Kaolin-loaded nano g-C3N4 composite photocatalytic material and preparation method thereof

By uniformly loading nanog-C3N4 on the kaolin flake layer, using intercalation-stripping method and ultrasonic treatment, the aggregation and high cost problems of a single g-C3N4 photocatalyst are solved, and efficient photocatalytic performance and low-cost wastewater are achieved. deal with.

CN118892857APending Publication Date: 2024-11-05NORTH CHINA UNIV OF WATER RESOURCES & ELECTRIC POWER +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410922550.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The single graphite phase carbon nitride (g-C3N4) photocatalyst is limited by its practical application due to its prone to agglomeration, high carrier recombination rate, poor adsorption performance and weak visible light response. In addition, the existing Pd-Ag loading of g-C3N4 light is limited. The catalyst preparation process is complex and costly, making it difficult to produce on a large scale.

Method used

Kaolin was used as a support, and nanog-C3N4 was uniformly loaded on the surface of the kaolin flake by solid phase sintering. The structure of kaolin was optimized to improve the loading and photocatalytic properties of nanog-C3N4 by intercalation-stripping method and ultrasonic treatment.

Benefits of technology

It improves the adsorption and capture performance of composite materials on pollutants, avoids the agglomeration of pure g-C3N4, reduces the production cost and production difficulty, provides more efficient photocatalytic performance, and is suitable for wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892857A_ABST
    Figure CN118892857A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of non-metallic mineral materials and environmental engineering, in particular to a kaolin loaded nano g-C3N4 composite photocatalytic material and a preparation method thereof. The composite photocatalytic material is prepared by uniformly loading nano g-C3N4 on the surface of kaolin, wherein the average particle size of the nano g-C3N4 is 3-5 [mu] m; the loading capacity of the nano g-C3N4 is 30-70% of the mass of the composite material; the preparation method comprises the following steps: by taking a kaolin lamella as a carrier and melamine as a carbon source and a nitrogen source, loading nano g-C3N4 on the surface of the kaolin lamella through a solid-phase sintering method; according to the preparation method disclosed by the invention, the pollutant adsorption and capture performance of the composite material is improved by utilizing a kaolin carrier effect and relatively strong adsorption capacity, the agglomeration problem of pure g-C3N4 is solved, and the photocatalytic performance of the composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of non-metallic mineral materials and environmental engineering, and in particular to a kaolin-loaded nano g-C3N4 composite photocatalytic material and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of modern industry, the dye wastewater, antibiotic wastewater and heavy metal ion wastewater generated in its production process endanger people's health, easily induce cancer, and even cause death. In order to solve the problem of wastewater treatment, photocatalytic technology is usually used to degrade organic pollutants. Photocatalytic technology has attracted widespread attention due to its green, high efficiency, simple operation and no secondary pollution. Graphitic carbon nitride (g-C3N4) is a semiconductor photocatalyst with visible light response, stable physicochemical properties and suitable bandgap width. However, the single g-C3N4 photocatalyst has defects such as easy agglomeration, high carrier recombination rate, poor adsorption performance and weak visible light response ability, which greatly limits its practical application.

[0003] The patent application with application number 202211054775.8 discloses a Pd-Ag loaded g-C3N4 nanosheet photocatalyst, preparation method and application. Although the nano Pd and nano Ag in the photocatalyst can promote the effective separation of g-C3N4 photogenerated carriers and further improve the photocatalytic activity of the g-C3N4 nanosheet photocatalyst, the reaction time in the preparation process is long and the production cost is high, and it cannot be mass-produced.

[0004] Kaolin is a 1:1 type layered silicate clay mineral with ion exchange properties and adsorption capacity. Its microscopic morphology is flaky. This flaky structure has a large specific surface area, which is very conducive to the loading of nano g-C3N4, avoiding the agglomeration of pure g-C3N4 and improving the photocatalytic performance of g-C3N4. In addition, kaolin is widely available, inexpensive, and environmentally friendly during use. Based on this, the present invention application proposes a kaolin-loaded nano g-C3N4 composite photocatalytic material with kaolin as a carrier and a preparation method thereof. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a kaolin-loaded nano g-C3N4 composite photocatalytic material and a preparation method thereof.

[0006] The technical solution of the present invention is: a kaolin-loaded nano g-C3N4 composite photocatalytic material, wherein the composite photocatalytic material is a kaolin surface uniformly loaded with nano g-C3N4, the average particle size of the nano g-C3N4 is 3-5μm, and the nano g-C3N4 is uniformly and densely distributed on the surface of the kaolin layer, and the loading amount of the nano g-C3N4 is 30-70% of the mass of the composite material.

[0007] Furthermore, the kaolin and nano g-C3N4 are both in a flaky structure;

[0008] Note: The thin sheet structure makes it easier to combine the loads of the two.

