Method for brazing Y2O3-MgO composite ceramic and metal by adopting TiZrNiCu active brazing filler metal

Through TiZrNiCu active brazing technology, the problems of low connection strength and poor airtightness between Y2O3-MgO composite ceramics and metals are solved, and reliable connections are achieved under high temperature and high pressure, improving the performance of infrared windows.

CN118893265APending Publication Date: 2024-11-05HARBIN INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411099840.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-11
Filing Date
2024-08-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The connection strength between Y2O3-MgO composite ceramics and metals is low and the airtightness is poor. The existing glued joints and stud connections have insufficient thermal shock resistance and stress concentration problems, which affects the reliability of infrared windows.

Method used

The soldering connection is carried out by TiZrNiCu active brazing, and the welding surface is smooth through ultrasonic cleaning and sandpaper grinding. The soldering is performed by using a vacuum brazing furnace. The thermal expansion coefficient matching is controlled to reduce stress concentration, and the ceramics and metals are promoted through Zr and Cu elements. The reaction forms a reliable linker.

Benefits of technology

It improves the connection strength and airtightness of Y2O3-MgO composite ceramics and metals, reduces the crack risk of welded joints, meets the requirements of high-temperature service and thermal shock, and improves the reliability of infrared windows.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893265A_ABST
    Figure CN118893265A_ABST
Patent Text Reader

Abstract

The invention discloses a method for brazing Y2O3-MgO multiphase ceramic and metal by adopting TiZrNiCu active brazing filler metal, and relates to a method for brazing Y2O3-MgO multiphase ceramic and metal. In order to solve the problems that the brazing connection strength of Y2O3-MgO composite ceramic and metal is low, and the air tightness of a connection joint is improved. The method comprises the steps that the Y2O3-MgO composite ceramic, the TiZrNiCu active brazing filler metal and metal to be welded are subjected to pre-welding treatment, the TiZrNiCu active brazing filler metal is placed between the Y2O3-MgO composite ceramic and the metal to be welded to obtain an assembly part, and the assembly part is placed in a vacuum brazing furnace for brazing. According to the method, the Y2O3-MgO multiphase ceramic and the metal are connected through a brazing method, an obtained welding joint is compact in structure and free of obvious defects such as air holes and cracks, and the airtightness requirement for connection of the Y2O3-MgO multiphase ceramic and the metal is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for brazing Y2O3-MgO composite ceramics and metal. Background Art

[0002] Since the mid-1960s, when the world's first forward-looking infrared imaging system was introduced in the United States, infrared window materials can greatly improve the combat capabilities of aircraft, submarines and other equipment, especially in smoke, night and other environments. In addition, platforms equipped with infrared optoelectronic systems are usually required to serve in harsh environments such as high temperature, high pressure, thermal shock, wind and sand, rain and snow. High-performance infrared windows need to isolate the optoelectronic system from the external environment to protect the infrared optoelectronic system. Therefore, infrared window materials need to have good infrared transparency and good mechanical properties. Y2O3-MgO nanocomposite ceramics have excellent mid-wave infrared transmittance, extremely low high-temperature emissivity, excellent high-temperature mechanical properties and thermal shock resistance, making it an excellent candidate material for infrared windows of future high-speed aircraft.

[0003] At present, the connection between Y2O3-MgO composite ceramics and metals is mostly made by adhesive bonding and stud bonding. When using adhesive bonding technology, the process is simple and easy to operate, but there are problems such as low strength, poor thermal shock resistance, and easy aging after long-term storage, which reduces the reliability of the joint. When using stud connection, it is necessary to drill threaded holes in the ceramic, which reduces the air tightness of the joint and causes stress concentration problems. Summary of the invention

[0004] In order to solve the problem of low brazing connection strength between Y2O3-MgO composite ceramics and metals and improve the air tightness of the connection joint, the present invention provides a method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal.

