Preparation method of macroporous hollow water treatment material

By coating the polyethylene microbeads with samarium titanate-copper oxide composite coating, the large-pore hollow water treatment materials are prepared, which solves the problems of low treatment efficiency of toxic and harmful organic pollutants and difficulty in separation of photocatalysts in traditional technology, and achieves high efficiency Wastewater treatment and material recycling.

CN118892838AActive Publication Date: 2024-11-05SHENYANG LIGONG UNIV

Patent Information

Application Number
CN202410934627.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

Traditional biochemical treatment technology is not efficient when dealing with toxic and harmful organic pollutants, and it is difficult to separate the photocatalyst from water, which affects the efficiency of wastewater treatment and resource recycling.

Method used

By adopting the preparation method of large pore hollow water treatment materials, by coating the samarium titanate-copper oxide composite active coating on polyethylene microbeads, a material with a density slightly greater than water is formed, with good suspension performance and photocatalytic activity, suitable for Purification and treatment of organic pollutants in wastewater, and easy separation from water after treatment, for easy recycling.

Benefits of technology

It realizes the activity of rapidly degrading organic pollutants in water, improves wastewater treatment efficiency, and facilitates the recycling of materials, and is suitable for various types of wastewater treatment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of a macroporous hollow water treatment material, and belongs to the field of environmental pollution purification materials. The method mainly comprises the following preparation steps: preparing a sol precursor, gelatinizing and laminating polyethylene microbeads, performing solvothermal synthesis and performing heat treatment. The polyethylene microbeads serve as an organic template material, the polyethylene microbeads are coated with the samarium titanate-copper oxide composite active coating, the density of the macroporous hollow water treatment material is slightly larger than that of water, the macroporous hollow water treatment material has ideal suspension performance under slight stirring, and the macroporous hollow water treatment material can be used for purification treatment of organic pollutants in wastewater; and the material is easily separated from water after the water treatment process is completed, so that the material is convenient to recycle. The macroporous hollow water treatment material has the activity of rapidly degrading organic pollutants in water, and has a wide application prospect in the field of treatment of various organic wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of environmental pollution purification materials, and in particular relates to a method for preparing a macroporous hollow water treatment material. Background Art

[0002] Industrial and civil wastewater contains a variety of pollutants, among which organic pollutants include various toxic and harmful organic substances. The treatment method for organic pollutants in wastewater can adopt traditional biochemical treatment technology, but due to the toxic effect of toxic and harmful substances on the microorganisms that are essential in the biochemical treatment process, the treatment efficiency of the biochemical treatment process is not satisfactory.

[0003] Photocatalytic oxidation technology is a deep oxidation technology that can degrade most organic pollutants in water. After half a century of in-depth research, photocatalytic technology is playing an increasingly important role in the purification of toxic and harmful organic pollutants. The key to the photocatalytic treatment process is to ensure that the catalyst is fully mixed with the organic pollutants in the wastewater, so that these organic substances can be decomposed under light to achieve the purpose of purification. In the continuous large-scale wastewater treatment process, the separation of photocatalysts and water is an important factor. Photocatalytic materials must not only have high treatment activity, but also be easy to separate from water after treatment for recycling. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention aims to provide a method for preparing a macroporous hollow water treatment material, which can be used in the photocatalytic purification process of organic pollutants in sewage.

[0005] The technical solution adopted by the present invention is:

[0006] A method for preparing a macroporous hollow water treatment material comprises the following process steps:

[0007] Step 1: Preparation of sol precursor

[0008] (1) Add 160-180 mL of anhydrous ethanol, 7.5-9 mL of 1,3-butanediol, 5.5-6.5 g of samarium nitrate, and 8.0-9.5 mL of n-butyl titanate into a flask in sequence and stir until solution A is formed;

[0009] (2) Add 2.3-2.7 g of Tween 80, 3.1-3.6 g of copper chloride, and 1.2-1.3 mL of acetic acid to 35-45 mL of pure water and stir until solution B is formed;

[0010] (3) Slowly adding solution B into solution A, heating to 65° C., and reflux for 75 min to obtain a sol precursor;

[0011] Step 2: Polyethylene microbeads glue coating

[0012] (1) Add 20 g of polyethylene microbeads into a flask containing the sol precursor and continue to reflux at 65 °C for 50 min to obtain a suspension A;

