ECM microsphere, injectable tissue repair filling material containing ECM microsphere and application of injectable tissue repair filling material

The preparation of ECM microspheres through low-temperature wet grinding technology solves the problem of structural damage during ECM microparticulation, achieves more stable degradation and higher biosafety, and improves tissue regeneration effect and injection portability.

CN118892580APending Publication Date: 2024-11-05CHONGQING DAQING HAIDE BIOTECHNOLOGY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411235313.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing ECM microparticulation process is prone to destroy the structure of active active ingredients, resulting in a decrease in tissue regeneration effect.

Method used

Low-temperature wet grinding technology is used to prepare ECM microspheres to protect the molecular structure, avoid the use of crosslinking agents, increase surface roughness and porosity to improve biocompatibility and degradation stability.

Benefits of technology

It reduces the degradation time of ECM microspheres in the body, improves biosafety and tissue regeneration effects, reduces the risk of side reactions after injection, and improves the portability and stability of injection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892580A_ABST
    Figure CN118892580A_ABST
Patent Text Reader

Abstract

The invention provides ECM microspheres, an injectable tissue repair filling material containing the ECM microspheres and application of the injectable tissue repair filling material, and relates to the technical field of biomedical materials. The preparation method of the ECM microspheres comprises the following steps: preparing an extracellular matrix from an animal-derived tissue raw material; dehydrating and drying the acellular matrix to obtain an ECM (extracellular matrix) material; the ECM material firstly absorbs water and then is subjected to low-temperature wet grinding treatment, and wet ECM particles are obtained; and the ECM particles are dried and then screened. The injectable tissue repair filling material is formed by compounding a dispersing agent and ECM microspheres, wherein the ECM microspheres account for 0.2-10% of the dispersing agent in percentage by mass. The injectable tissue repair filling material can be used for preparing a medical beauty injection filling preparation. The ECM particles are obtained in a low-temperature wet grinding mode, heating in the grinding process can be reduced, intermolecular gaps are increased to protect natural structures of molecules in ECM, and the advantages of the natural structures can be played after the ECM particles are injected into a human body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of biomedical materials, and in particular to an ECM microsphere, an injectable tissue repair filling material containing the ECM microsphere, and applications thereof. Background Art

[0002] In recent years, people have changed their mindset about facial rejuvenation, from subtractive surgery to additive surgery. Facial injections have become the most commonly used facial rejuvenation method because of their minimally invasive and easy operation. Common filler materials include hyaluronic acid, collagen, botulinum toxin, etc. These materials can temporarily increase the volume of the skin, making the face look younger and more energetic.

[0003] In recent years, with the development of regenerative medicine and biomaterials science, extracellular matrix (ECM) has become a potential high-quality material for facial medical cosmetic injections due to its unique biological activity and regenerative ability. As a natural biomaterial, ECM has a unique triple helical collagen structure, and ECM contains natural growth factors and is rich in collagen, elastin, fibronectin and other bioactive ingredients, which are essential for maintaining the structure and function of the skin. By extracting and purifying ECM, a filling material with excellent biocompatibility and bioactivity can be obtained.

[0004] However, the injection needles used in medical aesthetics are generally in the range of 23G-34G blunt and sharp needles, and tiny particles with a diameter of 60μm-340μm can pass through the needles. Therefore, mechanical grinding is currently used to prepare micronized ECM. However, this method will destroy the structure of macromolecular active ingredients such as collagen and growth factors in ECM, thereby losing the advantages of ECM as a natural biomaterial, accelerating the degradation time in the body and reducing the effect of promoting tissue regeneration. Summary of the invention

[0005] In order to improve the problem that the structure of active ingredients of ECM materials is easily destroyed during the micronization process, resulting in reduced effect of promoting tissue regeneration, the present application provides ECM microspheres, an injectable tissue repair filling material containing ECM microspheres and applications thereof.

