion problem caused by scar tissue hyperplasia after peripheral nerve injury. Through thermal cross-linking and the use of bioactive materials, adhesions at sutures are reduced and nerve repair is promoted , improves surgical efficiency and recovery of neurological function.
Patent Information
- Application Number
- CN202410924448.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
Adhesion problems caused by scar tissue hyperplasia often occur after peripheral nerve injury, which affects the effect of nerve repair. The existing cannula cannot be completely closed after incision, which increases the surgical time and may cause neuromagenesis and excessive fibrosis.
Using curly-shaped nerve sheaths prepared based on electrospinning membranes, the cannula is formed by heat crosslinking and heat setting. The cannula can be used to absorb polymer materials and collagen to increase the stiffness and biological activity of the cannula, mimicking the extracellular matrix environment , reduce adhesions at sutures and promote nerve repair.
It effectively avoids spillover of nerve growth factors and adhesions at sutures, improves surgical efficiency, promotes nerve repair, reduces the formation of neuroma and fibroblasts, and improves the recovery of nerve function.
Smart Images

Figure CN118892578A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nerve sheath technology, and in particular to a nerve sheath based on an electrospun membrane and a process for preparing a coiled nerve sheath. Background Technology
[0002] Peripheral nerve injury (PNI) is a clinical condition that causes motor and sensory dysfunction, easily leading to syndromes such as loss of sensory and motor function and pain, and even affecting the patient's quality of life and mental and physical health. In my country, there are already 20 million cases of PNI, and this number is increasing by approximately 2 million cases annually. In shorter injury gaps (less than 5 mm), peripheral nerves can self-repair and regenerate, with fibrin spontaneously forming between the two nerve stumps. Schwann cells (SCs) migrate to the injury gap along with the fibrin, forming Büngner's band, which guides axonal regeneration from proximal to distal, at a rate of up to 1 mm per day. However, patients often experience long-term scarring, neuroma formation, and even neurological dysfunction; only 50% of patients fully recover from the trauma. When the PNI gap is 5-10 mm, a nerve graft is required to bridge the proximal and distal ends of the PNI to restore nerve function. The preferred treatment for nerve grafts in clinical practice is autologous transplantation, which is used to repair gaps in peripheral nerve damage. This is because it provides ideal extracellular matrix (ECM) and a large number of glial cells, resulting in good therapeutic effects in restoring nerve function. However, autologous nerve transplantation has drawbacks such as scarcity of donors, size mismatch, donor dysfunction, neuroma formation, nerve torsion, or dislocation.
[0003] Currently, microsurgical suturing techniques are commonly used clinically to repair peripheral nerve injuries. However, due to the unique anatomy and cell regeneration of peripheral nerves, as well as various other factors, simply suturing the severed peripheral nerve can lead to local inflammation and scar tissue hyperplasia and adhesions, directly impacting the effectiveness of nerve repair. This results in less than ideal functional recovery after the repair surgery. Postoperative adhesions after peripheral nerve injury are one of the main problems hindering functional recovery. To achieve good functional recovery after peripheral nerve anastomosis repair, we must address not only the growth of damaged nerve fibers but also the issue of postoperative nerve adhesions. Methods to reduce postoperative adhesions after nerve injury include surgical incisions, minimizing dissection and traction during surgery, using cannulas to protect the nerve's blood supply, employing meticulous fiber suture techniques, utilizing effective membrane barriers, and postoperative medication.
[0004] To prevent postoperative nerve adhesion, a cannula is usually used to isolate the suture site and avoid adhesion to the surrounding connective tissue. The cannula is a hollow cylindrical material. During the operation, the cannula is cut along the center line and wrapped around the suture site. However, in actual use, the cut cannula cannot be completely closed again, and it needs to be closed by suturing, which increases the operation time and is prone to the formation of neuromas, fibroblast ingrowth, excessive scar repair (too severe fibrosis), and tissue adhesion, affecting the nerve repair effect.