[0009] The present invention also provides a method for preparing a kaolin-loaded nano g-C3N4 composite photocatalytic material, using a kaolin sheet as a carrier and melamine as a carbon source and a nitrogen source, and loading nano g-C3N4 on the surface of the kaolin sheet by a solid phase sintering method, comprising the following steps:

[0010] The kaolin and melamine are mixed in a mass ratio of 1:0.5-4, and then ground in a mortar for 0.5-1h to obtain a mixed powder; the mixed powder is then heated and calcined at a heating rate of 2.5-15°C / min, and the temperature is increased to 450-650°C and then kept warm for 1-5h to obtain a calcined product; finally, the calcined product is ground into 200-250 meshes to obtain a kaolin-loaded g-C3N4 composite photocatalytic material;

[0011] Description: The intercalation-stripping method and solid-phase sintering method in the present invention is to intercalate and ultrasonically treat kaolin, and then grind the kaolin and melamine mixture in a solid form in a mortar. Only one step of heat treatment is required, the preparation process is simple, the reaction conditions are mild, and it has good application prospects.

[0012] Furthermore, the kaolin is intercalated-exfoliated kaolin,

[0013] The preparation method of the intercalation-stripping kaolin is as follows: kaolin and an organic intercalation agent are fully mixed in a reaction kettle at a mass ratio of 1:1 to obtain a mixture, water is then added at a ratio of 0.15-0.25 g / mL, and the mixture is centrifuged at a speed of 6000-8000 r / min at 40-60° C. for 24-48 hours, the supernatant is removed, and the lower precipitate is washed and filtered, and the mixture is dried in a blast drying oven at 75-85° C. for 1-12 hours to obtain a dry product, and deionized water is then added to the dry product at a ratio of 1 g: 4.8-5.2 mL, and the mixture is ultrasonically assisted at a temperature of 50-70° C. for 6-10 minutes to obtain the intercalation-stripping kaolin;

[0014] Description: By preparing intercalation-stripping kaolin, kaolin can be loaded in the form of flakes, further providing better conditions for the loading of graphite phase carbon nitride, thereby improving the preparation efficiency of composite photocatalytic materials; appropriate ultrasonic time will make the reaction complete and avoid incomplete stripping of the product.

[0015] Furthermore, the parameters of ultrasound-assisted treatment are: ultrasonic frequency of 25-40KHz, ultrasonic power of 80-100kw;

[0016] Note: Too high ultrasonic frequency and power will break the product into pieces, which is not conducive to the loading of the catalyst.

[0017] Furthermore, the lower precipitate is washed, filtered and then subjected to high pressure treatment.

[0018] The method of high pressure treatment is:

[0019] 1) placing the lower precipitate in a reactor, and introducing an inert gas with a purity of 99-99.9% until the pressure in the reactor reaches 6-9 MPa;

[0020] 2) adding dispersant and methanol to the reactor in a weight ratio of lower layer precipitation: dispersant: methanol of 1:0.25-0.4:0.8-1.2, continuing centrifugal treatment for 5-10 minutes to obtain a dispersion, and then spraying the dispersion along the nozzle of the reactor at a spray rate of 200-500 mL / min, while releasing inert gas at a rate of 0.2-0.5 MPa / min to obtain a spray; wherein the pressure in the reactor is reduced by 1-1.5 MPa, the spray is collected once, and the inert gas release rate is reduced by 0.05-0.1 MPa / min;

[0021] 3) Repeat step 2) 2-3 times to obtain pre-intercalation-stripping kaolin; wherein the total amount of dispersant and methanol added each time is 45-65% of the amount added last time, the centrifugal treatment parameters and the dispersion spraying speed are unchanged each time, and the spray obtained each time is collected and added back to the reactor;

[0022] Description: The addition of dispersant can effectively improve the dispersibility of kaolin particles in the solvent and prevent particle agglomeration and sedimentation. This helps to transfer energy more evenly in the subsequent ultrasonic treatment, improve the stripping effect and the quality of the stripping product; methanol, as an organic solvent, can interact with the inorganic components in kaolin, which helps the further penetration of the intercalation agent and the stripping process. High-pressure treatment can accelerate the diffusion and reaction of the intercalation agent between kaolin layers, thereby more effectively achieving intercalation stripping. High pressure can also increase the solvent's ability to penetrate kaolin, which helps to complete the intercalation stripping;

[0023] Through multiple centrifugation and high-speed spraying treatments, the dispersibility of kaolin particles can be further improved, agglomeration can be reduced, and thus its specific surface area can be increased. The increase in specific surface area means that kaolin has more active sites and stronger adsorption capacity, which is conducive to the uniform loading and stable attachment of carbon nitride on its surface; during multiple spraying treatments, the layered structure of kaolin can be further optimized. This method can effectively reduce the particle size of kaolin and may make its flakes thinner, making the interlayer spacing more uniform and the layer plates flatter. This optimized structure is more conducive to the embedding and loading of carbon nitride molecules, improving the stability and efficiency of the loading.

