Constant-specification universal profile steel horizontal roll collar manufacturing method

Through the combined manufacturing method of the support layer and the working layer, the problem of unstable horizontal roller ring dimensions of universal steel is solved, constant specifications and efficient use are achieved, and the roller ring modification loss and production cost are significantly reduced.

CN118893214APending Publication Date: 2024-11-05SINOSTEEL XINGTAI MACHINERY & MILL ROLL +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410784446.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing universal steel horizontal roller rings are unstable during the rolling process, resulting in frequent modifications and high roller consumption, increasing production costs and waste.

Method used

The universal steel horizontal roller ring manufacturing method consisting of a support layer and a working layer is adopted to achieve constant specification roll ring manufacturing through arc furnace adjustment components casting, forging, heat treatment, assembly, submerged arc additive manufacturing and knocking operations.

Benefits of technology

It improves the strength, red hardness and wear resistance of the rolling ring, extends the service life, reduces the rolling ring modification loss, increases the single rolling volume by 2-3 times, and reduces the roller consumption by more than 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004898189060000051
    Figure BDA0004898189060000051
  • Figure BDA0004898189060000071
    Figure BDA0004898189060000071
Patent Text Reader

Abstract

The invention discloses a method for manufacturing a constant-specification universal profile steel horizontal roll collar, which comprises a supporting layer and a working layer, and comprises the following steps of: 1, manufacturing a steel ingot; step 2, forging and forming: heating the steel ingot in a heating furnace, taking out of the furnace and forging at a forging ratio of more than or equal to 4 after the temperature is reached, and annealing after the blank is formed; 3, heat treatment is carried out, quenching and tempering are directly carried out after discharging, water is adopted as a quenching medium, and then semi-finish turning is carried out; fourthly, assembling is conducted, specifically, the horizontal roll collar obtained after semi-finish turning is put into a furnace to be preheated, heat preservation is conducted, and the horizontal roll collar is discharged out of the furnace and assembled with a shaft in an interference mode; the upper and lower joints of the assembled shaft and the horizontal roller rings are subjected to full-length welding treatment through electric welding; (5) deposition additive manufacturing is conducted, specifically, alloy powder is prepared according to the requirement for chemical components of a working layer of the universal section steel horizontal roll collar, vibration mixing is conducted, and submerged arc additive manufacturing is conducted on a supporting layer of the universal section steel horizontal roll collar; sixthly, secondary heat treatment is carried out, and overall stress relief tempering is carried out on the universal profile steel horizontal roll collar; and seventhly, machining is conducted, specifically, the universal profile steel horizontal roll collar is machined to the finished product size.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of roller ring manufacturing, and in particular relates to a method for manufacturing a universal steel horizontal roller ring with constant specifications. Background Art

[0002] A universal steel rolling mill generally consists of a billet forming unit, a universal rough rolling unit, and a universal finishing rolling unit. The universal rough rolling unit includes at least one universal rolling mill and one edge rolling mill, and performs either continuous or reciprocating rolling.

[0003] The horizontal roll of the universal rolling mill is surrounded by steel sections, especially at the corners of the roll. The deformation of the rolled material is large and the thermal shock is large, so the roll is required to have high wear resistance and thermal cracking resistance. Since the rolling force is concentrated on the narrow roll in the middle of the roll, it needs to withstand alternating bending stress, and the large roll diameter makes the roll neck bear a large torque, so the roll is required to have good strength and toughness to prevent roll neck fatigue fracture or shaft head twisting. At the same time, the roll is required to have high anti-roughening performance to prevent the surface of the rolled material from deteriorating, such as wrinkles or scratches.

[0004] According to the national standards "Hot-rolled H-shaped steel and split T-shaped steel" (GB / T11263-2017) and "Hot-rolled steel" (GB / T706-2016), steel is divided into different specifications, and different universal steel horizontal roller rings are required during the rolling process. Generally, after the universal steel horizontal roller ring is rolled twice, its size cannot meet the same specification and needs to be modified to the next specification. During the modification process, the metal of the side wall of the horizontal roller ring is turned away, which is very wasteful, resulting in high roller consumption and high cost.