[0005] Therefore, there is an urgent need to develop a process for preparing nerve sheaths and coiled nerve sheaths based on electrospun membranes to solve the above problems. Summary of the Invention
[0006] The purpose of this invention is to disclose a process for preparing a nerve sheath based on an electrospun membrane and a coiled nerve sheath.
[0007] The first objective of this invention is to provide a nerve sheath based on an electrospun membrane.
[0008] The second objective of this invention is to provide a process for preparing a coiled nerve sheath.
[0009] To achieve the first objective mentioned above, this invention provides a nerve sheath based on an electrospun membrane, wherein a rectangular electrospun membrane is thermally cross-linked and heat-set into a coiled sheath within a temperature range of 90°C-150°C, and the coiled angle of the coiled sheath is 360°-720°.
[0010] The electrospun membrane comprises absorbable polymer materials and collagen.
[0011] Preferably, the curling angle of the curled sleeve is 540°-720°.
[0012] Preferably, the temperature for thermal crosslinking and heat setting is 100℃-120℃.
[0013] Preferably, the electrospun membrane has a thickness of 0.1 mm to 0.2 mm, a porosity of 50% to 80%, a pore size of 10 μm to 20 μm, and a spinning fiber diameter of 1 μm to 2 μm.
[0014] Preferably, the mass ratio of the absorbable polymer material to collagen is 1:2 to 2:1.
[0015] Preferably, the absorbable polymer material is a natural polymer material and / or a synthetic polymer material;
[0016] The collagen is at least one of recombinant collagen, type I collagen, type II collagen, type III collagen, or heterologous collagen.
[0017] The natural polymer material is chitosan or gelatin;
[0018] The synthetic polymer material is at least one of polyglycolic acid, polycaprolactone, poly-L-lactide-caprolactone, or lactide copolymer.
[0019] Based on the same inventive principle, and to achieve the second inventive objective mentioned above, this invention provides a process for preparing a coiled nerve sheath, comprising the following steps:
[0020] Prepare spinning solutions with a dynamic viscosity of 500 MPa·s to 3000 MPa·s;
[0021] Electrospun films with a thickness of 0.1 mm to 0.2 mm were prepared by electrospinning.
[0022] The electrospun film is cut to a predetermined size, and an isolation layer is covered on the surface of the electrospun film;
[0023] With the isolation layer facing inward, the electrospun film of a predetermined size is thermally cross-linked and heat-set in a temperature range of 90°C-150°C to form a curled sleeve with a curling angle of 360°-720°, and the thermal cross-linking and heat-setting time is 60min-90min.
[0024] The isolation layer is extracted, forming a coiled sleeve.
[0025] Based on the same inventive principle, in order to achieve the second inventive objective mentioned above, the present invention also provides a process for preparing a coiled nerve sheath, comprising the following steps:
[0026] A spinning solution with a dynamic viscosity of 500 MPa·s to 3000 MPa·s is prepared. The spinning solution comprises a solvent, an absorbable polymer material in a mass ratio of 1:2 to 2:1, and collagen. The solvent is one or more of chloroform, dichloromethane, acetone, N,N-dimethylformamide, and hexafluoroisopropanol. The absorbable polymer material is a natural polymer material and / or a synthetic polymer material. The collagen is at least one of recombinant collagen, type I collagen, type II collagen, type III collagen, or heterologous collagen. The natural polymer material is chitosan or gelatin. The synthetic polymer material is at least one of polyglycolic acid, polycaprolactone, poly-L-lactide-caprolactone, or lactide copolymer.
[0027] Electrospinning was used to prepare electrospun membranes with a thickness of 0.1 mm to 0.2 mm. The positive voltage of electrospinning was 10 kV to 15 kV, the negative voltage was 0 kV to 5 kV, the propulsion speed of the electrospinning solution was 10 μl / min to 30 μl / min, the distance between several spinning nozzles and the receiving end of the electrospun membrane was 15 cm to 30 cm, the ambient temperature was 18℃ to 25℃, the ambient humidity was 0% to 70%, and the electrospinning time was 30 min to 60 min.