[0024] Further, the organic intercalant is one of dimethyl sulfoxide, potassium acetate or urea, and the inert gas is argon or nitrogen;

[0025] Description: Dimethyl sulfoxide, potassium acetate or urea as small molecule organic intercalation can improve the fineness of the exfoliated kaolin, thereby improving the loading of carbon nitride. Using argon and nitrogen for pressure regulation can effectively achieve pressure regulation without affecting the composition of kaolin.

[0026] Further, the dispersant comprises, by mass percentage, 0.15-0.2% of a silicon source, 15-20% of polyethyleneimine, 5-8% of acetone, 0.25-0.5% of H2O2, and the balance of sodium hexametaphosphate;

[0027] Description: Conventional mechanical grinding process can increase the surface area of ​​kaolinite, but this method cannot significantly reduce the thickness of the lamellae. At the same time, the strong impact and shear force of the grinding medium will seriously damage the lamellae crystal structure of kaolinite. Water washing and ultrasonic treatment after small molecule intercalation can separate the kaolinite lamellae, but the kaolin nanosheets obtained by this method will have problems such as thick lamellae, large particle size, and small diameter-to-thickness ratio. The present invention can promote lamellae separation by using the auxiliary reagent H2O2 to obtain ultra-thin kaolin nanosheets with high diameter-to-thickness ratio and large specific surface area; the intercalator is pre-inserted into the interlayer of kaolin to weaken the interlayer interaction and facilitate the subsequent stripping. Subsequently, combined with the oxidation effect of the dispersant containing H2O2, H2O2 can penetrate into the interlayer of kaolin and react with the cations or functional groups between the layers to generate oxides or hydroxylation products. These reaction products occupy the interlayer space, increase the interlayer spacing, reduce the interlayer interaction force, and thus promote the stripping of the lamellae. In addition, H2O2 may also react with the hydroxyl groups on the surface of kaolin to form new functional groups, change the surface charge and polarity, enhance the repulsion between particles, facilitate dispersion and peeling, and achieve the peeling of the flakes; the addition of a small amount of silicon source can interact with H2O2 and change its oxidation ability and activity. This interaction may promote the adsorption and reaction of H2O2 on the surface of kaolin flakes, thereby enhancing the oxidation effect and accelerating the peeling process of the flakes.

[0028] Furthermore, the drying method is freeze-microwave coordinated drying, comprising the following steps: first freeze-drying for 13-16 hours at a temperature range of -40 to -20°C, microwave drying at 45-50°C when the relative humidity reaches 48-52%, adjusting the microwave temperature to 65-70°C when the relative humidity reaches 58-62%, and continuing microwave drying until the relative humidity reaches 78-82%, and finally cooling.

[0029] Description: First, freeze-drying is used to freeze and sublimate the water in the kaolin, and then microwave drying is used to further heat and dry the material, which helps to more thoroughly peel off the kaolin flakes. By controlling the temperature and humidity in the initial stage of drying, the drying rate is slowly increased, which can avoid the initial temperature being too high and help prevent the particle size of the kaolin nanosheets after freeze-drying from being too large.

[0030] At the same time, in the early stage of drying, if the humidity is too low and the solvent evaporates too quickly, the crystallization between the particles may be too close, making the sheet thicker. Therefore, by controlling the humidity and making the solvent evaporate at a moderate rate, it can help to form thinner kaolin nanosheets. Slowly increasing the drying rate can allow the kaolin nanosheets to have enough time to adjust their structure during the drying process, avoiding deformation of the sheet structure or increase in particle size due to drying too quickly.

[0031] The beneficial effects of the present invention are:

[0032] (1) The present invention utilizes the kaolin carrier effect and strong adsorption capacity to improve the adsorption and capture performance of the composite material for pollutants, solves the agglomeration problem of pure g-C3N4, and improves the photocatalytic performance of the composite material; utilizes the kaolin flaky morphology with a large specific surface area to increase the loading amount of nano g-C3N4; and the required raw materials are cheap and easy to obtain, the preparation process is simple, and the reaction conditions are mild, which has great application value in the field of wastewater treatment.

[0033] (2) The present invention effectively improves the dispersibility of kaolin particles in the solvent by adding a dispersant, preventing the particles from agglomerating and settling, which helps to transfer energy more evenly in the subsequent ultrasonic treatment, thereby improving the stripping effect and the quality of the stripping product; methanol, as an organic solvent, can interact with the inorganic components in kaolin, which helps the further penetration of the intercalating agent and the progress of the stripping process, and the high-pressure treatment can accelerate the diffusion and reaction of the intercalating agent between kaolin layers, thereby more effectively achieving intercalation and stripping. Through multiple centrifugation and high-speed spraying treatments, the specific surface area of ​​the intercalated-stripped kaolin can be further increased, so that it has more active sites and stronger adsorption capacity, which is conducive to the uniform loading and stable attachment of carbon nitride on its surface; during the multiple liquid spraying treatments, the layered structure of kaolin can be further optimized. This method can effectively reduce the particle size of kaolin and may make its flakes thinner, making the interlayer spacing more uniform and the layer plate more flat.