[0013] (2) Concentrating suspension A by rotary evaporation at 85° C. until the volume of suspension A is reduced by 30%, thereby obtaining suspension B;

[0014] Step 3: Solvothermal Synthesis

[0015] (1) Transfer suspension B into a stainless steel high-pressure reactor, control the solution temperature in the reactor to 155-165° C., the pressure in the reactor to less than 2.2 MPa, react for 60 hours, and then cool to room temperature to obtain suspension C;

[0016] (2) Filtering the suspension C, and drying the filtered solid at 150° C. for 18 h to obtain a solid A;

[0017] Step 4: Heat Treatment

[0018] (1) placing the solid A obtained in step 3 in a programmable box-type electric furnace, raising the temperature to 360° C. at a heating rate of 5° C. / min, and keeping the temperature for 3 h;

[0019] (2) continuing to raise the temperature to 670-750° C. at a heating rate of 10° C. / min and calcining for 5 h to obtain a calcined product;

[0020] (3) Cooling the calcined product to room temperature and grinding it to form loose powder to obtain a macroporous hollow water treatment material.

[0021] Furthermore, the polyethylene microbeads described in step (2) have a particle diameter of 0.7 to 0.8 mm and a density of 1.0 g / mL.

[0022] A macroporous hollow water treatment material is prepared by the above method, wherein the macroporous hollow water treatment material is coated with a samarium titanate-copper oxide composite active coating on polyethylene microbeads, so that the coating and the polyethylene microbeads are firmly composited;

[0023] Furthermore, the samarium titanate-copper oxide composite active coating is composed of two photocatalytically active substances, samarium titanate and copper oxide, wherein the mass percentage of samarium titanate in the macroporous hollow water treatment material is 5.6% to 5.9%, and the mass percentage of copper oxide in the macroporous hollow water treatment material is 3.7% to 4.1%. The relative mass ratio of samarium titanate and copper oxide is an important factor in ensuring material stability and good photocatalytic activity.

[0024] Furthermore, the macroporous hollow water treatment material maintains stable structure and performance below 650°C.

[0025] Furthermore, the macroporous hollow water treatment material particles have a diameter of 0.8 to 0.9 mm and a density of 1.2 to 1.3 g / mL.

[0026] Compared with the prior art, the method for preparing a macroporous hollow water treatment material of the present invention has the following advantages:

[0027] The present invention uses polyethylene microbeads as an organic template material, and coats the polyethylene microbeads with a samarium titanate-copper oxide composite active coating. The density of the material is slightly greater than that of water, and it has an ideal suspension performance under slight stirring, and can be used for the purification of organic pollutants in wastewater; and the material is easy to separate from water after the water treatment process is completed, which is convenient for the recycling of the material. The method provided by the present invention can scientifically regulate the density of the macroporous hollow water treatment material according to the actual situation of the wastewater, so that it is suitable for various types of wastewater. The macroporous hollow water treatment material has the activity of rapidly degrading organic pollutants in water, and has broad application prospects in various organic wastewater treatment fields. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples where no specific conditions are indicated are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0029] Unless otherwise specified, all chemical raw materials mentioned are pure materials.

[0030] Example 1

[0031] A method for preparing a macroporous hollow water treatment material comprises the following process steps:

[0032] Step 1: Preparation of sol precursor

[0033] (1) Add 160 mL of anhydrous ethanol, 7.5 mL of 1,3-butanediol, 5.5 g of samarium nitrate, and 8.0 mL of n-butyl titanate into a flask in sequence and stir until solution A is formed;

[0034] (2) Add 2.3 g of Tween 80, 3.1 g of copper chloride, and 1.2 mL of acetic acid to 35 mL of pure water and stir until solution B is formed;

[0035] (3) Solution B was slowly added into solution A, heated to 65°C, and refluxed for 75 min to obtain a sol precursor.

[0036] Step 2: Polyethylene microbeads glue coating

[0037] (1) Add 20 g of polyethylene microbeads into a flask containing the sol precursor and continue to reflux at 65 °C for 50 min to obtain a suspension A;

[0038] (2) The suspension A was concentrated by rotary evaporation at 85°C until the volume of the solution was reduced by 30%, thereby obtaining a suspension B.