[0028] The electrospun film is cut to a predetermined size, and an isolation layer is covered on the surface of the electrospun film;
[0029] With the isolation layer facing inward, the electrospun film of a predetermined size is thermally cross-linked and heat-set in a temperature range of 90°C-150°C to form a curled sleeve with a curling angle of 360°-720°, and the thermal cross-linking and heat-setting time is 60min-90min.
[0030] The isolation layer is extracted, forming a coiled sleeve.
[0031] Preferably, the electrospun membrane has a thickness of 0.1 mm to 0.2 mm, a porosity of 50% to 80%, a pore size of 10 μm to 20 μm, and a spinning fiber diameter of 1 μm to 2 μm.
[0032] Preferably, the plurality of spinning nozzles are arranged in a fan shape, and the adjacent spinning nozzles are equidistant or non-equidistant.
[0033] Compared with the prior art, the beneficial effects of the present invention are:
[0034] (1) After spinning, the electrospun membrane is cut into a suitable rectangular size without heat treatment and wound around the outer surface of a cylinder with a certain outer diameter. The winding angle is 360°-720°, that is, one to two turns. Then, it is thermally cross-linked and heat-set. During the thermal cross-linking and heat-setting process, thermal cross-linking reactions occur between collagen and between collagen and absorbable polymer materials, thereby increasing the stiffness of the electrospun membrane and maintaining its curled shape. In subsequent peripheral nerve suturing surgery, the curled cannula is manually unfolded and placed at the suture site. Then, it is released and the cannula rolls back and wraps around the suture site. After rolling back, it will form a complete enclosure of the suture site. Cell growth is induced by the surface morphology of the cannula, such as pore size, porosity, and spinning diameter. In addition, the cannula of this invention has biological activity, which can effectively prevent the leakage of nerve growth factors and reduce the adhesion between the suture site and other tissues. At the same time, the cannula does not need to be re-sutured, which improves the efficiency of the operation.
[0035] (2) The electrospun membrane is composed of absorbable polymer materials and collagen, all of which are biodegradable polymer materials. After thermal cross-linking and heat setting, the surface of the electrospun membrane has uneven micropores, which mimic the extracellular matrix (ECM) environment and provide a good microenvironment for nerve repair at the suture site.
[0036] (3) This invention uses synthetic polymers such as polyglycolic acid, polycaprolactone, and poly-L-lactide-caprolactone, along with collagen, as spinning raw materials. These materials exhibit excellent mechanical properties, ensuring that the inner wall of the sheath can act as a cell carrier. They possess biological activity and can effectively regulate nerve-releasing factors, promoting nerve repair and accelerating the healing cycle. Simultaneously, the spun sheath has good mechanical properties and morphological control, effectively preventing the formation of neuromas and avoiding adhesion between nerve fibers and surrounding tissues. Attached Figure Description
[0037] Figure 1 This is a schematic diagram of the preparation process of the nerve sheath based on the electrospun membrane of the present invention.
[0038] Figure 2 This is a cross-sectional schematic diagram of the electrospun film and the isolation layer of the present invention.
[0039] Figure 3 This is a flowchart of Embodiment 2 of the present invention.
[0040] Figure 4 This is a flowchart of Embodiment 3 of the present invention.
[0041] Figure 5 This is a schematic diagram showing the relative positions of the spinning nozzle and the receiving roller of the present invention.
[0042] Figure 6 This is an electron microscope image of the surface of the coiled sleeve of the present invention.
[0043] Among them, 1. electrospinning film; 11. isolation layer; 2. curled sleeve; 3. receiving roller; 4. spinning nozzle. Detailed Implementation
[0044] The present invention will now be described in detail with reference to the embodiments shown in the accompanying drawings. However, it should be noted that these embodiments are not intended to limit the present invention. Equivalent changes or substitutions in function, method, or structure made by those skilled in the art based on these embodiments are all within the scope of protection of the present invention.
[0045] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting this invention.
[0046] The specific implementation process of the present invention will be described below through several embodiments.