[0034] (3) The present invention effectively utilizes the oxidation effect of H2O2 by adding a small amount of H2O2 and a silicon source dispersant to the dispersant. H2O2 can react with the functional groups between kaolin layers to generate oxides or hydroxylation products to occupy the interlayer space, further increase the interlayer spacing, reduce the interlayer interaction force, and promote the peeling of the sheets. In addition, H2O2 may also react with the hydroxyl groups on the surface of kaolin to form new functional groups, change the surface charge and polarity, enhance the repulsion between particles, facilitate dispersion and peeling, and achieve the peeling of the sheets; a small amount of added silicon source can interact with H2O2 to change its oxidation ability and activity. This interaction may promote the adsorption and reaction of H2O2 on the surface of the kaolin sheets, thereby enhancing the oxidation effect and accelerating the peeling process of the sheets. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 XRD diagrams of kaolin, intercalation-stripping kaolin, g-C3N4 and kaolin-loaded nano-g-C3N4 composite photocatalytic materials with different loading amounts in the present invention;

[0036] Figure 2 The XRD patterns of kaolin-loaded nano-g-C3N4 composite photocatalysts at different calcination temperatures;

[0037] Figure 3 is the SEM image of kaolin in the present invention;

[0038] Figure 4 This is a SEM image of the flake intercalated-exfoliated kaolin in the present invention;

[0039] Figure 5 This is a SEM image of the kaolin-loaded nano-g-C3N4 composite photocatalytic material prepared using kaolin as a carrier in the present invention;

[0040] Figure 6 This is the XPS graph of the kaolin-loaded nano g-C3N4 composite photocatalytic material prepared using kaolin as a carrier in the present invention. DETAILED DESCRIPTION

[0041] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.

[0042] Embodiment 1: A kaolin-loaded nano-g-C3N4 composite photocatalytic material, wherein the composite photocatalytic material is a kaolin-loaded nano-g-C3N4 uniformly loaded on the surface of the kaolin, wherein the average particle size of the nano-g-C3N4 is 4 μm; the loading amount of the nano-g-C3N4 is 50% of the mass of the composite material; both the kaolin and the nano-g-C3N4 are in a flaky structure;

[0043] A method for preparing a kaolin-loaded nano g-C3N4 composite photocatalytic material, based on the above-mentioned kaolin-loaded nano g-C3N4 composite photocatalytic material, using kaolin flakes as carriers, melamine as carbon source and nitrogen source, and loading nano g-C3N4 on the surface of kaolin flakes by solid phase sintering method, comprising the following steps:

[0044] Kaolin is intercalated-stripped kaolin,

[0045] The preparation method of intercalation-stripping kaolin is as follows: 5 g of kaolin and 5 g of urea are fully mixed in a reactor to obtain a mixture, and then 50 mL of water is added, and the mixture is centrifuged at 40° C. and 7000 r / min for 36 hours, the supernatant is removed, and the lower precipitate is washed and filtered, and dried in a blast drying oven at 80° C. for 6 hours, 8 g of the dry product is taken, and then 40 mL of deionized water is added to the dry product, and ultrasonic-assisted treatment is performed at a temperature of 50° C. for 6 minutes, and drying is performed to obtain intercalation-stripping kaolin;

[0046] 2.5 g of intercalated-stripped kaolin and 1.875 g of melamine were added and mixed, and then ground in a mortar for 1 hour to obtain a mixed powder; the mixed powder was then heated and calcined at a heating rate of 2.5°C / min, and the temperature was raised to 550°C and kept for 4 hours to obtain a calcined product; finally, the calcined product was ground into 200 meshes to obtain a kaolin-loaded g-C3N4 composite photocatalytic material;

[0047] The parameters of ultrasonic-assisted treatment were: ultrasonic frequency of 35 KHz, ultrasonic power of 90 kW;

[0048] The drying method is freeze-microwave coordinated drying, which includes the following steps: first freeze-drying for 14 hours at a temperature range of -30°C, then microwave drying at 48°C when the relative humidity reaches 50%, then adjusting the microwave temperature to 68°C when the relative humidity reaches 60%, and then continuing microwave drying until the relative humidity reaches 80%, and finally cooling.

[0049] Example 2: Different from Example 1, the preparation method of intercalation-stripping kaolin is as follows: 5 g of kaolin and 5 g of urea are fully mixed in a reactor to obtain a mixture, and then 50 mL of water is added, and the mixture is centrifuged at 45°C and 6000 r / min for 30 h, the supernatant is removed, and the lower precipitate is washed and filtered, and dried in a blast drying oven at 82°C for 1 h, 8 g of the dry product is taken, and then 40 mL of deionized water is added to the dry product, and ultrasonic-assisted treatment is performed at a temperature of 55°C for 7 min, and the intercalation-stripping kaolin is obtained by drying;

[0050] 2.5 g of intercalated-exfoliated kaolin and 2.5 g of melamine were added and mixed, and then ground in a mortar for 1 hour to obtain a mixed powder; then the mixed powder was heated and calcined at a heating rate of 5.0° C. / min.