[0005] Therefore, there is an urgent need to improve the manufacturing method of the universal steel horizontal roller ring to solve the current problem of large roller ring loss. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for manufacturing a horizontal roller ring of universal steel with constant specifications. The horizontal roller ring is composed of a supporting layer and a working layer. After the horizontal roller ring is worn due to rolling, the size cannot meet the same specifications. After the fatigue layer is turned, the roller ring is subjected to working layer surfacing welding, and the process is repeated to achieve a horizontal roller ring of steel with constant specifications.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is:

[0008] A method for manufacturing a universal steel horizontal roller ring with constant specifications, comprising a support layer and a working layer, and the specific steps are as follows:

[0009] Step 1: Steel ingot production: according to the requirements of the chemical composition of each part of the universal steel horizontal roller ring support layer, pig iron, scrap steel, and material heads are added to the electric arc furnace in sequence, and the composition is adjusted for pouring;

[0010] Step 2: Forging and forming: put the steel ingot into a heating furnace for heating. After reaching the temperature, take it out of the furnace for forging. The forging ratio is ≥4. After the blank is formed, annealing is performed.

[0011] Step 3: Heat treatment: After the product is taken out of the furnace, it is directly subjected to quenching and tempering treatment, and the quenching medium is water, followed by semi-finishing turning;

[0012] Step 4: Assemble, preheat the semi-finished horizontal roller ring in the furnace, keep it warm, and assemble it with the shaft by interference fit after taking it out of the furnace; the upper and lower joints of the assembled shaft and the horizontal roller ring are fully welded by electric welding;

[0013] Step 5: Additive deposition: prepare alloy powder and vibrate and mix according to the requirements of the chemical composition of the working layer of the universal steel horizontal roller ring, and perform submerged arc additive manufacturing on the supporting layer of the universal steel horizontal roller ring;

[0014] Step 6: Perform a tapping operation simultaneously behind the additively manufactured probe;

[0015] Step 7: Processing: Process the universal steel horizontal roller ring to the finished product size.

[0016] A further improvement of the technical solution of the present invention is that the chemical composition of the supporting layer and the mass percentage of each component are C 0.3-0.5%, Si 0.2-0.4%, Mn 0.6-0.8%, Cr 1.0-1.2%, Ni≤0.5%, Mo 0.15-0.30%, P≤0.03%, S≤0.03%, and the rest are Fe and inevitable impurities; the chemical composition of the working layer and the mass percentage of each component are C 0.2-0.4%, Cr 5.0-8.0%, Ni3.0-4.0%, Mo 3.0-4.0%, W2.0-3.0%, V2.0-3.0%, and the rest are Fe and inevitable impurities.

[0017] A further improvement of the technical solution of the present invention is that the hardness of the prepared universal steel horizontal roller ring is HSD65-75. After the universal steel horizontal roller is rolled for a cycle, the fatigue layer of its outer layer is turned, the metal powder according to the chemical composition of the working layer is evenly mixed, and steps five and seven are repeated.

[0018] The further improvement of the technical solution of the present invention is that the specific steps in step one are:

[0019] A1. According to the requirements of the chemical composition of each part of the universal steel horizontal roller ring support layer, pig iron, scrap steel, and material heads are added to the electric arc furnace in order to obtain primary molten steel;

[0020] A2. The molten steel is transferred to the LF ladle refining furnace to further adjust the composition to obtain finished molten steel;

[0021] A3. After the molten steel is qualified, the temperature is raised to 1650-1700℃, and vacuum is drawn. After the vacuum is over, the ladle is opened for pouring.

[0022] The further improvement of the technical solution of the present invention is that: in step 2, two upsetting and one punching and hole expansion processes are adopted, and after the blank is formed, a 600-700°C stress relief annealing process is performed.