[0047] Example 1
[0048] Example 1 discloses a nerve sheath based on an electrospun membrane, see [link to example]. Figure 1 and Figure 2 As shown, a rectangular electrospun membrane 1 is thermally crosslinked and heat-set into a coiled sleeve 2 at a temperature range of 90°C-150°C. The coiled sleeve 2 has a coiling angle of 360°-720°. The electrospun membrane 1 includes absorbable polymer materials and collagen.
[0049] Specifically, see Figure 1 and Figure 2As shown, after spinning, the electrospun membrane 1 is cut into a suitable rectangular size without heat treatment. An isolation layer 11 is then applied to the surface of the electrospun membrane 1, with the isolation layer 11 extending 2mm-3mm beyond the rectangular size. The isolation layer 11 can be a thin sheet material capable of withstanding 90℃-150℃, such as PTFE film, tin foil, or PET film. With the isolation layer 11 facing inwards, the electrospun membrane 1 is wound around the outer surface of a cylinder with a certain outer diameter, preferably 2mm-5mm. The winding angle is 360°-720°. To facilitate subsequent wrapping of the nerve suture site, the winding angle is preferably 540°-720°, i.e., one and a half to two turns. Then, thermal crosslinking and heat setting are performed. The preferred temperature for thermal crosslinking and heat setting is 100℃-120℃. Within this temperature range, during the thermal crosslinking and heat setting process, the collagen fibers interact with each other, and the collagen fibers and absorbable polymer materials... A thermal cross-linking reaction occurs between the materials, thereby increasing the stiffness of the electrospun membrane and maintaining its curled shape. During subsequent peripheral nerve suturing surgery, the curled cannula is manually unfolded and placed at the suture site. After being released, the cannula rolls back on its own, forming a complete enclosure of the suture site. Cell growth is induced through the surface morphology of the cannula, such as pore size, porosity, and spinning diameter. Furthermore, the cannula of this invention is bioactive, effectively preventing the leakage of nerve growth factors and reducing adhesion between the suture site and other tissues. At the same time, the cannula does not require re-suturing, improving surgical efficiency. In this embodiment, during the thermal cross-linking and heat setting process, the isolation layer 11 isolates the contact surfaces between the electrospun membranes 1, preventing adhesion between the contact surfaces of the electrospun membranes 1. After setting, the isolation layer 11, which exceeds the rectangular size by 2mm-3mm, is pulled out, completing the curled cannula 2.
[0050] The electrospun membrane has a thickness of 0.1 mm-0.2 mm, a porosity of 50%-80%, a pore size of 10 μm-20 μm, and a fiber diameter of 1 μm-2 μm. The electrospun membrane is composed of absorbable polymer materials and collagen, with a mass ratio of 1:2 to 2:1. The absorbable polymer materials are natural and / or synthetic polymer materials. The collagen is at least one of recombinant collagen, type I collagen, type II collagen, type III collagen, or heterologous collagen. The natural polymer material is chitosan or gelatin. The synthetic polymer material is at least one of polyglycolic acid, polycaprolactone, poly-L-lactide-caprolactone, or lactide copolymer. Performance parameters of the electrospun membrane and the coiled sleeve are shown in Table 1. Electron micrographs of the surface of the coiled sleeve are shown in [reference needed]. Figure 6Without wetting the coiled cannula 2, the coiled cannula 2, after being heat-crosslinked and heat-set, was manually unfolded and observed to see if it could naturally roll back. It was found that the number of unfolding and rolling back of the coiled cannula 2 from number 1 to number 3 all exceeded 5 times. This means that when doctors use it in clinical applications, they can unfold it multiple times and adjust its position. The coiled cannula 2 can then naturally wrap around the suture, meeting the actual clinical needs.