[0051] Example 3: Different from Example 1, the preparation method of intercalation-stripping kaolin is as follows: 5 g of kaolin and 5 g of urea are fully mixed in a reactor to obtain a mixture, and then 50 mL of water is added, and the mixture is centrifuged at 50° C. and 8000 r / min for 36 h, the supernatant is removed, and the lower precipitate is washed and filtered, and dried in a blast drying oven at 75° C. for 12 h, 8 g of the dry product is taken, and then 40 mL of deionized water is added to the dry product, and ultrasonic-assisted treatment is performed at a temperature of 60° C. for 8 min, and drying is performed to obtain intercalation-stripping kaolin;

[0052] 2.5 g of intercalated-exfoliated kaolin and 3.33 g of melamine were added and mixed, and then ground in a mortar for 1 hour to obtain a mixed powder; then the mixed powder was heated and calcined at a heating rate of 7.5° C. / min.

[0053] Example 4: Different from Example 2, in the preparation method of intercalation-stripping kaolin: 8 g of the dried product was taken, and then 41.6 mL of deionized water was added to the dried product, and ultrasonic-assisted treatment was performed at a temperature of 65° C. for 9 minutes, and the intercalation-stripping kaolin was obtained by drying;

[0054] During the preparation of the mixed powder: 2.5 g of intercalated-exfoliated kaolin and 5.0 g of melamine were added and mixed, and then ground in a mortar for 1 h.

[0055] Example 5: Different from Example 2, the preparation method of intercalation-stripping kaolin is as follows: 5 g of kaolin and 5 g of urea are fully mixed in a reactor to obtain a mixture, and then 50 mL of water is added, and the mixture is centrifuged at 60°C and 8000 r / min for 48 h, the supernatant is removed, and the lower precipitate is washed and filtered, and dried in a blast drying oven at 80°C for 1 h, 8 g of the dry product is taken, and then 38.4 mL of deionized water is added to the dry product, and ultrasonic-assisted treatment is performed at a temperature of 70°C for 10 min, and drying is performed to obtain intercalation-stripping kaolin;

[0056] During the preparation of the mixed powder: 2.5 g of intercalated-exfoliated kaolin and 10.0 g of melamine were added and mixed, and then ground in a mortar for 1 h.

[0057] Example 6: The difference from Example 2 is that the mixed powder is calcined at a heating rate of 5.0°C / min and kept at 450°C for 1 hour.

[0058] Example 7: The difference from Example 2 is that the mixed powder is calcined at a heating rate of 5.0°C / min and kept at 500°C for 2h.

[0059] Example 8: The difference from Example 2 is that the mixed powder is calcined at a heating rate of 5.0°C / min and kept at 600°C for 3h.

[0060] Example 9: The difference from Example 2 is that the mixed powder is calcined at a heating rate of 5.0°C / min and kept at 650°C for 5h.

[0061] Example 10: The difference from Example 2 is that the average particle size of nano g-C3N4 is 3 μm; the loading amount of nano g-C3N4 is 30% of the mass of the composite material.

[0062] Example 11: The difference from Example 2 is that the average particle size of nano g-C3N4 is 5 μm; the loading amount of nano g-C3N4 is 70% of the mass of the composite material.

[0063] Example 12: The difference from Example 2 is that the lower precipitate is washed and filtered and then subjected to high pressure treatment.

[0064] The method of high pressure treatment is:

[0065] 1) placing the lower layer of precipitation in a reactor, and introducing an inert gas with a purity of 99% until the pressure in the reactor reaches 6 MPa;

[0066] 2) adding dispersant and methanol to the reactor at a weight ratio of lower layer precipitation: dispersant: methanol of 1:0.25:0.8, continuing centrifugal treatment for 5 minutes to obtain a dispersion, and then spraying the dispersion along the nozzle of the reactor at a spray rate of 200 mL / min, while releasing an inert gas at a rate of 0.2 MPa / min to obtain a spray; wherein the pressure in the reactor is reduced by 1 MPa, the spray is collected once, and the inert gas release rate is reduced by 0.05 MPa / min; the inert gas is argon;

[0067] The dispersant comprises, by mass percentage, 0.15% of a silicon source, 15% of polyethyleneimine, 5% of acetone, 0.25% of H2O2, and the balance of sodium hexametaphosphate;

[0068] 3) Repeat step 2) twice to obtain pre-intercalation-stripping kaolin; wherein the total amount of dispersant and methanol added each time is 45% of the amount added last time, the centrifugal treatment parameters and the dispersion spraying speed are unchanged each time, and the spray obtained each time is collected and added back to the reactor.