[0006] In the first aspect, the present application provides an ECM microsphere, which adopts the following technical solution: An ECM microsphere, wherein the preparation method of the ECM microsphere comprises the following steps: S1: Take animal-derived tissue materials and prepare decellularized extracellular matrix; S2: dehydrating and drying the decellularized extracellular matrix described in step S1 to obtain an ECM material; S3: subjecting the ECM material described in step S2 to water absorption treatment first, and then to low-temperature wet grinding treatment, to obtain wet ECM particles; S4: subjecting the ECM particles of step S3 to drying treatment and then to sieving treatment, to obtain ECM microspheres of 10-150 μm.

[0007] The present application obtains ECM microparticles by adopting low-temperature wet grinding in the preparation process of ECM microspheres, which can reduce the heat generated during grinding, increase the gap between molecules to protect the natural structure of molecules in ECM, and can give full play to the advantages of its natural structure after injection into the human body. In addition, the present application does not use a cross-linking agent in the process of ECM micronization, which has higher safety, and because its natural structure is not destroyed, it can have a more stable degradation time.

[0008] Compared with the ECM material obtained in step S2, the surface roughness of the ECM microspheres in step S4 increases and the stacking porosity increases after low-temperature wet grinding. Therefore, when the ECM microspheres are injected into the human body, they are beneficial to fluid exchange and cell climbing in the body and reduce the incidence of nodules.

[0009] Optionally, the animal source described in step S1 is selected from one of humans, cattle, pigs, and sheep, and the tissue material is selected from one or more of dermis, muscle, tendon, heart, fat, small intestine, umbilical cord, placenta, blood vessels, nerves, bones, and cartilage.

[0010] Optionally, the water absorption of the ECM material is 10% to 400% of the mass of the ECM material.

[0011] Optionally, the low-temperature wet grinding treatment in step S3 is specifically performed as follows: grinding at a temperature of -200°C to -30°C for 10-300s, pausing for 5-60s, and repeating this process 10-300 times.

[0012] In a second aspect, the present application provides an injectable tissue repair filling material, which adopts the following technical solution: An injectable tissue repair filling material is composed of a dispersant and the ECM microspheres, wherein the ECM microspheres account for 0.2wt.%-10wt.%.

[0013] Because the ECM microspheres used have a large surface area and pores, they are easier to dissolve than traditional smooth microspheres, which is conducive to injection operation. They can also prevent the microspheres from agglomerating in the body and causing surface immune responses to form nodules, thereby avoiding side effects after injection.

[0014] Once the existing hyaluronic acid filler is overfilled and in thin skin sites, the Tyndall effect is likely to occur, and the appearance changes to light blue, purple, etc., affecting the injection effect. However, due to the rough surface of the ECM microspheres in the filling material of the present application, the probability of vertical light penetrating the injection site is reduced, and the Tyndall effect is not easily formed, so that the injection effect is better.

[0015] Optionally, the dispersant comprises, by weight percentage: 0.5%-10% gel, The balance is solvent.

[0016] Optionally, the gel is selected from one or more of carboxymethyl chitin, carboxymethyl chitosan, oxidized cellulose, carboxymethyl cellulose, sodium carboxymethyl cellulose, hydroxyethyl cellulose, sodium hydroxyethyl cellulose, hyaluronic acid, sodium hyaluronate, chondroitin sulfate, sodium trehalose, polyglutamic acid, porcine natural collagen, bovine natural collagen, human natural collagen, and recombinant human collagen; The solvent is pure water.

[0017] Since ECM will settle in water after absorbing water and swelling, the present application adopts the above-mentioned gel as the mobile phase, which has high viscosity and low solid content, so that the final filling material can be formed into a long-term suspended suspension, which has an improvement effect on improving the portability of surgical operations and preventing displacement.

[0018] Optionally, the gelling agent includes a cross-linked gel and / or a non-cross-linked gel.

[0019] The cross-linked gel medium is a cross-linked product of the above gel phase.

[0020] The present application designs the selection of gelling agents based on the stress environment of the human epidermis and dermis. After being injected into the human body, it is not easy to diffuse or disperse, and can better mechanically stimulate fibroblasts to synthesize collagen.