[0005] The method for brazing Y2O3-MgO composite ceramic and metal using TiZrNiCu active brazing filler metal is carried out according to the following steps:

[0006] 1. Pre-welding treatment of Y2O3-MgO composite ceramics and metal to be welded:

[0007] The Y2O3-MgO composite ceramic and the metal to be welded are cut into predetermined sizes respectively, and the welded surface of the Y2O3-MgO composite ceramic and the welded surface of the metal to be welded are sanded and ultrasonically cleaned respectively;

[0008] The ultrasonic cleaning process is as follows: the polished Y2O3-MgO composite ceramic and the metal to be welded are placed in a cleaning agent, and ultrasonically cleaned for 5-10 minutes in a 100kHz ultrasonic cleaning machine, and a new cleaning agent is replaced and the cleaning is repeated 2-3 times, and the cleaned Y2O3-MgO composite ceramic is placed in acetone for liquid sealing for standby use;

[0009] The metal to be welded is TC4 titanium alloy;

[0010] The cleaning agent is anhydrous ethanol or acetone;

[0011] The sandpaper grinding process uses 400-3000 mesh sandpaper for step-by-step grinding; the sandpaper grinding step can remove surface impurities and ensure that the surface to be welded is smooth and flat;

[0012] 2. Pretreatment of TiZrNiCu active brazing filler metal:

[0013] Take powdered TiZrNiCu active solder or foil-shaped TiZrNiCu active solder; cut the foil-shaped TiZrNiCu active solder to a predetermined size to ensure that the TiZrNiCu active solder is larger than the to-be-welded surface of the Y2O3-MgO composite ceramic, and grind and clean both surfaces of the foil-shaped TiZrNiCu active solder;

[0014] The TiZrNiCu active solder composition comprises 15-26wt% Cu, 19-27wt% Zr, 7-13wt% Ni and the remainder Ti;

[0015] The thickness of the foil-shaped TiZrNiCu active solder is 3 to 10 μm;

[0016] The grinding process is performed using 1500-5000 mesh sandpaper;

[0017] The cleaning process is as follows: putting the polished TiZrNiCu active solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5-10 minutes, replacing the cleaning agent with a new one, and repeating the cleaning 2-3 times;

[0018] The cleaning agent is anhydrous ethanol or acetone;

[0019] 3. Assembly of parts to be welded:

[0020] The TiZrNiCu active solder is placed between the Y2O3-MgO composite ceramic and the metal to be welded to obtain an assembly;

[0021] 4. Vacuum brazing connection: put the assembly into the vacuum brazing furnace for brazing;

[0022] The vacuum degree of the vacuum brazing furnace during the brazing process is 5×10 -3 Pa;

[0023] The brazing process is as follows: firstly, the temperature is increased to 600°C at a rate of 5-15°C / min, then, the temperature is increased to 850-1000°C at a rate of 5-15°C / min and kept at this temperature for 10-30 minutes, then, the temperature is cooled to below 150°C at a rate of ≤5°C / min, the sample is taken out, and the brazing is completed.

[0024] The principles and beneficial effects of the present invention are:

[0025] The thermal expansion coefficient of the TiZrNiCu solder in the present invention is 10 to 15×10 -6 / K, the thermal expansion coefficient of TC4 titanium alloy is 11~12×10 -6 / K, the thermal expansion coefficient of Y2O3-MgO composite ceramics is 10~11×10 -6 / K, the difference in thermal expansion coefficients of the three is small, which will reduce the stress concentration problem caused by thermal expansion coefficient mismatch, the residual stress during welding is small, the joint is not easy to crack, which is conducive to improving welding quality. The melting point of TiZrNiCu solder can reach above 870℃, which also makes the welded joint meet the requirements of high temperature service and high temperature thermal shock.

[0026] The active solder TiZrNiCu in the present invention can react with the Y2O3-MgO composite ceramic and the metal to promote mutual connection and obtain a reliable joint. The Zr element in the TiZrNiCu active solder diffuses into the ceramic matrix to promote the connection between the ceramic and the metal to be welded, and Zr and Cu form a reaction layer on the ceramic surface to ensure the reliability of the brazed joint; thus, the connection reliability of the infrared window of the high-speed aircraft is improved, and the application foundation of the high-performance Y2O3-MgO composite ceramic is laid.

[0027] The present invention adopts a brazing method to connect Y2O3-MgO composite ceramics and metals, and the obtained welded joint has a dense structure without obvious defects such as pores and cracks, meeting the requirements of air tightness and connection strength of the connection between Y2O3-MgO composite ceramics and metals. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a microstructure picture of the Y2O3-MgO composite ceramic brazed joint obtained in Example 1;

[0029] Figure 2 This is a microstructure picture of the Y2O3-MgO composite ceramic brazed joint obtained in Example 2;

[0030] Figure 3This is a microstructure picture of the Y2O3-MgO composite ceramic brazed joint obtained in Example 3;

[0031] Figure 4 This is a microstructure picture of the Y2O3-MgO composite ceramic brazed joint obtained in Example 4. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.