[0051] Table 1 Performance parameters of electrospun films and coiled tubing
[0052]
[0053] Example 2
[0054] See Figure 3 The preparation process of the coiled nerve sheath includes the following steps:
[0055] Step S1: Prepare a spinning solution with a dynamic viscosity of 500 MPa.S-3000 MPa.S; specifically, the spinning solution includes a solvent, an absorbable polymer material in a mass ratio of 1:2-2:1, and collagen. The solvent is one or more of chloroform, dichloromethane, acetone, N,N-dimethylformamide, and hexafluoroisopropanol; the absorbable polymer material is a natural polymer material and / or a synthetic polymer material; the collagen is recombinant collagen, type I collagen, type II collagen, type III collagen, or heterologous collagen. At least one of the following: the natural polymer material is chitosan or gelatin; the synthetic polymer material is at least one of polyglycolic acid, polycaprolactone, poly-L-lactide-caprolactone, or lactide copolymer; in order to ensure the strength of the finally prepared coiled sleeve, in step S1, the spinning solution preferably contains polyglycolic acid and collagen in a mass ratio of 1:1 as the spinning raw material. The coiled sleeve has excellent mechanical properties, ensuring that the inner wall of the sleeve can act as a cell carrier, has biological activity, and can effectively regulate nerve release factors, promote nerve repair, and accelerate the healing cycle.
[0056] Step S2: Electrospinning to prepare an electrospun membrane with a thickness of 0.1mm-0.2mm; specifically, the positive voltage of electrospinning is 10kV-15kV, the negative voltage is 0kV-5kV, the propulsion speed of the electrospinning solution is 10μl / min-30μl / min, the distance between the spinning nozzles and the receiving end of the electrospun membrane is 15cm-30cm, the receiving end is the receiving roller 3, the ambient temperature is 18℃-25℃, the ambient humidity is 0%-70%, and the electrospinning time is 30min-60min; the spinning nozzles 4 are arranged in a fan shape, and the adjacent spinning nozzles are equidistant or non-equidistant, see [reference]. Figure 5Given that the surface of the receiving roller 3 is curved, in order to ensure the uniformity of the final electrospun film thickness, the distance between each spinning nozzle 4 and the surface of the receiving roller 3 must be consistent. The fan-shaped arrangement of the spinning nozzles 4 ensures that the distance of electrostatic spinning of each spinning nozzle 4 is equal, which can ensure the uniformity of the electrospun film thickness. Through step S2, the electrospun film formed has a thickness of 0.1mm-0.2mm, a porosity of 50%-80%, a pore size of 10μm-20μm, and a spinning fiber diameter of 1μm-2μm.
[0057] Step S3: Cut the electrospun film to a predetermined size and cover the surface of the electrospun film with an insulating layer; specifically, see Figure 1 and Figure 2 After spinning, the electrospun film 1 is cut into a suitable rectangular size without heat treatment, and an isolation layer 11 is covered on the surface of the electrospun film 1. The size of the isolation layer 11 exceeds the rectangular size by 2mm-3mm.
[0058] Step S4: With the isolation layer facing inward, the electrospun membrane of a predetermined size is thermally cross-linked and heat-set in a temperature range of 90℃-150℃ to form a coiled sleeve with a curling angle of 360°-720°. The thermal cross-linking and heat-setting time is 60min-90min. Specifically, with the isolation layer 11 facing inward, the electrospun membrane 1 is wound around the outer surface of a cylinder with a certain outer diameter, preferably 2mm-5mm, and the winding angle is 360°-720°. To facilitate subsequent wrapping of the nerve suture site, the winding angle is preferably 540°.
[0059] -720°, i.e., one and a half to two turns, followed by thermal cross-linking and heat setting. The preferred temperature for thermal cross-linking and heat setting is 100°C-120°C. Within this temperature range, thermal cross-linking reactions occur between collagen fibers and between collagen and absorbable polymer materials during the thermal cross-linking and heat setting process, thereby increasing the stiffness of the electrospun membrane and maintaining its curled shape. In subsequent peripheral nerve suturing surgery, the curled cannula is manually unfolded and placed at the suture site, then released and allowed to roll back on its own. After rolling back, it forms a complete enclosure of the suture site, preventing adhesion between the suture site and other tissues. At the same time, the cannula does not need to be sutured again, improving surgical efficiency.