[0021] Optionally, the dispersant comprises, by mass percentage: 0.5%-10% gel, 0.1%-5% non-gel agent, The balance is solvent; The non-gel agent includes one or more of a nutrient, an osmotic pressure balancer, a growth factor, and an anesthetic.

[0022] Optionally, the nutrient may be selected from any one or more of the 21 essential amino acids for the human body, vitamin A, vitamin B, vitamin C, vitamin E, acetyl tetrapeptide, oligopeptide, human recombinant collagen, nucleotides, glutathione, resveratrol, glutathione reductase, glutathione peroxidase, glutathione S-transferase, ubiquinone, tea polyphenols and ascorbyl palmitate.

[0023] Optionally, the osmotic pressure balancing agent can be selected from a mixed solution of one or more selected from pure water, physiological saline, phosphate buffer, sodium potassium buffer, bicarbonate buffer, borate buffer, magnesium sulfate, zinc sulfate, strontium sulfate, copper sulfate, and zinc sulfate.

[0024] Optionally, the growth factor may be selected from one or more of TGF-β, VEGF, FGF, EGF, TGF, TNF.

[0025] Optionally, the anesthetic may be selected from one or more of lidocaine, procaine, bupivacaine, ropivacaine and articaine.

[0026] In a third aspect, the present application also provides a use of an injectable tissue repair filling material for preparing medical cosmetic injectable filling preparations.

[0027] In summary, the present application includes at least one of the following beneficial effects: 1. The ECM microspheres prepared in the present application have a rough surface, a large number of pores, and a large specific surface area, which can accelerate their dissolution rate in the dispersant and reduce side effects after injection.

[0028] 2. The ECM microspheres prepared in this application have a rough surface, a high degree of light refraction, and low light transmittance after compounding with gel, which reduces direct light and reduces the Tyndall effect.

[0029] 3. Compared with cross-linked ECM microparticles for facial injection, the ECM microspheres of the present application can achieve the purpose of maintaining the structural integrity of collagen and growth factors, reduce the safety risks brought by the use of cross-linking agents, have high biosafety and at the same time increase the degradation time of ECM microspheres.

[0030] 4. The present application compounds the ECM microspheres with a dispersant containing a gelling agent, so that the ECM microspheres can be stably suspended in the gelling agent for a long time without settling, which is convenient for the storage of the injection before injection and is not easy to form nodules or shift after injection.

[0031] 5. The injection material of the present application can stimulate the surrounding fibroblasts to synthesize collagen, while reducing the displacement of the material after injection. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1is a surface morphology image of the ECM microspheres prepared according to Example 1 of the present application under a microscope; Figure 2 They are the results of rat back dermal slices after sample injection of Example 6, wherein a, b, c, and d respectively show the results of rat back dermal slices after sample injection for 2 weeks, 4 weeks, 6 weeks, and 8 weeks; Figure 3 The graph shows the comparison of dermal collagen concentration between the sample of Example 6 and the normal saline control group 8 weeks after injection. DETAILED DESCRIPTION

[0033] The term “comprise” or “include” is an open expression, that is, including the contents specified in the present invention but not excluding other contents.

[0034] In the present invention, “consisting of the following components”, “consisting essentially of the following components”, or “consisting of” means that inevitable impurities and / or water may be contained.

[0035] In the description of this specification, the description with reference to terms such as "one embodiment", "some embodiments", "some implementation methods", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention.

[0036] In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples without contradiction.

[0037] Example 1 Example 1 provides a method for preparing ECM microspheres, and the specific operations are as follows: S1: Take fresh biological tissue, the submucosa of porcine small intestine, inactivate the virus, defat, decellularize and descale, and obtain the water-containing decellularized extracellular matrix; S2: draining the above-mentioned water-containing decellularized extracellular matrix at 37° C. and normal pressure for 8 hours to obtain a dry ECM material; S3: After the dried ECM material absorbs water, it is subjected to low-temperature wet grinding using an electromagnetic impact grinder, and the amount of water absorbed is 20% of the mass of the ECM material. The specific steps of the low-temperature wet grinding are: grinding at -196°C for 50 seconds, pausing for 10 seconds, and repeating this cycle 30 times to obtain wet ECM particles; S4: The wet ECM microparticles are collected, freeze-dried, and then sieved to obtain ECM microspheres of 20-50 μm.