[0033] Specific implementation method 1: In this implementation method, the method of brazing Y2O3-MgO composite ceramic and metal using TiZrNiCu active brazing filler metal is carried out according to the following steps:

[0034] 1. Pre-welding treatment of Y2O3-MgO composite ceramics and metal to be welded:

[0035] The Y2O3-MgO composite ceramic and the metal to be welded are cut into predetermined sizes respectively, and the welded surface of the Y2O3-MgO composite ceramic and the welded surface of the metal to be welded are sanded and ultrasonically cleaned respectively;

[0036] The ultrasonic cleaning process is as follows: the polished Y2O3-MgO composite ceramic and the metal to be welded are placed in a cleaning agent, and ultrasonically cleaned for 5-10 minutes in a 100kHz ultrasonic cleaning machine, and a new cleaning agent is replaced and the cleaning is repeated 2-3 times, and the cleaned Y2O3-MgO composite ceramic is placed in acetone for liquid sealing for standby use;

[0037] The metal to be welded is TC4 titanium alloy;

[0038] The cleaning agent is anhydrous ethanol or acetone;

[0039] The sandpaper grinding process uses 400-3000 mesh sandpaper for step-by-step grinding; the sandpaper grinding step can remove surface impurities and ensure that the surface to be welded is smooth and flat;

[0040] 2. Pretreatment of TiZrNiCu active brazing filler metal:

[0041] Take powdered TiZrNiCu active solder or foil-shaped TiZrNiCu active solder; cut the foil-shaped TiZrNiCu active solder to a predetermined size to ensure that the TiZrNiCu active solder is larger than the to-be-welded surface of the Y2O3-MgO composite ceramic, and grind and clean both surfaces of the foil-shaped TiZrNiCu active solder;

[0042] The TiZrNiCu active solder composition comprises 15-26wt% Cu, 19-27wt% Zr, 7-13wt% Ni and the remainder Ti;

[0043] The thickness of the foil-shaped TiZrNiCu active solder is 3 to 10 μm;

[0044] The grinding process is performed using 1500-5000 mesh sandpaper;

[0045] The cleaning process is as follows: putting the polished TiZrNiCu active solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5-10 minutes, replacing the cleaning agent with a new one, and repeating the cleaning 2-3 times;

[0046] The cleaning agent is anhydrous ethanol or acetone;

[0047] 3. Assembly of parts to be welded:

[0048] The TiZrNiCu active solder is placed between the Y2O3-MgO composite ceramic and the metal to be welded to obtain an assembly;

[0049] 4. Vacuum brazing connection: put the assembly into the vacuum brazing furnace for brazing;

[0050] The vacuum degree of the vacuum brazing furnace during the brazing process is 5×10 -3 Pa;

[0051] The brazing process is as follows: firstly, the temperature is increased to 600°C at a rate of 5-15°C / min, then, the temperature is increased to 850-1000°C at a rate of 5-15°C / min and kept at this temperature for 10-30 minutes, then, the temperature is cooled to below 150°C at a rate of ≤5°C / min, the sample is taken out, and the brazing is completed.

[0052] This embodiment has the following beneficial effects:

[0053] In this embodiment, the thermal expansion coefficient of the TiZrNiCu solder is 10 to 15×10 -6 / K, the thermal expansion coefficient of TC4 titanium alloy is 11~12×10 -6 / K, the thermal expansion coefficient of Y2O3-MgO composite ceramics is 10~11×10 -6 / K, the difference in thermal expansion coefficients of the three is small, which will reduce the stress concentration problem caused by thermal expansion coefficient mismatch, the residual stress during welding is small, the joint is not easy to crack, which is conducive to improving welding quality. The melting point of TiZrNiCu solder can reach above 870℃, which also makes the welded joint meet the requirements of high temperature service and high temperature thermal shock.

[0054] In this embodiment, the active solder TiZrNiCu can react with the Y2O3-MgO composite ceramic and the metal to promote mutual connection and obtain a reliable joint. Among them, the Zr element in the TiZrNiCu active solder diffuses into the ceramic matrix, promoting the connection between the ceramic and the metal to be welded, and Zr and Cu form a reaction layer on the ceramic surface, which ensures the reliability of the brazed joint; thus, the connection reliability of the infrared window of the high-speed aircraft is improved, and the application foundation of high-performance Y2O3-MgO composite ceramics is laid.

[0055] This embodiment adopts the brazing method to connect Y2O3-MgO composite ceramics and metals, and the obtained welded joint has a dense structure without obvious defects such as pores and cracks, which meets the requirements of air tightness and connection strength of the connection between Y2O3-MgO composite ceramics and metals.