[0060] Step S5: Remove the isolation layer to form a coiled sleeve. Specifically, in this embodiment, during the thermal crosslinking and heat setting process, the isolation layer 11 isolates the contact surfaces between the electrospun films 1, preventing adhesion between the contact surfaces of the electrospun films 1. After setting, the isolation layer 11 is removed by clamping the 2mm-3mm portion exceeding the rectangular size, thus completing the coiled sleeve 2.
[0061] The nerve sheath based on the electrospun membrane described in Example 1 was prepared by Example 2. For the same parts, please refer to Example 1, and they will not be repeated here.
[0062] Example 3
[0063] See Figure 4 The preparation process of the coiled nerve sheath includes the following steps:
[0064] Step A1: Prepare a spinning solution with a dynamic viscosity of 500 MPa·s-3000 MPa·s. The spinning solution includes a solvent, an absorbable polymer material in a mass ratio of 1:2 to 2:1, and collagen. The solvent is one or more of chloroform, dichloromethane, acetone, N,N-dimethylformamide, and hexafluoroisopropanol. The absorbable polymer material is a natural polymer material and / or a synthetic polymer material. The collagen is at least one of recombinant collagen, type I collagen, type II collagen, type III collagen, or heterologous collagen. The natural polymer material is chitosan. Sugar or gelatin; the synthetic polymer material is at least one of polyglycolic acid, polycaprolactone, poly-L-lactide-caprolactone, or lactide copolymer; specifically, the spinning solution has a dynamic viscosity of 500 MPa.S-3000 MPa.S. The selection of dynamic viscosity is related to the content of absorbable polymer materials and collagen in the spinning solution and their average molecular weight. Specifically, when the average molecular weight is small, the dynamic viscosity of the spinning solution is preferably 500 MPa.S-1500 MPa.S; when the average molecular weight is large, the dynamic viscosity of the spinning solution is preferably 1000 MPa.S-3000 MPa.S.
[0065] Step A2: Electrospinning is used to prepare an electrospun membrane with a thickness of 0.1 mm-0.2 mm. The positive voltage of electrospinning is 10 kV-15 kV, the negative voltage is 0 kV-5 kV, the propulsion speed of the electrospinning solution is 10 μl / min-30 μl / min, the distance between the spinning nozzles and the receiving end of the electrospun membrane is 15 cm-30 cm, the ambient temperature is 18℃-25℃, the ambient humidity is 0%-70%, and the electrospinning time is 30 min-60 min. The spinning nozzles are arranged in a fan shape, and the adjacent spinning nozzles are equidistant or non-equidistant. The final electrospun membrane has a thickness of 0.1 mm-0.2 mm, a porosity of 50%-80%, a pore size of 10 μm-20 μm, and a fiber diameter of 1 μm-2 μm.
[0066] Step A3: Cut the electrospun film to a predetermined size and cover the surface of the electrospun film with an isolation layer; the same as step S3 in Example 2, and will not be repeated.
[0067] Step A4: With the isolation layer facing inward, the electrospun film of a predetermined size is thermally crosslinked and heat-set in a temperature range of 90°C-150°C to form a curled sleeve with a curling angle of 360°-720°. The thermal crosslinking and heat-setting time is 60min-90min. This is the same as step S4 in Example 2 and will not be repeated.
[0068] Step A5: Remove the isolation layer to form a coiled sleeve. This is the same as step S5 in Example 2, and will not be described again.
[0069] The nerve sheath based on the electrospun membrane described in Example 1 was prepared by Example 3. For the same parts, please refer to Example 1, and they will not be repeated here.
Claims
1. A neural sheath based on an electrospinning membrane, characterized in that: The rectangular electrospun membrane is thermally cross-linked and heat-set into a curled sleeve at a temperature range of 90°C to 150°C, wherein the curling angle of the curled sleeve is 360° to 720°; The electrostatic spinning membrane comprises absorbable polymer material and collagen.
2. The neural sheath tube based on electrospinning membrane according to claim 1, characterized in that: The curling angle of the curled sleeve is 540°-720°.