[0038] Figure 1 is a surface morphology diagram of the ECM microspheres according to Example 1 of the present application under a microscope. Figure 1 , it can be seen that the surface of ECM microspheres is rough and has many pores.

[0039] Example 2 Example 2 provides a method for preparing ECM microspheres, and the specific operations are as follows: S1: Take fresh biological tissue, the submucosa of porcine small intestine, inactivate the virus, defat, decellularize and descale, and obtain the water-containing decellularized extracellular matrix; S2: draining the above-mentioned water-containing decellularized extracellular matrix at 37° C. and normal pressure for 8 hours to obtain a dry ECM material; S3: After the dried ECM material absorbs water, it is subjected to low-temperature wet grinding using an electromagnetic impact grinder, and the amount of water absorbed is 50% of the mass of the ECM material. The specific steps of the low-temperature wet grinding treatment are: grinding at -196°C for 50 seconds, pausing for 10 seconds, and repeating this cycle 50 times to obtain wet ECM particles; S4: The wet ECM microparticles are collected, freeze-dried, and then sieved to obtain ECM microspheres of 20-50 μm.

[0040] Example 3 Example 3 provides a method for preparing ECM microspheres, and the specific operations are as follows: S1: Take fresh biological tissue, the submucosa of porcine small intestine, inactivate the virus, defat, decellularize and descale, and obtain the water-containing decellularized extracellular matrix; S2: freeze-drying the above-mentioned water-containing decellularized extracellular matrix for 8 hours to obtain a dry ECM material; S3: After the dried ECM material absorbs water, it is subjected to low-temperature wet grinding using an electromagnetic impact grinder, and the amount of water absorbed is 100% of the mass of the ECM material. The specific steps of the low-temperature wet grinding are: grinding at -196°C for 50 seconds, pausing for 10 seconds, and repeating this cycle 100 times to obtain wet ECM particles; S4: The wet ECM microparticles are collected, freeze-dried, and then sieved to obtain ECM microspheres of 20-50 μm.

[0041] Example 4 Example 4 provides a method for preparing ECM microspheres, and the specific operations are as follows: S1: Take fresh biological tissue, the submucosa of porcine small intestine, inactivate the virus, defat, decellularize and descale, and obtain the water-containing decellularized extracellular matrix; S2: freeze-drying the above-mentioned water-containing decellularized extracellular matrix for 8 hours to obtain a dry ECM material; S3: After the dried ECM material absorbs water, it is subjected to low-temperature wet grinding using an electromagnetic impact grinder, and the amount of water absorbed is 400% of the mass of the ECM material. The specific steps of the low-temperature wet grinding are: grinding at -196°C for 50 seconds, pausing for 10 seconds, and repeating this cycle 100 times to obtain wet ECM particles; S4: The wet ECM microparticles are collected, freeze-dried, and then sieved to obtain ECM microspheres of 20-50 μm.

[0042] Example 5 Example 5 provides a method for preparing ECM microspheres, and the specific operations are as follows: S1: fresh biological tissue porcine dermis is taken, and virus inactivation, degreasing, decellularization and descaling are performed to obtain a water-containing decellularized extracellular matrix; S2: draining the above-mentioned water-containing decellularized extracellular matrix at 37° C. and normal pressure for 8 hours to obtain a dry ECM material; S3: After the dried ECM material absorbs water, it is subjected to low-temperature wet grinding using an electromagnetic impact grinder, and the amount of water absorbed is 30% of the mass of the ECM material. The specific steps of the low-temperature wet grinding treatment are: grinding at -196°C for 50 seconds, pausing for 10 seconds, and repeating this cycle for 60 times to obtain wet ECM particles; S4: The wet ECM microparticles are collected, freeze-dried, and then sieved to obtain ECM microspheres of 20-50 μm.