[0056] Specific implementation method 2: The difference between this implementation method and specific implementation method 1 is that: the ultrasonic cleaning process in step 1 is: put the polished Y2O3-MgO composite ceramics and the metal to be welded into the cleaning agent, ultrasonically clean them in a 100kHz ultrasonic cleaning machine for 10 minutes, replace the new cleaning agent and repeat the cleaning twice, and put the cleaned Y2O3-MgO composite ceramics into acetone for liquid sealing for standby use.

[0057] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that the cleaning process described in step two is: putting the polished foil-shaped TiZrNiCu active solder into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 10 minutes, replacing the cleaning agent with a new one, and repeating the cleaning twice.

[0058] Specific implementation method 4: This implementation method is different from any one of specific implementation methods 1 to 3 in that: the TiZrNiCu active solder composition described in step 2 contains 22wt% Cu, 12wt% Zr, 13wt% Ni, and the rest is Ti.

[0059] Specific implementation mode 5: This implementation mode is different from any one of specific implementation modes 1 to 4 in that: the thickness of the foil-shaped TiZrNiCu active solder in step 2 is 6 μm.

[0060] Specific implementation method six: This implementation method is different from any of specific implementation methods one to five in that: in step one, the Y2O3-MgO composite ceramic is cut into 4mm×4mm, and the metal to be welded is cut into 6mm×10mm, and the welding surface of the Y2O3-MgO composite ceramic and the welding surface of the metal to be welded are polished and ultrasonically cleaned step by step using 400, 600, 800, 1200, 1500, and 3000 grit sandpapers respectively.

[0061] Specific embodiment seven: The difference between this embodiment and any one of specific embodiments one to six is ​​that the brazing process described in step four is: first, heat the temperature to 600°C at a rate of 5 to 15°C / min, then heat to 910°C at a heating rate of 5 to 15°C / min and keep warm for 10 to 30 minutes, then cool to below 150°C at a cooling rate of ≤5°C / min, take out the sample, and complete the brazing.

[0062] Specific embodiment eight: The difference between this embodiment and any one of specific embodiments one to seven is that the brazing process described in step four is: first, heat the temperature to 600°C at a rate of 5 to 15°C / min, then heat to 970°C at a heating rate of 5 to 15°C / min and keep warm for 10 to 30 minutes, then cool to below 150°C at a cooling rate of ≤5°C / min, take out the sample, and complete the brazing.

[0063] Specific embodiment nine: The difference between this embodiment and any one of specific embodiments one to eight is that the brazing process described in step four is: first, heat the temperature to 600°C at a rate of 5 to 15°C / min, then heat to 930°C at a heating rate of 5 to 15°C / min and keep warm for 10 to 30 minutes, then cool to below 150°C at a cooling rate of ≤5°C / min, take out the sample, and complete the brazing.

[0064] Specific embodiment ten: The difference between this embodiment and any one of specific embodiments one to nine is that the brazing process described in step four is: first, heat the temperature to 600°C at a rate of 5 to 15°C / min, then heat to 950°C at a heating rate of 5 to 15°C / min and keep warm for 10 to 30 minutes, then cool to below 150°C at a cooling rate of ≤5°C / min, take out the sample, and complete the brazing.

[0065] Embodiment 1:

[0066] The method for brazing Y2O3-MgO composite ceramic and metal using TiZrNiCu active brazing filler metal in this embodiment is carried out according to the following steps:

[0067] 1. Pre-welding treatment of Y2O3-MgO composite ceramics and metal to be welded:

[0068] The Y2O3-MgO composite ceramic was cut into 4 mm×4 mm, and the metal to be welded was cut into 6 mm×10 mm. The surface to be welded of the Y2O3-MgO composite ceramic and the surface to be welded of the metal to be welded were polished and ultrasonically cleaned in sequence using 400, 600, 800, 1200, 1500, and 3000 grit sandpapers.