[0023] A further improvement of the technical solution of the present invention is that in step three, the tempering temperature is 850-900°C, kept warm for 10-15 hours, taken out of the furnace and water quenched to a roller surface temperature of ≤200°C, the water is removed, and then charged into the furnace for tempering, the temperature is raised to 550-680°C, and then kept warm for 10-25 hours, and then taken out of the furnace and air-cooled to room temperature, and transferred to the processing workshop for polishing.

[0024] A further improvement of the technical solution of the present invention is that in step four, the preheating temperature is 250-350°C, the insulation time is 5-10 hours, the inner hole of the universal horizontal roller ring after semi-finishing turning is not a turned surface, but is ground, the assembly position of the shaft assembled with it is ground, and the assembly adopts interference fit, and the interference amount is controlled at 1.0-1.5‰.

[0025] The further improvement of the technical solution of the present invention is that the specific steps of step five are:

[0026] E1. Select additive materials, vibrate and mix alloy powders according to the chemical composition requirements of each part of the working layer of the universal steel horizontal roller ring, and make φ6mm welding wire;

[0027] E2. Preheat the universal steel horizontal roller ring support layer to 300-400℃ and keep it warm for 10-16h;

[0028] E3. After the insulation is completed, place the universal steel horizontal roller ring support layer on the automatic rotating device;

[0029] E4 is equipped with a submerged arc welding deposition material probe in parallel arrangement according to the shape of the universal steel horizontal roller ring;

[0030] E5. Implement submerged arc additive manufacturing, bury the homemade additive under the flux, set the computer program, control the line speed to 0.03-0.06m / s, and realize automatic additive manufacturing according to the hole size.

[0031] A further improvement of the technical solution of the present invention is that the tapping operation in step six is ​​performed by a tapping device arranged behind the submerged arc welding deposition additive probe to tap the weld overlay layer, performing a reciprocating cycle of alternating weld overlay and tapping.

[0032] A further improvement of the technical solution of the present invention is that: in the step A3, vacuuming is performed by VD, the vacuuming time is 15-20 minutes, and the vacuum pressure is ≤100 Pa.

[0033] Due to the adoption of the above technical solution, the technical progress achieved by the present invention is:

[0034] The universal steel horizontal roller ring prepared by the present invention has high strength, good red hardness, good wear resistance, good accident resistance, small wear after being used on the machine, and the single steel passing amount is extended by 2 times compared with conventional semi-steel materials.

[0035] The invention discloses a universal steel horizontal roller ring and a manufacturing method thereof, which realizes high red hardness and wear resistance of the outer layer through additive manufacturing. By optimizing the forging and heat treatment process parameters, the strength, toughness and other mechanical properties of the support layer of the universal steel horizontal roller ring are further improved. At the same time, after the rolling process of the working layer of the universal steel horizontal roller ring is consumed, the support layer can repeat the above operation for many times to achieve reuse, keep rolling the same specification of H-shaped steel, achieve constant specifications, and reduce the loss of roller ring modification.

[0036] The universal steel horizontal roller ring of the present invention adopts 3D additive manufacturing method, which is essentially different from conventional semi-steel materials. After conventional semi-steel is rolled twice, it is forced to be reshaped to the rolling of the next specification H-steel due to fatigue grinding, until it exceeds the limit of the material hardening layer and is scrapped. The above conventional material is rolled at 3000-5000t per time; while the 3D additive bimetallic composite universal steel horizontal roller ring of the present invention is rolled at 6000-10000t per time, achieving exponential growth.

[0037] After rolling a conventional horizontal roller ring, the roller will be fatigued and worn (normal fatigue + wear is 1-2mm), and the outer circle and side wall fatigue layer need to be turned. The thickness of the side wall after turning cannot meet the rolling requirements of the previous H-beam specification, and it needs to be turned to the next specification. The single-side turning amount is 25mm (much larger than the fatigue layer and wear), which causes the roller wear to increase. In addition, there is a difference in the depth and hardness of the hardened layer of the roller. After turning to the next specification, the hardness of the universal horizontal roller ring decreases, and the rolling amount will also be affected.