[0069] Example 13: The difference from Example 2 is that the high pressure treatment method is:

[0070] 1) placing the lower precipitate in a reactor, and introducing an inert gas with a purity of 99.9% until the pressure in the reactor reaches 7 MPa;

[0071] 2) adding dispersant and methanol to the reactor at a weight ratio of lower layer precipitation: dispersant: methanol of 1:0.32:1, continuing centrifugal treatment for 7 minutes to obtain a dispersion, and then spraying the dispersion along the nozzle of the reactor at a spray rate of 350 mL / min, while releasing an inert gas at a rate of 0.3 MPa / min to obtain a spray; wherein the spray is collected once the pressure in the reactor decreases by 1.2 MPa, and the inert gas release rate decreases by 0.08 MPa / min; the inert gas is argon;

[0072] The dispersant comprises, by mass percentage, 0.18% of silicon source, 18% of polyethyleneimine, 6% of acetone, 0.35% of H2O2, and the balance of sodium hexametaphosphate;

[0073] 3) Repeat step 2) 3 times to obtain pre-intercalation-stripping kaolin; wherein the total amount of dispersant and methanol added each time is 55% of the amount added last time, the centrifugal treatment parameters and the dispersion spraying speed are unchanged each time, and the spray obtained each time is collected and added back to the reactor.

[0074] Example 14: The difference from Example 2 is that the high pressure treatment method is:

[0075] 1) placing the lower layer of precipitation in a reactor, and introducing an inert gas with a purity of 99.9% until the pressure in the reactor reaches 9 MPa;

[0076] 2) adding dispersant and methanol to the reactor at a weight ratio of lower layer precipitation: dispersant: methanol of 1:0.4:1.2, continuing centrifugal treatment for 10 minutes to obtain a dispersion, and then spraying the dispersion along the nozzle of the reactor at a spray rate of 500 mL / min, while releasing an inert gas at a rate of 0.5 MPa / min to obtain a spray; wherein the spray is collected once the pressure in the reactor decreases by 1.5 MPa, and the inert gas release rate decreases by 0.1 MPa / min; the inert gas is argon;

[0077] The dispersant comprises, by weight percentage, 0.2% of a silicon source, 20% of polyethyleneimine, 8% of acetone, 0.5% of H2O2, and the remainder of sodium hexametaphosphate;

[0078] 3) Repeat step 2) 3 times to obtain pre-intercalation-stripping kaolin; wherein the total amount of dispersant and methanol added each time is 65% of the amount added last time, the centrifugal treatment parameters and the dispersion spraying speed are unchanged each time, and the spray obtained each time is collected and added back to the reactor.

[0079] Example 15: The difference from Example 13 is that the parameters of ultrasonic assisted treatment are: ultrasonic frequency is 25KHz, and ultrasonic power is 80kw.

[0080] Example 16: The difference from Example 13 is that the parameters of ultrasonic assisted treatment are: ultrasonic frequency is 40KHz, and ultrasonic power is 100kw.

[0081] Example 17: The difference from Example 13 is that the drying method is freeze-microwave coordinated drying, which includes the following steps: first freeze-drying at a temperature range of -40°C for 13 hours, then microwave drying at 50°C when the relative humidity reaches 48%, and then adjusting the microwave temperature to 70°C when the relative humidity reaches 58%, and then continuing microwave drying until the relative humidity reaches 78%, and finally cooling.

[0082] Example 18: The difference from Example 13 is that the drying method is freeze-microwave coordinated drying, which includes the following steps: first freeze-drying at a temperature range of -20°C for 16 hours, then microwave drying at 45°C when the relative humidity reaches 52%, and then adjusting the microwave temperature to 65°C when the relative humidity reaches 62%, and then continuing microwave drying until the relative humidity reaches 82%, and finally cooling.

[0083] Experimental example:

[0084] XRD test

[0085] XRD analysis was performed on kaolin, intercalated-exfoliated kaolin, g-C3N4, and kaolin-loaded nano-g-C3N4 composite photocatalysts with different loading amounts and calcination temperatures. Figure 1 As shown in the figure, with the increase of g-C3N4 content, the characteristic diffraction peak at 2θ=27.6° gradually increases, and the peak shape becomes sharper and its symmetry improves, which indicates that with the increase of g-C3N4 content, the crystallinity of g-C3N4 in the composite material is improved. Figure 2 As shown in the figure, it can be found that with the gradual increase of calcination temperature, the characteristic peak of kaolin basically disappears. This phenomenon reveals that too high calcination temperature will damage the internal structure of kaolin, causing its crystal form to change. At the same time, with the increase of heat treatment temperature, the characteristic diffraction peak intensity of g-C3N4 gradually increases, and the peak shape gradually narrows. This phenomenon shows that the crystal structure of g-C3N4 becomes more complete at high temperature, and the grain size also increases.

[0086] SEM Testing

[0087] SEM analysis was performed on kaolin, intercalated-exfoliated kaolin, g-C3N4, and kaolin-loaded nano-g-C3N4 composite photocatalytic materials. Figure 3 As shown in the figure, pure kaolin is stacked in the shape of books, and the aggregates of kaolin after intercalation and stripping are significantly reduced, and the number of thin kaolin flakes increases. Figure 4 As shown in Figure 2, for pure g-C3N4 particles, due to the high-temperature polymerization process, their original lamellar structure is severely agglomerated to form larger block aggregates, which effectively reduces the specific surface area of ​​the material. Figure 5 As shown, in the kaolin-loaded nano g-C3N4 composite photocatalytic material, it can be seen that the agglomeration phenomenon of g-C3N4 can be significantly improved, and the g-C3N4 nanoparticles can be well dispersed on the kaolin sheets.