[0069] The ultrasonic cleaning process is as follows: the polished Y2O3-MgO composite ceramic and the metal to be welded are placed in a cleaning agent, and ultrasonically cleaned for 10 minutes in a 100kHz ultrasonic cleaning machine, and a new cleaning agent is replaced and the cleaning is repeated twice, and the cleaned Y2O3-MgO composite ceramic is placed in acetone for liquid sealing for standby use;

[0070] The metal to be welded is TC4 titanium alloy;

[0071] The cleaning agent is anhydrous ethanol;

[0072] 2. Pre-treatment of TiZrNiCu active brazing filler metal:

[0073] Take a foil-shaped TiZrNiCu active solder; cut the foil-shaped TiZrNiCu active solder to 5 mm×5 mm, ensure that the TiZrNiCu active solder is larger than the to-be-welded surface of the Y2O3-MgO composite ceramic, and grind and clean both surfaces of the foil-shaped TiZrNiCu active solder;

[0074] The TiZrNiCu active solder composition comprises 22wt% Cu, 12wt% Zr, 13wt% Ni and the remainder Ti;

[0075] The thickness of the foil-shaped TiZrNiCu active solder is 6 μm;

[0076] The grinding process uses 1500 mesh and 3000 mesh sandpaper for grinding in sequence;

[0077] The cleaning process is as follows: putting the polished TiZrNiCu active solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 10 minutes, replacing the cleaning agent with a new one, and repeating the cleaning twice;

[0078] The cleaning agent is anhydrous ethanol;

[0079] 3. Assembly of parts to be welded:

[0080] The TiZrNiCu active solder is placed between the Y2O3-MgO composite ceramic and the metal to be welded to obtain an assembly;

[0081] 4. Vacuum brazing connection: put the assembly into the vacuum brazing furnace for brazing;

[0082] The vacuum degree of the vacuum brazing furnace during the brazing process is 5×10 -3 Pa;

[0083] The brazing process is as follows: first, heating to 600°C at a rate of 15°C / min, then heating to 910°C at a rate of 10°C / min and keeping the temperature for 10 minutes, then cooling to 150°C at a rate of 5°C / min, taking out the sample, and completing the brazing.

[0084] Figure 1 The microstructure of the Y2O3-MgO composite ceramic brazed joint obtained in Example 1 is shown in FIG. Figure 1 It can be seen that the welded joint is intact, without obvious defects such as pores and cracks. The shear test was carried out using an electronic universal testing machine with a loading speed of 0.5 mm / min. The room temperature shear strength of the obtained connection joint was measured to reach 20 MPa.

[0085] Embodiment 2:

[0086] The method for brazing Y2O3-MgO composite ceramic and metal using TiZrNiCu active brazing filler metal in this embodiment is carried out according to the following steps:

[0087] 1. Pre-welding treatment of Y2O3-MgO composite ceramics and metal to be welded:

[0088] The Y2O3-MgO composite ceramic was cut into 4 mm×4 mm, and the metal to be welded was cut into 6 mm×10 mm. The surface to be welded of the Y2O3-MgO composite ceramic and the surface to be welded of the metal to be welded were polished and ultrasonically cleaned in sequence using 400, 600, 800, 1200, 1500, and 3000 grit sandpapers.

[0089] The ultrasonic cleaning process is as follows: the polished Y2O3-MgO composite ceramic and the metal to be welded are placed in a cleaning agent, and ultrasonically cleaned for 10 minutes in a 100kHz ultrasonic cleaning machine, and a new cleaning agent is replaced and the cleaning is repeated twice, and the cleaned Y2O3-MgO composite ceramic is placed in acetone for liquid sealing for standby use;

[0090] The metal to be welded is TC4 titanium alloy;

[0091] The cleaning agent is anhydrous ethanol;

[0092] 2. Pre-treatment of TiZrNiCu active brazing filler metal:

[0093] Take a foil-shaped TiZrNiCu active solder; cut the foil-shaped TiZrNiCu active solder to 5 mm×5 mm, ensure that the TiZrNiCu active solder is larger than the to-be-welded surface of the Y2O3-MgO composite ceramic, and grind and clean both surfaces of the foil-shaped TiZrNiCu active solder;

[0094] The TiZrNiCu active solder composition comprises 22wt% Cu, 12wt% Zr, 13wt% Ni and the remainder Ti;

[0095] The thickness of the foil-shaped TiZrNiCu active solder is 6 μm;

[0096] The grinding process uses 1500 mesh and 3000 mesh sandpaper for grinding in sequence;

[0097] The cleaning process is as follows: putting the polished TiZrNiCu active solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 10 minutes, replacing the cleaning agent with a new one, and repeating the cleaning twice;

[0098] The cleaning agent is anhydrous ethanol;

[0099] 3. Assembly of parts to be welded:

[0100] The TiZrNiCu active solder is placed between the Y2O3-MgO composite ceramic and the metal to be welded to obtain an assembly;

[0101] 4. Vacuum brazing connection: put the assembly into the vacuum brazing furnace for brazing;

[0102] The vacuum degree of the vacuum brazing furnace during the brazing process is 5×10 -3 Pa;

[0103] The brazing process is as follows: first, heating to 600°C at a rate of 15°C / min, then heating to 930°C at a rate of 10°C / min and keeping the temperature for 10 minutes, then cooling to 150°C at a rate of 5°C / min, taking out the sample, and completing the brazing.