[0038] In the composite additive manufacturing, the input current and voltage of the conventional surfacing process are increased. After the probe is welded, an automatic tapping device is installed, which is fully coupled with the process to tap the surfacing layer. The surfacing and tapping are repeated in a reciprocating cycle until the entire continuous rolling roller is manufactured. The composite additive manufacturing is synchronized with the surfacing process, and the tapping is performed using the residual heat of the high-temperature weld bead, which increases the hardness by 2-3HSD, reduces the online wear by 10%, and reduces the finishing machining allowance.

[0039] The universal steel horizontal roller ring support layer of the present invention can be reused for more than 20 times until the shaft and the support layer are naturally scrapped due to high-cycle fatigue. Such operation, on the one hand, reduces the capital occupation of the steel plant, and on the other hand, the roller consumption can be reduced by more than 90%, generating huge economic benefits for the steel plant. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below in conjunction with embodiments:

[0041] Example 1

[0042] The components and weight percentages of the working layer and supporting layer of a universal steel horizontal roller ring are as follows:

[0043]

[0044] The rest is Fe and inevitable impurities.

[0045] A method for preparing a universal steel horizontal roller ring comprises the following steps:

[0046] A. Steel Ingot Production

[0047] A1. According to the requirements of chemical composition of each part of the universal steel horizontal roll ring, pig iron, scrap steel, and head are added to the 30t electric arc furnace in order, slag-making materials are added, oxygen is blown to make slag, decarbonize, and dephosphorize to obtain primary molten steel;

[0048] A2. Put the primary molten steel into LF refining ladle, heat the deoxidizer Al cake, add lime, silicon carbide, fluorite, make white slag, make S≤0.010%, and adjust the final product composition;

[0049] A3. After the molten steel is qualified, the temperature is raised to 1650-1700℃, and vacuum is drawn. After the vacuum is over, the ladle is opened for pouring, and the steel ingot is cast. The vacuum time is 15-20min, and the vacuum pressure is ≤100pa.

[0050] B. Forging

[0051] B1. After the steel ingot is kept warm for 48 hours, it is unpacked and transferred to a gas furnace. After being heated to temperature, it is taken out of the furnace for forging. The forging is divided into two fires. The first fire is to remove the riser and ingot tail, and perform a punching process. The second fire is to perform a roughening, punching, and hole expansion process again, and at the same time correct it to the blank shape. The actual forging ratio is 6.25;

[0052] B3. After the blank is formed, it is transferred to a resistance furnace, heated to 680°C, kept warm for 25 hours, and subjected to stress relief annealing process;

[0053] C. Heat treatment

[0054] C1. After the seamless universal steel horizontal roller ring support is taken out of the furnace, it is loaded into a 30t high-temperature resistance furnace and heated to 880℃. Then it is taken out of the furnace and placed in a water pool with stirring. After 1h20min, the water is removed and loaded into a low-temperature resistance furnace and heated to 600℃. Then it is taken out of the furnace and air-cooled to complete the quenching and tempering treatment. Then it is transferred to the processing workshop for semi-finishing turning.

[0055] D-Assembly

[0056] D1. Assemble the semi-finished horizontal roller ring (the inner hole is ground and the rest is turned) with the shaft, measure the interference between the inner hole and the shaft and control it within 1.2‰, then preheat the horizontal roller ring in the furnace to 250-350℃, keep it warm for 5-10 hours, and then take it out of the furnace and assemble it with the shaft through interference fit.

[0057] D2. After assembly, use horizontal roller rings and the upper and lower surfaces of the shaft for full welding. After welding, use coloring to detect whether there are cracks, and re-weld the cracked areas.