[0088] XPS Test

[0089] XPS analysis of kaolin-loaded nano-g-C3N4 composite photocatalytic materials was carried out. Figure 6 As shown, a large number of NC=N bonds, CNH bonds and Si-OC bonds were generated in the composite material, indicating that kaolin and g-C3N4 were successfully composited.

[0090] According to the following method, the performance and parameters of the final products in Examples 1 to 18 and the control examples were tested and calculated, and the results are listed in Table 1; wherein, the difference between Control Example 1 and Example 13 is that step 1) is not repeated; the difference between Control Example 2 and Example 13 is that the dispersant does not contain H2O2; the difference between Control Example 3 and Example 1 is that the relative humidity is not limited during the microwave drying process;

[0091] Determination of photocatalytic degradation performance of tetracycline wastewater: Tetracycline is widely used and used in the largest amount, and is one of the main antibiotic pollutants. Therefore, tetracycline was selected as the target pollutant to test the degradation performance of the sample on antibiotic wastewater. The smaller the absorbance of tetracycline under specific conditions, the better the photocatalytic degradation performance of the composite material. In this specific embodiment, the concentration of the tetracycline solution used is 10 mg / L, and 50 mL of tetracycline solution is taken each time and mixed with 0.02 g of the product, and ultrasonically dispersed for 5 minutes. After dark reaction for 1 hour, turn on a 500W xenon lamp for photocatalytic reaction, take samples at regular intervals, extract 3 mL of solution each time, filter out the catalyst with a 0.22 μm filter membrane, and use an ultraviolet spectrophotometer to accurately measure the absorbance C of the tetracycline solution at a wavelength of 355 nm. t The removal rate of tetracycline solution is calculated as follows: Removal rate = (C0-C t ) / C0×100%, where C0 is the absorbance of the initial tetracycline solution, C t is the absorbance value of the tetracycline solution when the reaction is complete.

[0092] Table 1 Performance of the final products in Examples 1 to 18 and Comparative Examples 1 to 3

[0093]

[0094] Conclusion: From the data in Table 1, it can be seen from the data comparison of Examples 1 to 11 and Examples 12 to 14 that Examples 12 to 14 use argon to adjust the pressure in the reactor, and then use dispersants and methanol to pre-treat kaolin, which can effectively accelerate the diffusion and reaction of the intercalation agent between kaolin layers, thereby more effectively achieving intercalation stripping. High pressure can also increase the permeability of the solvent to kaolin, which is helpful for the completion of intercalation stripping; the photocatalytic performance of the product of Control Example 1, which is only centrifuged once, is weakened, which shows that in this scheme, multiple centrifugation and high-speed ejection treatments can further improve the dispersibility of kaolin particles, reduce agglomeration, make the sheet thinner, make the interlayer spacing more uniform, and make the layer flatter. This optimized structure is more conducive to the embedding and loading of carbon nitride molecules, and improves the stability and efficiency of the loading, and Example 13 is the best scheme;

[0095] From the data comparison of Examples 12-14 and Control Example 2, it can be seen that the parameters of the high-pressure treatment within the protection scope of this scheme have little effect on the photocatalytic effect of the product, and the fact that no H2O2 is added to the dispersant in Control Example 2 also causes the photocatalytic performance of the product to weaken. This is because H2O2 can penetrate into the interlayer of kaolin and react with the cations or functional groups between the layers to generate oxides or hydroxylation products. These reaction products occupy the interlayer space, increase the interlayer spacing, reduce the interlayer interaction force, and thus promote the peeling of the sheets. In addition, H2O2 will also react with the hydroxyl groups on the surface of kaolin to form new functional groups, change the surface charge and polarity, enhance the repulsion between particles, facilitate dispersion and peeling, and achieve the peeling of the sheets. The addition of a small amount of silicon source can interact with H2O2 and change its oxidation ability and activity. This interaction may promote the adsorption and reaction of H2O2 on the surface of the kaolin sheets, thereby enhancing the oxidation effect and accelerating the peeling process of the sheets.

[0096] From the data comparison of Example 1, Example 15-Example 18 and Control Example 3, it can be seen that the parameters of the ultrasonic treatment within the protection scope of this scheme and the parameter changes during the drying process have little effect on the photocatalytic effect of the product. In Control Example 3, the lack of humidity control has an impact on the performance of the nanosheets, resulting in a weakened photocatalytic performance of the generated product. In Example 1 and Examples 17-18, by controlling the humidity, the solvent evaporation rate is moderate, which can help to form a thinner kaolin nanosheet layer. Slowly increasing the drying rate can give the kaolin nanosheet enough time to adjust its structure during the drying process, avoiding deformation of the sheet structure and increase in particle size due to excessive drying. In summary, Example 13 is the best solution.