[0104] Figure 2 The microstructure of the Y2O3-MgO composite ceramic brazed joint obtained in Example 2; Figure 2 It can be seen that the welded joint is intact, without obvious defects such as pores and cracks. The shear test was carried out using an electronic universal testing machine with a loading speed of 0.5 mm / min. The room temperature shear strength of the obtained connection joint was measured to reach 24 MPa.

[0105] Embodiment 3:

[0106] The method for brazing Y2O3-MgO composite ceramic and metal using TiZrNiCu active brazing filler metal in this embodiment is carried out according to the following steps:

[0107] 1. Pre-welding treatment of Y2O3-MgO composite ceramics and metal to be welded:

[0108] The Y2O3-MgO composite ceramic was cut into 4 mm×4 mm, and the metal to be welded was cut into 6 mm×10 mm. The surface to be welded of the Y2O3-MgO composite ceramic and the surface to be welded of the metal to be welded were polished and ultrasonically cleaned in sequence using 400, 600, 800, 1200, 1500, and 3000 grit sandpapers.

[0109] The ultrasonic cleaning process is as follows: the polished Y2O3-MgO composite ceramic and the metal to be welded are placed in a cleaning agent, and ultrasonically cleaned for 10 minutes in a 100kHz ultrasonic cleaning machine, and a new cleaning agent is replaced and the cleaning is repeated twice, and the cleaned Y2O3-MgO composite ceramic is placed in acetone for liquid sealing for standby use;

[0110] The metal to be welded is TC4 titanium alloy;

[0111] The cleaning agent is anhydrous ethanol;

[0112] 2. Pretreatment of TiZrNiCu active brazing filler metal:

[0113] Take a foil-shaped TiZrNiCu active solder; cut the foil-shaped TiZrNiCu active solder to 5 mm×5 mm, ensure that the TiZrNiCu active solder is larger than the to-be-welded surface of the Y2O3-MgO composite ceramic, and grind and clean both surfaces of the foil-shaped TiZrNiCu active solder;

[0114] The TiZrNiCu active solder composition comprises 22wt% Cu, 12wt% Zr, 13wt% Ni and the remainder Ti;

[0115] The thickness of the foil-shaped TiZrNiCu active solder is 6 μm;

[0116] The grinding process uses 1500 mesh and 3000 mesh sandpaper for grinding in sequence;

[0117] The cleaning process is as follows: putting the polished TiZrNiCu active solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 10 minutes, replacing the cleaning agent with a new one, and repeating the cleaning twice;

[0118] The cleaning agent is anhydrous ethanol;

[0119] 3. Assembly of parts to be welded:

[0120] The TiZrNiCu active solder is placed between the Y2O3-MgO composite ceramic and the metal to be welded to obtain an assembly;

[0121] 4. Vacuum brazing connection: put the assembly into the vacuum brazing furnace for brazing;

[0122] The vacuum degree of the vacuum brazing furnace during the brazing process is 5×10 -3 Pa;

[0123] The brazing process is as follows: first, heating to 600°C at a rate of 15°C / min, then heating to 950°C at a rate of 10°C / min and keeping the temperature for 10 minutes, then cooling to 150°C at a rate of 5°C / min, taking out the sample, and completing the brazing.

[0124] Figure 3 The microstructure of the Y2O3-MgO composite ceramic brazed joint obtained in Example 3; Figure 3 It can be seen that the welded joint is intact, without obvious defects such as pores and cracks. The shear test was carried out using an electronic universal testing machine with a loading speed of 0.5 mm / min. The room temperature shear strength of the obtained connection joint was measured to reach 32 MPa.

[0125] Embodiment 4:

[0126] The method for brazing Y2O3-MgO composite ceramic and metal using TiZrNiCu active brazing filler metal in this embodiment is carried out according to the following steps:

[0127] 1. Pre-welding treatment of Y2O3-MgO composite ceramics and metal to be welded:

[0128] The Y2O3-MgO composite ceramic was cut into 4 mm×4 mm, and the metal to be welded was cut into 6 mm×10 mm. The surface to be welded of the Y2O3-MgO composite ceramic and the surface to be welded of the metal to be welded were polished and ultrasonically cleaned in sequence using 400, 600, 800, 1200, 1500, and 3000 grit sandpapers.