[0058] E. Additive Deposition

[0059] E1. Self-made additive materials, according to the requirements of the chemical composition of the working layer of the universal steel horizontal roller ring, purchase the alloy powder of each component, then put it into the rotating stirring roller, stir for 8 hours, mix it evenly, and evenly heat the folded steel strip, pass it through the wire winding machine and wire drawing machine to form a wire containing alloy powder. of welding wire.

[0060] E2. Place the semi-finished universal steel horizontal roller ring support into a low-temperature resistance furnace, heat it to 350℃, and keep it warm for 12 hours.

[0061] E3. After preheating, the universal steel horizontal roller ring support is placed on the automatic rotating device after insulation. The linear speed of the automatic rotating device is set to 0.048m / s according to the universal steel horizontal roller ring.

[0062] E4 is equipped with a deposition additive probe that can be moved in three directions, X / Z, in the axial direction of the universal steel horizontal roller ring according to the hole position. The probe is perpendicular to the universal steel horizontal roller ring support.

[0063] E5. Implement submerged arc additive manufacturing, bury the homemade additive under the flux to achieve automatic additive manufacturing, and use neutral flux to avoid brittleness and reduce crack sensitivity. Perform a tapping operation behind the additive manufacturing probe at the same time. The tapping device is set behind the submerged arc welding additive probe to tap the cladding layer, and the cladding and tapping are repeated in a reciprocating cycle.

[0064] F. Processing

[0065] F1. The universal steel horizontal roller is fine-turned in the processing workshop and the finished products are put into storage.

[0066] The universal steel horizontal roller ring prepared by the present invention has high strength, good red hardness, good wear resistance, good accident resistance, small wear after being used on the machine, and the single rolling capacity is increased from 4000t to 800t.

[0067] After fatigue wear of the surfacing working layer, steps E and F were repeated again, the hardness test was 72HSD, and the single steel rolling amount was 8200t.

[0068] Example 2

[0069] The components and weight percentages of the working layer and supporting layer of a universal steel horizontal roller ring are as follows:

[0070]

[0071] The rest is Fe and inevitable impurities.

[0072] A method for preparing a universal steel horizontal roller ring comprises the following steps:

[0073] A. Steel Ingot Production

[0074] A1. According to the requirements of chemical composition of each part of the universal steel horizontal roll ring, pig iron, scrap steel, and head are added to the 30t electric arc furnace in order, slag-making materials are added, oxygen is blown to make slag, decarbonize, and dephosphorize to obtain primary molten steel;

[0075] A2. Put the primary molten steel into LF refining ladle, heat the deoxidizer Al cake, add lime, silicon carbide, fluorite, make white slag, make S≤0.010%, and adjust the final product composition;

[0076] A3. After the molten steel is qualified, the temperature is raised to 1650-1700℃, and vacuum is drawn. After the vacuum is over, the ladle is opened for pouring, and the steel ingot is cast. The vacuum time is 20 minutes, and the vacuum pressure is ≤100pa.

[0077] B. Forging

[0078] B1. After the steel ingot is kept warm for 48 hours, it is unpacked and transferred to a gas furnace. After being heated to temperature, it is taken out of the furnace for forging. The forging is divided into two fires. The first fire is to remove the riser and ingot tail, and perform a punching process. The second fire is to perform a roughening, punching, and hole expansion process again, and at the same time correct it to the blank shape. The actual forging ratio is 6.25;

[0079] B3. After the blank is formed, it is transferred to a resistance furnace, heated to 680°C, kept warm for 25 hours, and subjected to stress relief annealing process;

[0080] C. Heat treatment

[0081] C1. After the seamless universal steel horizontal roller ring support is taken out of the furnace, it is loaded into a 30t high-temperature resistance furnace and heated to 880℃. Then it is taken out of the furnace and placed in a water pool with stirring. After 1h20min, the water is removed and loaded into a low-temperature resistance furnace and heated to 600℃. Then it is taken out of the furnace and air-cooled to complete the quenching and tempering treatment. Then it is transferred to the processing workshop for semi-finishing turning.