[0043] Comparative Example 1 Comparative Example 1 is basically the same as Example 1, except that the specific operation of step S3 is as follows: the dried ECM material is subjected to room temperature wet grinding treatment using an electromagnetic impact grinder after absorbing water, and the amount of water absorbed is 20% of the mass of the ECM material. The specific steps of the room temperature wet grinding treatment are: grinding at room temperature for 50 seconds, pausing for 10 seconds, and repeating this cycle 30 times to obtain wet ECM particles.

[0044] Comparative Example 2 Comparative Example 2 provides a method for preparing ECM microspheres, and the specific operations are as follows: S1: Take fresh biological tissue, the submucosa of porcine small intestine, inactivate the virus, defat, decellularize and descale, and obtain the water-containing decellularized extracellular matrix; S2: The above-mentioned water-containing decellularized extracellular matrix is ​​subjected to cryogenic grinding using an electromagnetic impact grinder, wherein the specific steps are as follows: grinding at -196°C for 50 seconds, pausing for 10 seconds, and repeating this cycle 30 times to obtain wet ECM particles; S3: The wet ECM microparticles are collected, freeze-dried, and then sieved to obtain ECM microspheres of 20-50 μm.

[0045] Performance test 1 1. Particle size distribution The ECM microspheres obtained in step S4 of Examples 1-5 and Comparative Examples 1-2 were sieved, and the mass proportions of particles in each particle size range were counted. The specific results are shown in Table 1.

[0046] Table 1 Mass proportion of ECM microspheres in each particle size range It is not difficult to see from the results in Table 1 that after the ECM microspheres of Examples 1-5 were treated with low-temperature wet grinding, the particle size distribution was relatively uniform, and the particles with a particle size range of 20-50 μm accounted for more than 1 / 3, which can meet the requirements of the target particle size range of this application. The ECM microspheres of Comparative Example 1 were treated with room temperature wet grinding, and the particle size distribution was extreme, in which the vast majority (95.8%) of the particles were larger than 100 μm, and particles with smaller particle sizes were almost non-existent. The main reason was that the ECM material had strong toughness and wet grinding at room temperature could not crush the ECM material. The ECM microspheres of Comparative Example 2 showed a biased distribution, mainly concentrated in 50-100 μm. The main reason was that the collagen of the ECM material of Comparative Example 2 had not been repeatedly frozen and thawed or dehydrated, resulting in strong toughness and difficulty in uniform grinding. Specifically, in the particle size distribution of the ECM microspheres of Comparative Example 2, the target particle size range of 20-50 μm in this application accounted for only 1 / 4, and the product utilization rate was too low to meet the requirements of the target particle size range of this application.

[0047] 2. Growth factor detection The ECM microspheres prepared in Examples 1-5 and Comparative Examples 1-2 were tested for growth factor content using an ELISA kit. The specific results are shown in Table 2.

[0048] Table 2 Growth factor content of ECM microspheres It is not difficult to see from the results of Table 2 that the ECM microspheres of Examples 1-4 have high growth factor contents, indicating that the treatment method of low-temperature wet grinding can help protect the activity of growth factors and reduce their degradation during the treatment process. Example 5 uses pig dermis as the raw material of ECM material, so the content of growth factors in the ECM microspheres prepared therefrom is lower than that of the ECM microspheres prepared using pig small intestinal submucosal layer as raw material. Comparative Example 1 uses a treatment method of normal temperature wet grinding, and its various growth factor contents are lower than those of Example 1. The reason is that normal temperature wet grinding easily leads to the inactivation of growth factors in ECM materials, while low temperature wet grinding helps to reduce the degradation or inactivation of growth factors while breaking cells. The growth factor content of Comparative Example 2 is slightly lower than that of Example 1. The reason may be that the ECM material of Comparative Example 2 has not undergone a process of first dehydration and then water absorption, and it is not easy to release growth factors during the low-temperature wet grinding process.