3. The neural sheath tube based on electrospinning membrane according to claim 1, characterized in that: The temperature of the heat crosslinking and heat setting is 100°C-120°C.
4. The neural sheath tube based on electrospinning membrane according to any one of claims 1 to 3, characterized in that: The electrostatic spinning membrane has a thickness of 0.1 mm to 0.2 mm, a porosity of 50% to 80%, a pore size of 10 μm to 20 μm, and a spinning fiber diameter of 1 μm to 2 μm.
5. The neural sheath tube based on electrospinning membrane according to claim 4, characterized in that: The mass ratio of the absorbable polymer material to collagen is 1:2-2:
1.
6. The neural sheath tube based on electrospinning membrane according to claim 5, characterized in that: The absorbable polymer material is a natural polymer material and / or a synthetic polymer material; The collagen is at least one of recombinant collagen, type I collagen, type II collagen, type III collagen or heterosexual collagen; The natural polymer material is chitosan or gelatin; The synthetic polymer material is at least one of polyglycolide, polycaprolactone, poly-L-lactide-caprolactone or lactide copolymer.
7. A process for preparing a curled neural sheath, characterized in that: The following steps are involved: Preparing a spinning solution with a dynamic viscosity of 500MPa.S-3000MPa.S; Electrospinning was used to prepare electrospinning membranes with a thickness of 0.1 mm to 0.2 mm; Cutting the electrospun membrane into a predetermined size and covering the surface of the electrospun membrane with an isolation layer; With the isolation layer facing inward, the electrospun membrane of a predetermined size is thermally cross-linked and heat-set in a temperature range of 90°C-150°C into a curled sleeve with a curling angle of 360°-720°, and the thermal cross-linking and heat-setting time is 60min-90min; The insulating layer is pulled out to form a curled sleeve.
8. A process for preparing a curled neural sheath, characterized in that: The following steps are involved: A spinning solution with a dynamic viscosity of 500MPa.S-3000MPa.S is prepared, wherein the spinning solution comprises a solvent, an absorbable polymer material and collagen in a mass ratio of 1:2-2:1, wherein the solvent is one or more of chloroform, dichloromethane, acetone, N,N-dimethylformamide and hexafluoroisopropanol, and the absorbable polymer material is a natural polymer material and / or a synthetic polymer material; the collagen is at least one of recombinant collagen or type I collagen, type II collagen, type III collagen or hetero-collagen; the natural polymer material is chitosan or gelatin; and the synthetic polymer material is at least one of polyglycolide, polycaprolactone, poly-L-lactide-caprolactone or a lactide copolymer; Electrospinning is used to prepare an electrospinning membrane with a thickness of 0.1 mm to 0.2 mm. The positive voltage of the electrospinning is 10 kv to 15 kv, the negative high voltage is 0 kv to 5 kv, the propulsion speed of the electrospinning solution is 10 μl / min to 30 μl / min, the distance between the spinning nozzles and the receiving end of the electrospinning membrane is 15 cm to 30 cm, the ambient temperature is 18°C to 25°C, the ambient humidity is 0% to 70%, and the electrospinning time is 30 min to 60 min. Cutting the electrospun membrane into a predetermined size and covering the surface of the electrospun membrane with an isolation layer; With the isolation layer facing inward, the electrospun membrane of a predetermined size is thermally cross-linked and heat-set in a temperature range of 90°C-150°C into a curled sleeve with a curling angle of 360°-720°, and the thermal cross-linking and heat-setting time is 60min-90min; The insulating layer is pulled out to form a curled sleeve.
9. The process for preparing the curled nerve sheath tube according to claim 7 or 8, characterized in that: The electrostatic spinning membrane has a thickness of 0.1 mm to 0.2 mm, a porosity of 50% to 80%, a pore size of 10 μm to 20 μm, and a spinning fiber diameter of 1 μm to 2 μm.
10. The process for preparing the curled nerve sheath tube according to claim 7 or 8, characterized in that: The plurality of spinning nozzles are arranged in a fan shape, and adjacent spinning nozzles are equidistant or unequally spaced.