[0129] The ultrasonic cleaning process is as follows: the polished Y2O3-MgO composite ceramic and the metal to be welded are placed in a cleaning agent, and ultrasonically cleaned for 10 minutes in a 100kHz ultrasonic cleaning machine, and a new cleaning agent is replaced and the cleaning is repeated twice, and the cleaned Y2O3-MgO composite ceramic is placed in acetone for liquid sealing for standby use;

[0130] The metal to be welded is TC4 titanium alloy;

[0131] The cleaning agent is anhydrous ethanol;

[0132] 2. Pretreatment of TiZrNiCu active brazing filler metal:

[0133] Take a foil-shaped TiZrNiCu active solder; cut the foil-shaped TiZrNiCu active solder to 5 mm×5 mm, ensure that the TiZrNiCu active solder is larger than the to-be-welded surface of the Y2O3-MgO composite ceramic, and grind and clean both surfaces of the foil-shaped TiZrNiCu active solder;

[0134] The TiZrNiCu active solder composition comprises 22wt% Cu, 12wt% Zr, 13wt% Ni and the remainder Ti;

[0135] The thickness of the foil-shaped TiZrNiCu active solder is 6 μm;

[0136] The grinding process uses 1500 mesh and 3000 mesh sandpaper for grinding in sequence;

[0137] The cleaning process is as follows: putting the polished TiZrNiCu active solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 10 minutes, replacing the cleaning agent with a new one, and repeating the cleaning twice;

[0138] The cleaning agent is anhydrous ethanol;

[0139] 3. Assembly of parts to be welded:

[0140] The TiZrNiCu active solder is placed between the Y2O3-MgO composite ceramic and the metal to be welded to obtain an assembly;

[0141] 4. Vacuum brazing connection: put the assembly into the vacuum brazing furnace for brazing;

[0142] The vacuum degree of the vacuum brazing furnace during the brazing process is 5×10 -3 Pa;

[0143] The brazing process is as follows: first, heating to 600°C at a rate of 15°C / min, then heating to 970°C at a rate of 10°C / min and keeping the temperature for 10 minutes, then cooling to 150°C at a rate of 5°C / min, taking out the sample, and completing the brazing.

[0144] Figure 4 This is a microstructure picture of the Y2O3-MgO composite ceramic brazed joint obtained in Example 4. Figure 4 It can be seen that the welded joint is intact without obvious defects such as pores and cracks. The shear test was carried out using an electronic universal testing machine with a loading speed of 0.5 mm / min. The room temperature shear strength of the obtained connection joint was measured to reach 16 MPa.

Claims

1. A method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal, characterized in that: The method of brazing Y2O3-MgO composite ceramic and metal using TiZrNiCu active brazing filler metal is carried out in the following steps:

1. Pre-welding treatment of Y2O3-MgO composite ceramics and metal to be welded: The Y2O3-MgO composite ceramic and the metal to be welded are cut into predetermined sizes respectively, and the welded surface of the Y2O3-MgO composite ceramic and the welded surface of the metal to be welded are sanded and ultrasonically cleaned respectively; The ultrasonic cleaning process is as follows: the polished Y2O3-MgO composite ceramic and the metal to be welded are placed in a cleaning agent, and ultrasonically cleaned for 5-10 minutes in a 100kHz ultrasonic cleaning machine, and a new cleaning agent is replaced and the cleaning is repeated 2-3 times, and the cleaned Y2O3-MgO composite ceramic is placed in acetone for liquid sealing for standby use; The metal to be welded is TC4 titanium alloy; The cleaning agent is anhydrous ethanol or acetone; The sandpaper grinding process uses 400-3000 mesh sandpaper for step-by-step grinding; the sandpaper grinding step can remove surface impurities and ensure that the surface to be welded is smooth and flat; 2. Pretreatment of TiZrNiCu active brazing filler metal: Take powdered TiZrNiCu active solder or foil-shaped TiZrNiCu active solder; cut the foil-shaped TiZrNiCu active solder to a predetermined size to ensure that the TiZrNiCu active solder is larger than the to-be-welded surface of the Y2O3-MgO composite ceramic, and grind and clean both surfaces of the foil-shaped TiZrNiCu active solder; The TiZrNiCu active solder composition comprises 15-26wt% Cu, 19-27wt% Zr, 7-13wt% Ni and the remainder Ti; The thickness of the foil-shaped TiZrNiCu active solder is 3 to 10 μm; The grinding process is performed using 1500-5000 mesh sandpaper; The cleaning process is as follows: putting the polished TiZrNiCu active solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5-10 minutes, replacing the cleaning agent with a new one, and repeating the cleaning 2-3 times; The cleaning agent is anhydrous ethanol or acetone; 3. Assembly of parts to be welded: The TiZrNiCu active solder is placed between the Y2O3-MgO composite ceramic and the metal to be welded to obtain an assembly; 4. Vacuum brazing connection: put the assembly into the vacuum brazing furnace for brazing; The vacuum degree of the vacuum brazing furnace during the brazing process is 5×10 -3 Pa; The brazing process is as follows: firstly, the temperature is increased to 600°C at a rate of 5-15°C / min, then, the temperature is increased to 850-1000°C at a rate of 5-15°C / min and kept at this temperature for 10-30 minutes, then, the temperature is cooled to below 150°C at a rate of ≤5°C / min, the sample is taken out, and the brazing is completed.