[0039] Step 3: Solvothermal Synthesis

[0040] (1) Transfer suspension B into a stainless steel high-pressure reactor, control the solution temperature in the reactor to 155° C., the pressure in the reactor to less than 2.2 MPa, react for 60 hours, and then cool to room temperature to obtain suspension C;

[0041] (2) The suspension C was filtered, and the solid matter obtained by filtration was dried at 150° C. for 18 h to obtain a solid matter A.

[0042] Step 4: Heat Treatment

[0043] (1) placing the solid A obtained in step 3 in a programmable box-type electric furnace, raising the temperature to 360° C. at a heating rate of 5° C. / min, and keeping the temperature for 3 h;

[0044] (2) continue to increase the temperature to 670°C at a heating rate of 10°C / min and calcine for 5 h;

[0045] (3) The calcined product was cooled to room temperature and gently ground to form loose powder, thereby obtaining a macroporous hollow water treatment material with a particle diameter of 0.8 to 0.9 mm and a density of 1.2 g / mL.

[0046] Example 2

[0047] A method for preparing a macroporous hollow water treatment material comprises the following process steps:

[0048] Step 1: Preparation of sol precursor

[0049] (1) Add 165 mL of anhydrous ethanol, 7.8 mL of 1,3-butanediol, 5.7 g of samarium nitrate, and 8.3 mL of n-butyl titanate into a flask in sequence and stir until solution A is formed;

[0050] (2) Add 2.4 g of Tween 80, 3.2 g of copper chloride, and 1.2 mL of acetic acid to 37 mL of pure water and stir until solution B is formed;

[0051] (3) Solution B was slowly added into solution A, heated to 65°C, and refluxed for 75 min to obtain a sol precursor.

[0052] Step 2: Polyethylene microbeads glue coating

[0053] (1) Add 20 g of polyethylene microbeads into a flask containing the sol precursor and continue to reflux at 65 °C for 50 min to obtain a suspension A;

[0054] (2) The suspension A was concentrated by rotary evaporation at 85°C until the volume of the solution was reduced by 30%, thereby obtaining a suspension B.

[0055] Step 3: Solvothermal Synthesis

[0056] (1) Transfer suspension B into a stainless steel high-pressure reactor, control the solution temperature in the reactor to 158° C., the pressure in the reactor to less than 2.2 MPa, react for 60 hours, and then cool to room temperature to obtain suspension C;

[0057] (2) The suspension C was filtered, and the solid matter obtained by filtration was dried at 150° C. for 18 h to obtain a solid matter A.

[0058] Step 4: Heat Treatment

[0059] (1) placing the solid A obtained in step 3 in a programmable box-type electric furnace, raising the temperature to 360° C. at a heating rate of 5° C. / min, and keeping the temperature for 3 h;

[0060] (2) continue to increase the temperature to 690°C at a heating rate of 10°C / min and calcine for 5 h;

[0061] (3) The calcined product was cooled to room temperature and gently ground to form loose powder, thereby obtaining a macroporous hollow water treatment material with a particle diameter of 0.8 to 0.9 mm and a density of 1.2 g / mL.

[0062] Example 3

[0063] A method for preparing a macroporous hollow water treatment material comprises the following process steps:

[0064] Step 1: Preparation of sol precursor

[0065] (1) Add 170 mL of anhydrous ethanol, 8.2 mL of 1,3-butanediol, 6.0 g of samarium nitrate, and 8.7 mL of n-butyl titanate into a flask in sequence and stir until solution A is formed;

[0066] (2) Add 2.5 g of Tween 80, 3.4 g of copper chloride, and 1.2 mL of acetic acid to 40 mL of pure water and stir until solution B is formed;

[0067] (3) Solution B was slowly added into solution A, heated to 65°C, and refluxed for 75 min to obtain a sol precursor.

[0068] Step 2: Polyethylene microbeads glue coating

[0069] (1) Add 20 g of polyethylene microbeads into a flask containing the sol precursor and continue to reflux at 65 °C for 50 min to obtain a suspension A;

[0070] (2) The suspension A was concentrated by rotary evaporation at 85°C until the volume of the solution was reduced by 30%, thereby obtaining a suspension B.

[0071] Step 3: Solvothermal Synthesis

[0072] (1) Transfer suspension B into a stainless steel high-pressure reactor, control the solution temperature in the reactor to 160° C., the pressure in the reactor to less than 2.2 MPa, react for 60 hours, and then cool to room temperature to obtain suspension C;

[0073] (2) The suspension C was filtered, and the solid matter obtained by filtration was dried at 150° C. for 18 h to obtain a solid matter A.