Claims

1. A kaolin-loaded nano g-C3N4 composite photocatalytic material, characterized in that: The composite photocatalytic material is prepared by uniformly loading nano g-C3N4 on the surface of kaolin, wherein the average particle size of the nano g-C3N4 is 3-5 μm; and the loading amount of the nano g-C3N4 is 30-70% of the mass of the composite material.

2. The kaolin-loaded nano-g-C3N4 composite photocatalytic material according to claim 1, characterized in that: The kaolin and nano g-C3N4 are both in flaky structures.

3. The method for preparing a kaolin-loaded nano-g-C3N4 composite photocatalytic material according to any one of claims 1 to 2, characterized in that: Using kaolin flakes as carriers and melamine as carbon and nitrogen sources, nano g-C3N4 is loaded on the surface of kaolin flakes by solid phase sintering method, comprising the following steps: Kaolin and melamine are mixed in a mass ratio of 1:0.5-4, and then ground in a mortar for 0.5-1h to obtain a mixed powder; the mixed powder is then heated and calcined at a heating rate of 2.5-15°C / min, and the temperature is increased to 450-650°C and then kept warm for 1-5h to obtain a calcined product; finally, the calcined product is ground into 200-250 mesh to obtain a kaolin-loaded g-C3N4 composite photocatalytic material.

4. The method for preparing a kaolin-loaded nano-g-C3N4 composite photocatalytic material according to claim 3, characterized in that: The kaolin is intercalated-exfoliated kaolin, The preparation method of the intercalation-stripping kaolin is as follows: kaolin and an organic intercalation agent are fully mixed in a reaction kettle at a mass ratio of 1:1 to obtain a mixture, water is then added at a ratio of 0.15-0.25 g / mL, and the mixture is centrifuged at a speed of 6000-8000 r / min at 40-60° C. for 24-48 hours, the supernatant is removed, and the lower precipitate is washed and filtered, and the mixture is dried in a blast drying oven at 75-85° C. for 1-12 hours to obtain a dry product, and deionized water is then added to the dry product at a ratio of 1 g:4.8-5.2 mL, and the mixture is ultrasonically assisted for 6-10 minutes at a temperature of 50-70° C. to obtain the intercalation-stripping kaolin.

5. The method for preparing a kaolin-loaded nano-g-C3N4 composite photocatalytic material according to claim 4, characterized in that: The parameters of ultrasonic assisted treatment are: ultrasonic frequency is 25-40KHz, and ultrasonic power is 80-100kw.

6. The method for preparing a kaolin-loaded nano-g-C3N4 composite photocatalytic material according to claim 4, characterized in that: The lower sediment is washed and filtered and then subjected to high pressure treatment. The method of high pressure treatment is: 1) placing the lower precipitate in a reactor, and introducing an inert gas with a purity of 99-99.9% until the pressure in the reactor reaches 6-9 MPa; 2) adding dispersant and methanol to the reactor in a weight ratio of lower layer precipitation: dispersant: methanol of 1:0.25-0.4:0.8-1.2, continuing centrifugal treatment for 5-10 minutes to obtain a dispersion, and then spraying the dispersion along the nozzle of the reactor at a spray rate of 200-500 mL / min, while releasing inert gas at a rate of 0.2-0.5 MPa / min to obtain a spray; wherein the pressure in the reactor is reduced by 1-1.5 MPa, the spray is collected once, and the inert gas release rate is reduced by 0.05-0.1 MPa / min; 3) Repeat step 2) 2-3 times to obtain pre-intercalation-stripping kaolin; wherein the total amount of dispersant and methanol added each time is 45-65% of the amount added last time, the centrifugal treatment parameters and the dispersion spraying speed remain unchanged each time, and the spray obtained each time is collected and added back to the reactor.

7. The method for preparing a kaolin-loaded nano-g-C3N4 composite photocatalytic material according to claim 6, characterized in that: The organic intercalant is one of dimethyl sulfoxide, potassium acetate or urea, and the inert gas is argon or nitrogen.

8. The method for preparing a kaolin-loaded nano-g-C3N4 composite photocatalytic material according to claim 6, characterized in that: The dispersant comprises, by mass percentage, 0.15-0.2% of silicon source, 15-20% of polyethyleneimine, 5-8% of acetone, 0.25-0.5% of H2O2, and the balance of sodium hexametaphosphate.

9. The method for preparing a kaolin-loaded nano-g-C3N4 composite photocatalytic material according to claim 3, characterized in that: The drying method is freeze-microwave coordinated drying, comprising the following steps: first freeze-drying for 13-16 hours at a temperature range of -40 to -20°C, performing microwave drying at 45-50°C when the relative humidity reaches 48-52%, adjusting the microwave temperature to 65-70°C when the relative humidity reaches 58-62%, and continuing microwave drying until the relative humidity reaches 78-82%, and finally cooling.

Citation Information

Patent Citations

  • Pd-Ag loaded g-C3N4 nanosheet photocatalyst as well as preparation method and application thereof

    CN115463654A