[0049] Example 6 Example 6 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 3.5 g of the ECM microspheres prepared in Example 1 were mixed with 96.5 g of a dispersant to prepare an injectable tissue repair filling material, wherein the dispersant includes a gelling agent and pure water, and is composed of 2.3 g of sodium hyaluronate with a molecular weight of 3 MDa, 1 g of sodium hyaluronate with a molecular weight of 1 MDa and 93.2 g of pure water.

[0050] Example 7 Example 7 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 3.5 g of the ECM microspheres prepared in Example 1 were mixed with 96.5 g of a dispersant to prepare an injectable tissue repair filling material, wherein the dispersant includes a gelling agent and pure water, and is composed of 2.3 g of sodium hyaluronate with a molecular weight of 3 MDa, 1 g of sodium hyaluronate with a molecular weight of 1 MDa and a BDDE cross-linking degree of 0.6%, and 93.2 g of pure water.

[0051] Example 8 Example 8 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 3.5 g of the ECM microspheres prepared in Example 2 were mixed with 96.5 g of a dispersant to prepare an injectable tissue repair filling material, wherein the dispersant includes a gelling agent and pure water, and is composed of 2.1 g of sodium hyaluronate with a molecular weight of 3 MDa, 1 g of sodium hyaluronate with a molecular weight of 1 MDa and 93.4 g of pure water.

[0052] Example 9 Example 9 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 4.5 g of the ECM microspheres prepared in Example 3 were mixed with 95.5 g of a dispersant to prepare an injectable tissue repair filling material. The dispersant included a gelling agent, compound vitamins, glutathione and pure water, specifically 1.3 g of sodium hyaluronate with a molecular weight of 3 MDa, 1 g of sodium hyaluronate with a molecular weight of 1 MDa, 0.2 g of compound vitamins, 0.2 g of glutathione and 92.8 g of pure water.

[0053] Example 10 Example 10 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 4.5 g of the ECM microspheres prepared in Example 4 were mixed with 95.5 g of a dispersant to prepare an injectable tissue repair filling material, wherein the dispersant includes a gelling agent and pure water, and is composed of 1.6 g of sodium hyaluronate with a molecular weight of 3 MDa, 1 g of carboxymethyl chitosan with a molecular weight of 0.5 MDa (degree of substitution of 0.8) and 92.9 g of pure water.

[0054] Embodiment 11 Example 11 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 3.5 g of the ECM microspheres prepared in Example 2 were mixed with 96.5 g of a dispersant to prepare an injectable tissue repair filling material, wherein the dispersant includes a gelling agent and pure water, and is composed of 1 g of sodium carboxymethyl cellulose (substitution degree 0.9) with a molecular weight of 0.7 MDa and 95.5 g of pure water.

[0055] Example 12 Example 12 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 3.5 g of the ECM microspheres prepared in Example 2 were mixed with 96.5 g of a dispersant to prepare an injectable tissue repair filling material, wherein the dispersant includes a gelling agent and pure water, and is composed of 1 g of sodium carboxymethyl cellulose (substitution degree 0.9) with a molecular weight of 0.25 MDa and 95.5 g of pure water.

[0056] Embodiment 13 Example 13 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 3.5 g of the ECM microspheres prepared in Example 2 were mixed with 96.5 g of a dispersant to prepare an injectable tissue repair filling material, wherein the dispersant included a gelling agent and pure water, and was composed of 2 g of sodium carboxymethyl cellulose (substitution degree 0.7) with a molecular weight of 0.25 MDa and 94.5 g of pure water.

[0057] Embodiment 14 Example 14 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 4.5 g of the ECM microspheres prepared in Example 2 were mixed with 95.5 g of a dispersant to prepare an injectable tissue repair filling material, wherein the dispersant includes a gelling agent and pure water, and is composed of 1 g of sodium hyaluronate with a molecular weight of 3 MDa, 1 g of sodium carboxymethyl cellulose with a molecular weight of 0.25 MDa (degree of substitution of 0.9) and 93.5 g of pure water.