[0074] Step 4: Heat Treatment

[0075] (1) placing the solid A obtained in step 3 in a programmable box-type electric furnace, raising the temperature to 360° C. at a heating rate of 5° C. / min, and keeping the temperature for 3 h;

[0076] (2) continue to increase the temperature to 710°C at a heating rate of 10°C / min and calcine for 5 h;

[0077] (3) The calcined product was cooled to room temperature and gently ground to form loose powder, thereby obtaining a macroporous hollow water treatment material with a particle diameter of 0.8 to 0.9 mm and a density of 1.25 g / mL.

[0078] Example 4

[0079] A method for preparing a macroporous hollow water treatment material comprises the following process steps:

[0080] Step 1: Preparation of sol precursor

[0081] (1) Add 175 mL of anhydrous ethanol, 8.5 mL of 1,3-butanediol, 6.2 g of samarium nitrate, and 9.1 mL of n-butyl titanate into a flask in sequence and stir until solution A is formed;

[0082] (2) Add 2.6 g of Tween 80, 3.5 g of copper chloride, and 1.3 mL of acetic acid to 42 mL of pure water and stir until solution B is formed;

[0083] (3) Solution B was slowly added into solution A, heated to 65°C, and refluxed for 75 min to obtain a sol precursor.

[0084] Step 2: Polyethylene microbeads glue coating

[0085] (1) Add 20 g of polyethylene microbeads into a flask containing the sol precursor and continue to reflux at 65 °C for 50 min to obtain a suspension A;

[0086] (2) The suspension A was concentrated by rotary evaporation at 85°C until the volume of the solution was reduced by 30%, thereby obtaining a suspension B.

[0087] Step 3: Solvothermal Synthesis

[0088] (1) Transfer suspension B into a stainless steel high-pressure reactor, control the solution temperature in the reactor to 162° C., the pressure in the reactor to less than 2.2 MPa, react for 60 hours, and then cool to room temperature to obtain suspension C;

[0089] (2) The suspension C was filtered, and the solid matter obtained by filtration was dried at 150° C. for 18 h to obtain a solid matter A.

[0090] Step 4: Heat Treatment

[0091] (1) placing the solid A obtained in step 3 in a programmable box-type electric furnace, raising the temperature to 360° C. at a heating rate of 5° C. / min, and keeping the temperature for 3 h;

[0092] (2) continue to increase the temperature to 730°C at a heating rate of 10°C / min and calcine for 5 h;

[0093] (3) The calcined product was cooled to room temperature and gently ground to form loose powder, thereby obtaining a macroporous hollow water treatment material with a particle diameter of 0.8 to 0.9 mm and a density of 1.3 g / mL.

[0094] Example 5

[0095] A method for preparing a macroporous hollow water treatment material comprises the following process steps:

[0096] Step 1: Preparation of sol precursor

[0097] (1) Add 180 mL of anhydrous ethanol, 9 mL of 1,3-butanediol, 6.5 g of samarium nitrate, and 9.5 mL of n-butyl titanate into a flask in sequence and stir until solution A is formed;

[0098] (2) Add 2.7 g of Tween 80, 3.6 g of copper chloride, and 1.3 mL of acetic acid to 45 mL of pure water and stir until solution B is formed;

[0099] (3) Solution B was slowly added into solution A, heated to 65°C, and refluxed for 75 min to obtain a sol precursor.

[0100] Step 2: Polyethylene microbeads glue coating

[0101] (1) Add 20 g of polyethylene microbeads into a flask containing the sol precursor and continue to reflux at 65 °C for 50 min to obtain a suspension A;

[0102] (2) The suspension A was concentrated by rotary evaporation at 85°C until the volume of the solution was reduced by 30%, thereby obtaining a suspension B.

[0103] Step 3: Solvothermal Synthesis

[0104] (1) Transfer suspension B into a stainless steel high-pressure reactor, control the solution temperature in the reactor to 165° C., the pressure in the reactor to less than 2.2 MPa, react for 60 hours, and then cool to room temperature to obtain suspension C;

[0105] (2) The suspension C was filtered, and the solid matter obtained by filtration was dried at 150° C. for 18 h to obtain a solid matter A.