[0082] D-Assembly

[0083] D1. Assemble the semi-finished horizontal roller ring (the inner hole is ground and the rest is turned) with the shaft, measure the interference between the inner hole and the shaft and control it within 1.4‰, then preheat the horizontal roller ring in the furnace to 300℃, keep it warm for 8 hours, and then take it out of the furnace and assemble it with the shaft through interference fit.

[0084] D2. After assembly, use horizontal roller rings and the upper and lower surfaces of the shaft for full welding. After welding, use coloring to detect whether there are cracks, and re-weld the cracked areas.

[0085] E. Additive Deposition

[0086] E1. Self-made additive materials, according to the requirements of the chemical composition of the working layer of the universal steel horizontal roller ring, purchase the alloy powder of each component, then put it into the rotating stirring roller, stir for 8 hours, mix it evenly, and evenly heat the folded steel strip, pass it through the wire winding machine and wire drawing machine to form a wire containing alloy powder. of welding wire.

[0087] E2. Place the semi-finished universal steel horizontal roller ring support into a low-temperature resistance furnace, heat it to 350℃, and keep it warm for 12 hours.

[0088] E3. After preheating, the universal steel horizontal roller ring support is placed on the automatic rotating device after insulation. The linear speed of the automatic rotating device is set to 0.048m / s according to the universal steel horizontal roller ring.

[0089] E4 is equipped with a deposition additive probe that can be moved in three directions, X / Z, in the axial direction of the universal steel horizontal roller ring according to the hole position. The probe is perpendicular to the universal steel horizontal roller ring support.

[0090] E5. Implement submerged arc additive manufacturing, bury the homemade additive under the flux to achieve automatic additive manufacturing, and use neutral flux to avoid brittleness and reduce crack sensitivity. Perform a tapping operation behind the additive manufacturing probe at the same time. The tapping device is set behind the submerged arc welding additive probe to tap the cladding layer, and the cladding and tapping are repeated in a reciprocating cycle.

[0091] F. Processing

[0092] F1. The universal steel horizontal roller is fine-turned in the processing workshop and the finished products are put into storage.

[0093] The universal steel horizontal roller ring prepared by the present invention has high strength, good red hardness, good wear resistance, good accident resistance, small wear after being used on the machine, and the single rolling capacity is increased from 4000t to 800t.

[0094] After fatigue wear of the surfacing working layer, steps E and F were repeated again, the hardness test was 72HSD, and the single steel rolling amount was 8200t.

Claims

1. A method for manufacturing a universal steel horizontal roller ring with constant specifications. Features: Including the support layer and the working layer, the specific steps are as follows: Step 1: Steel ingot production: according to the requirements of the chemical composition of each part of the universal steel horizontal roller ring support layer, pig iron, scrap steel, and material heads are added to the electric arc furnace in sequence, and the composition is adjusted for pouring; Step 2: Forging and forming: put the steel ingot into a heating furnace for heating. After reaching the temperature, take it out of the furnace for forging. The forging ratio is ≥4. After the blank is formed, annealing is performed. Step 3: Heat treatment: After the product is taken out of the furnace, it is directly subjected to quenching and tempering treatment, and the quenching medium is water, followed by semi-finishing turning; Step 4: Assemble, preheat the semi-finished horizontal roller ring in the furnace, keep it warm, and assemble it with the shaft by interference fit after taking it out of the furnace; the upper and lower joints of the assembled shaft and the horizontal roller ring are fully welded by electric welding; Step 5: Additive deposition: prepare alloy powder and vibrate and mix according to the requirements of the chemical composition of the working layer of the universal steel horizontal roller ring, and perform submerged arc additive manufacturing on the supporting layer of the universal steel horizontal roller ring; Step 6: Perform a tapping operation simultaneously behind the additively manufactured probe; Step seven: Processing: Process the universal steel horizontal roller ring to the finished product size.