2. The method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal according to claim 1, characterized in that: Step 1: Ultrasonic cleaning process: put the polished Y2O3-MgO composite ceramic and the metal to be welded into the cleaning agent, ultrasonically clean them in a 100kHz ultrasonic cleaning machine for 10 minutes, replace the new cleaning agent and repeat the cleaning twice, and put the cleaned Y2O3-MgO composite ceramic into acetone for liquid sealing for standby use.

3. The method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal according to claim 1, characterized in that: The cleaning process described in step 2 is: putting the polished TiZrNiCu active solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 10 minutes, replacing the cleaning agent with a new one, and repeating the cleaning twice.

4. The method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal according to claim 1, characterized in that: The TiZrNiCu active solder composition described in step 2 includes 22wt% Cu, 12wt% Zr, 13wt% Ni and the rest Ti.

5. The method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal according to claim 1, characterized in that: The thickness of the foil-shaped TiZrNiCu active solder in step 2 is 6 μm.

6. The method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal according to claim 1, characterized in that: In step 1, the Y2O3-MgO composite ceramic is cut into 4mm×4mm, and the metal to be welded is cut into 6mm×10mm. The welding surface of the Y2O3-MgO composite ceramic and the welding surface of the metal to be welded are polished and ultrasonically cleaned in stages using 400, 600, 800, 1200, 1500, and 3000 grit sandpapers respectively.

7. The method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal according to claim 1, characterized in that: The brazing process described in step 4 is: first, heat to 600°C at a rate of 5 to 15°C / min, then heat to 910°C at a rate of 5 to 15°C / min and keep warm for 10 to 30 minutes, then cool to below 150°C at a cooling rate of ≤5°C / min, take out the sample, and complete the brazing.

8. The method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal according to claim 1, characterized in that: The brazing process described in step 4 is: first, heat to 600°C at a rate of 5 to 15°C / min, then heat to 970°C at a rate of 5 to 15°C / min and keep warm for 10 to 30 minutes, then cool to below 150°C at a cooling rate of ≤5°C / min, take out the sample, and complete the brazing.

9. The method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal according to claim 1, characterized in that: The brazing process described in step 4 is: first, heat to 600°C at a rate of 5 to 15°C / min, then heat to 930°C at a rate of 5 to 15°C / min and keep warm for 10 to 30 minutes, then cool to below 150°C at a cooling rate of ≤5°C / min, take out the sample, and complete the brazing.

10. The method for brazing Y2O3-MgO composite ceramics and metals using TiZrNiCu active brazing filler metal according to claim 1, characterized in that: The brazing process described in step 4 is: first, heat to 600°C at a rate of 5 to 15°C / min, then heat to 950°C at a rate of 5 to 15°C / min and keep warm for 10 to 30 minutes, then cool to below 150°C at a cooling rate of ≤5°C / min, take out the sample, and complete the brazing.

Citation Information

Patent Citations

  • TiZr base amorphous alloy with low Cu and Ni contents and preparation method thereof

    CN103286473A

  • Amorphous composite brazing filler metal for brazing ceramic and alloy

    CN110153591A

  • Method for relieving stress in ceramic-metal

    CN114043026A

  • Vacuum brazing connection method for C / C radiating fins and Ti tubes

    CN114247947A

  • Joined body consisting of metallic plate and ceramic substrate

    JP1993186278A