[0058] Embodiment 15 Example 15 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 3.5 g of the ECM microspheres prepared in Example 2 were mixed with 96.5 g of a dispersant to prepare an injectable tissue repair filling material, wherein the dispersant includes a gelling agent and pure water, and is composed of 1.5 g of sodium carboxymethyl cellulose with a molecular weight of 0.7 MDa (degree of substitution of 0.9), 0.3 g of lidocaine and 94.7 g of pure water.

[0059] Example 16 Example 16 provides a method for preparing an injectable tissue repair filling material, and the specific operations are as follows: 3.5 g of the ECM microspheres prepared in Example 2 were mixed with 96.5 g of a dispersant to prepare an injectable tissue repair filling material. The dispersant included a gelling agent and pure water, and was composed of 1.5 g of sodium carboxymethyl cellulose with a molecular weight of 0.7 MDa (degree of substitution of 0.9), 0.2 g of compound vitamins, 0.2 g of glutathione, 0.3 g of lidocaine and 94.3 g of pure water.

[0060] Performance Test 2 3. Sedimentation test The injectable tissue repair filling materials prepared in Examples 6-16 were placed at room temperature and pressure for 6 months, during which the sedimentation of the ECM microspheres was observed. The specific results are shown in Table 3.

[0061] Table 3 Sedimentation test results It is not difficult to see from the results in Table 3 that the injectable tissue repair filling materials prepared in Examples 6 to 16 of the present application have good stability and will not delaminate or settle even if placed for a long time at room temperature and pressure.

[0062] 4. Elastic modulus The elastic modulus of the injectable tissue repair filling materials prepared in Examples 6-16 was tested by compression method using a universal mechanical tensile machine. The test method is as follows: the gel is filled into a sample tank of 3×3×1 cm, a probe with a surface area of ​​1×1 cm is used to compress and measure the maximum stress value at a speed of 5 cm / s, and the elastic modulus is calculated by drawing a curve and calculating. The specific results are shown in Table 4.

[0063] Table 4 Elastic modulus test results It can be seen from the results in Table 4 that the injectable tissue repair filling materials prepared in Examples 6 to 16 of the present application all have a relatively high elastic modulus.

[0064] 5. Light transmittance At room temperature, the luminous flux of the samples of Examples 6-16 at 400 nm was tested using a spectrometer, and the transmittance of the samples was obtained by calculating the ratio of the luminous flux to the incident luminous flux. The specific results are shown in Table 5.

[0065] Table 5 Transmittance test results Example No. Light transmittance Example 6 55% Example 7 52% Example 8 42% Example 9 35% Example 10 37% Embodiment 11 43% Example 12 40% Embodiment 13 46% Embodiment 14 34% Embodiment 15 45% Example 16 46% It can be seen from the results in Table 5 that the injectable tissue repair filling materials prepared in Examples 6 to 16 of the present application have low light transmittance, which reduces direct light and prevents the occurrence of the Tyndall effect.

[0066] 6. In vivo experiments This part of the experiment is used to inject the injectable tissue repair filling material prepared in Example 6 as a sample into the experimental rats for in vivo experiments, and a normal saline control group is set up for comparison. The experimental process is: select healthy adult rats, inject 0.5% sodium pentobarbital solution at a weight ratio of 40.0 mg / kg for anesthesia, shave the back of the rats and disinfect them with iodine and alcohol. Select a single point on the back of the rat, and use a syringe to slowly inject 0.2 mL of the filling material / normal saline into the subcutaneous part.