2. A method for manufacturing a universal steel horizontal roller ring with constant specifications according to claim 1, Features: The chemical composition of the supporting layer and the mass percentage of each component are C 0.3-0.5%, Si 0.2-0.4%, Mn 0.6-0.8%, Cr 1.0-1.2%, Ni≤0.5%, Mo 0.15-0.30%, P≤0.03%, S≤0.03%, and the rest are Fe and inevitable impurities; the chemical composition of the working layer and the mass percentage of each component are C 0.2-0.4%, Cr 5.0-8.0%, Ni3.0-4.0%, Mo 3.0-4.0%, W2.0-3.0%, V2.0-3.0%, and the rest are Fe and inevitable impurities.

3. A method for manufacturing a universal steel horizontal roller ring with constant specifications according to claim 1, Features: The hardness of the prepared universal steel horizontal roller ring is HSD65-75. After the universal steel horizontal roller is rolled for one cycle, the fatigue layer of the outer layer is turned, and the metal powder according to the chemical composition of the working layer is evenly mixed, and steps five and seven are repeated.

4. A method for manufacturing a universal steel horizontal roller ring with constant specifications according to claim 1, Features: The specific steps in step one are: A1. According to the requirements of the chemical composition of each part of the universal steel horizontal roller ring support layer, pig iron, scrap steel, and material heads are added to the electric arc furnace in order to obtain primary molten steel; A2. The primary molten steel is transferred to the LF ladle refining furnace to further adjust the composition to obtain finished molten steel; A3. After the molten steel is qualified, the temperature is raised to 1650-1700℃, and vacuum is drawn. After the vacuum is over, the ladle is opened for pouring.

5. A method for manufacturing a universal steel horizontal roller ring with constant specifications according to claim 1, Features: In step 2, two piercing and one punching and hole expansion processes are adopted. After the blank is formed, a 600-700°C stress relief annealing process is performed.

6. A method for manufacturing a universal steel horizontal roller ring with constant specifications according to claim 1, Features: In step three, the tempering temperature is 850-900℃, and it is kept warm for 10-15 hours. After being taken out of the furnace and quenched in water until the surface temperature of the roll is ≤200℃, the water is removed, and then the furnace is charged for tempering, the temperature is raised to 550-680℃, and then kept warm for 10-25h, and then taken out of the furnace and air-cooled to room temperature, and transferred to the processing workshop for polishing.

7. A method for manufacturing a universal steel horizontal roller ring with constant specifications according to claim 1, Features: In step 4, the preheating temperature is 250-350°C and the insulation time is 5-10 hours. The inner hole of the universal horizontal roller ring after semi-finishing turning is not a turned surface, but a ground surface. The assembly position of the shaft assembled with it is ground. The assembly adopts interference fit, and the interference amount is controlled at 1.0-1.5‰.

8. A method for manufacturing a universal steel horizontal roller ring with constant specifications according to claim 1, Features: The specific steps of step five are: E1. Select additive materials, prepare alloy powder and vibrate and mix according to the requirements of the chemical composition of the working layer of the universal steel horizontal roller ring to make welding wire; E2. Preheat the universal steel horizontal roller ring support layer to 300-400℃ and keep it warm for 10-16h; E3. After the insulation is completed, place the universal steel horizontal roller ring support layer on the automatic rotating device; E4 is equipped with a submerged arc welding deposition material probe in parallel arrangement according to the shape of the universal steel horizontal roller ring; E5. Implement submerged arc additive manufacturing, bury the homemade additive under the flux, set the computer program, control the line speed to 0.03-0.06m / s, and realize automatic additive manufacturing according to the hole size.

9. A method for manufacturing a universal steel horizontal roller ring with constant specifications according to claim 8, Features: The tapping operation in step six is ​​performed by a tapping device arranged behind the submerged arc welding deposition additive probe to tap the weld overlay layer, performing a reciprocating cycle of alternating weld overlay and tapping.