[0106] Step 4: Heat Treatment

[0107] (1) placing the solid A obtained in step 3 in a programmable box-type electric furnace, raising the temperature to 360° C. at a heating rate of 5° C. / min, and keeping the temperature for 3 h;

[0108] (2) continue to increase the temperature to 750°C at a heating rate of 10°C / min and calcine for 5 h;

[0109] (3) The calcined product was cooled to room temperature and gently ground to form loose powder, thereby obtaining a macroporous hollow water treatment material with a particle diameter of 0.8 to 0.9 mm and a density of 1.3 g / mL.

Claims

1. A method for preparing a macroporous hollow water treatment material, characterized in that: The process steps include: Step 1: Preparation of sol precursor (1) Add 160-180 mL of anhydrous ethanol, 7.5-9 mL of 1,3-butanediol, 5.5-6.5 g of samarium nitrate, and 8.0-9.5 mL of n-butyl titanate into a flask in sequence and stir until solution A is formed; (2) Add 2.3-2.7 g of Tween 80, 3.1-3.6 g of copper chloride, and 1.2-1.3 mL of acetic acid to 35-45 mL of pure water and stir until solution B is formed; (3) Slowly adding solution B into solution A, heating to 65° C., and reflux for 75 min to obtain a sol precursor; Step 2: Polyethylene microbeads glue coating (1) Add 20 g of polyethylene microbeads into a flask containing the sol precursor and continue to reflux at 65 °C for 50 min to obtain a suspension A; (2) Concentrating suspension A by rotary evaporation at 85° C. until the volume of suspension A is reduced by 30%, thereby obtaining suspension B; Step 3: Solvothermal Synthesis (1) Transfer suspension B into a stainless steel high-pressure reactor, control the solution temperature in the reactor to 155-165° C., the pressure in the reactor to less than 2.2 MPa, react for 60 hours, and then cool to room temperature to obtain suspension C; (2) Filtering the suspension C, and drying the filtered solid at 150° C. for 18 h to obtain a solid A; Step 4: Heat Treatment (1) placing the solid A obtained in step 3 in a programmable box-type electric furnace, raising the temperature to 360° C. at a heating rate of 5° C. / min, and keeping the temperature for 3 h; (2) continuing to raise the temperature to 670-750° C. at a heating rate of 10° C. / min and calcining for 5 h to obtain a calcined product; (3) Cooling the calcined product to room temperature and grinding it to form loose powder to obtain a macroporous hollow water treatment material.

2. The method for preparing a macroporous hollow water treatment material according to claim 1, characterized in that: The polyethylene microbeads described in step (2) have a particle diameter of 0.7-0.8 mm and a density of 1.0 g / mL.

3. A macroporous hollow water treatment material, prepared by the method of claim 1 or 2, characterized in that: The macroporous hollow water treatment material is coated with a samarium titanate-copper oxide composite active coating on polyethylene microbeads, and the coating is firmly composited with the polyethylene microbeads.

4. A macroporous hollow water treatment material according to claim 3, characterized in that: The samarium titanate-copper oxide composite active coating is composed of two photocatalytically active substances, samarium titanate and copper oxide, wherein the mass percentage of samarium titanate in the macroporous hollow water treatment material is 5.6% to 5.9%, and the mass percentage of copper oxide in the macroporous hollow water treatment material is 3.7% to 4.1%. The relative mass ratio of samarium titanate and copper oxide is an important factor in ensuring material stability and good photocatalytic activity.

5. The macroporous hollow water treatment material according to claim 3, characterized in that: The macroporous hollow water treatment material maintains stable structure and performance at a temperature below 650°C.

6. The macroporous hollow water treatment material according to claim 3, characterized in that: The macroporous hollow water treatment material particles have a diameter of 0.8 to 0.9 mm and a density of 1.2 to 1.3 g / mL.

Citation Information

Patent Citations

  • Method of preparing magnetic hollow micro-nano ball with template of high molecule micro-nano ball

    CN101183588A

  • Preparation method of density-adjustable hollow strontium titanate material

    CN106348339A

  • Preparation method of macroporous hollow cerium titanate microspheres

    CN107082447A

  • Preparation method of suspensible praseodymium titanate material

    CN108033483A

  • Preparation method of hollow microsphere for treating oil gas

    CN108126676A

Cited By

  • Organic pollution purification capillary tube and preparation method thereof

    CN119503948A