[0067] 6.1 Samples were collected at 2 weeks, 4 weeks, 6 weeks, and 8 weeks after injection, and the removed tissue blocks were quickly immersed in 4% paraformaldehyde solution for fixation for more than 24 hours. The fixed tissues were placed in gradient ethanol for dehydration, and xylene was used for transparent treatment. The transparent tissue blocks were immersed in molten paraffin for embedding. The embedded wax blocks were cut into 5-10 μm thick slices using a tissue slicer. The slices were attached to glass slides and placed in an oven for drying. They were stained according to the standard HE staining process, including dewaxing, hydration, staining, dehydration, transparentization, and sealing. The slices were observed under a microscope to evaluate the degradation of the filling material. Figure 2The following are the results of rat back dermal slices after sample injection in Example 6, where a, b, c, and d respectively show the results of rat back dermal slices after sample injection for 2 weeks, 4 weeks, 6 weeks, and 8 weeks. Figure 2 No obvious inflammatory reaction was observed, and the dermis thickness increased over time after the material was implanted, proving that the material was safe and effective after implantation.

[0068] 6.2 Eight weeks after injection, the ELISA kit was used to detect the dermal collagen concentration (ng / ml) within a circle with a diameter of 1 cm at the injection point. Figure 3 The figure shows the comparison of dermal collagen concentration of the sample of Example 6 and the saline control group 8 weeks after injection. Figure 3 It is not difficult to find that the dermal collagen concentration around the injection point of the sample increased significantly.

[0069] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. An ECM microsphere, It is characterized in that The preparation method of the ECM microspheres comprises the following steps: S1: Take animal-derived tissue materials and prepare decellularized extracellular matrix; S2: dehydrating and drying the decellularized extracellular matrix described in step S1 to obtain an ECM material; S3: subjecting the ECM material described in step S2 to water absorption treatment, and then to low-temperature wet grinding treatment to obtain wet ECM particles; S4: drying the ECM microparticles from step S3 and then sieving them to obtain ECM microspheres of 10-150 μm.

2. The ECM microspheres according to claim 1, It is characterized in that The animal source described in step S1 is selected from one of humans, cattle, pigs, and sheep, and the tissue material is selected from one or more of dermis, muscle, tendon, heart, fat, small intestine, umbilical cord, placenta, blood vessel, nerve, bone, and cartilage.

3. The ECM microspheres according to claim 1, It is characterized in that In step S3, the water absorption of the ECM material is 10% to 400% of the mass of the ECM material.

4. The ECM microspheres according to claim 1, It is characterized in that The specific operation of the low-temperature wet grinding treatment in step S3 is as follows: grinding at a temperature of -200°C to -30°C for 10-300s, pausing for 5-60s, and repeating this process 10-300 times.

5. An injectable tissue repair filling material, It is characterized in that The method comprises a dispersant and the ECM microspheres according to any one of claims 1 to 4, wherein the ECM microspheres account for 0.2wt.%-10wt.%.

6. The injectable tissue repair filling material according to claim 5, It is characterized in that By weight percentage, the dispersant comprises: 5%-10% gel, The balance is solvent.

7. The injectable tissue repair filling material according to claim 6, It is characterized in that The gel is selected from one or more of carboxymethyl chitin, carboxymethyl chitosan, oxidized cellulose, carboxymethyl cellulose, sodium carboxymethyl cellulose, hydroxyethyl cellulose, sodium hydroxyethyl cellulose, hyaluronic acid, sodium hyaluronate, chondroitin sulfate, sodium trehalose, polyglutamic acid, porcine natural collagen, bovine natural collagen, human natural collagen, and recombinant human collagen; The solvent is pure water.

8. The injectable tissue repair filling material according to claim 7, It is characterized in that The gelling agent includes a cross-linked gel and / or a non-cross-linked gel.

9. The injectable tissue repair filling material according to claim 5, It is characterized in that In terms of mass percentage, the dispersant comprises: 5%-10% gel, 1%-5% non-gel agent, The balance is solvent; The non-gel agent includes one or more of a nutrient, an osmotic pressure balancer, a growth factor, and an anesthetic.

10. Use of an injectable tissue repair filling material as claimed in any one of claims 5 to 9, It is characterized in that Used to prepare medical cosmetic injectable filling preparations.

Citation Information

Cited By

  • Composition for improving skin state, application of composition and medical beauty material

    CN120837724A

  • A composition for improving the condition of skin, its use and a medical aesthetic material

    CN120837724B

  • Absorbable injection filler based on four-phase gradient and preparation method thereof