Method for controlling porosity of extruded part
By detecting and controlling the volatile content in the rubber, the problem of uncontrollable porosity during the tire component pressing process is solved, the dimensional accuracy and performance of the component is improved, and the incidence of unqualified products is reduced.
Patent Information
- Application Number
- CN202310495485.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-05
AI Technical Summary
The porosity of the tire components is uncontrollable during the pressing process, which affects the dimensional accuracy and performance of the components, resulting in defects such as leakage lines and bubbles. The existing technology lacks effective control methods.
By detecting the volatile content in the glue, if the content is ≤0.3%, it will be pressed out. If the content is >0.30%, measures will be taken to control its content, including checking the raw materials, cooling systems and mixing machines, refining or replacing carbon black to Reduce the volatile content and ensure the quality of the glue.
The porosity of the tire pressed parts is effectively controlled, the incidence of unqualified products is reduced, and the dimensional accuracy and stability of component performance is ensured.
Smart Images

Figure CN118893804A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tires, and in particular to a method for controlling the porosity of an extruded component. Background Art
[0002] The tire manufacturing process is mainly divided into the mixing of rubber compounds, the extrusion (calendering) of various components, the component molding and the vulcanization process.
[0003] In the actual tire production process, component extrusion is a critical process, and the most critical control indicator in component extrusion is the component dimensional accuracy. Component dimensional accuracy will directly affect the performance of various aspects of the tire, such as dynamic and static balance, the pass rate of out-of-roundness, and even produce defects such as missing wires and bubbles, resulting in tire scrapping.
[0004] One of the factors that affect the dimensional accuracy of components is porosity. Currently, tire components are mainly extruded by heating and plasticizing the rubber through a screw machine (cold feed or hot feed) and then extruding it into shape. In this process, the volatile small molecules in the rubber and the air brought in expand due to heat to produce pores. Compared with other factors that affect the size of components, porosity is more uncontrollable and has large seasonal fluctuations. There is currently no effective control method. Summary of the invention
[0005] The purpose of the present invention is to provide a method for controlling the porosity of an extruded component in order to overcome the defects of the prior art, by controlling the volatile content in the rubber compound, thereby controlling the porosity of the tire extruded component.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A method for controlling the porosity of an extruded component, comprising the following steps:
[0008] S1. Detect the volatile content in the rubber;
[0009] S2, if the volatile content of the rubber obtained in step S1 is ≤0.3%, using the rubber to extrude the tread component;
[0010] S3. If the volatile content of the rubber obtained in step S1 is greater than 0.30%, measures are taken to control the volatile content of the rubber to be ≤ 0.3%, and the rubber is then used to extrude the tread component.
[0011] Furthermore, in step S1, the testing method for the volatile matter content in the rubber material is as follows:
[0012] (1) Take a certain amount of rubber sample used to prepare tires and weigh its mass as M1;
[0013] (2) drying the rubber sample weighed in step S1, cooling it to room temperature, and weighing its mass as M2;
[0014] (3) Calculate the volatile matter content W in mass fraction (%): W = (M1-M2)÷M1×100%.
[0015] Furthermore, in step (1), 10 g of a rubber sample for preparing a tire is taken, cut into 2 mm rubber sample pieces, placed in a watch glass and weighed, the weighed mass is M1, accurate to 1 mg.
[0016] Furthermore, the rubber sample for preparing the tire includes: 100 parts by weight of natural rubber or synthetic rubber, 25 to 35 parts by weight of carbon black, 15 to 25 parts by weight of white carbon black, 1 to 2 parts by weight of vulcanizing agent, 1 to 2 parts by weight of accelerator, 3 to 4 parts by weight of antioxidant and 5 to 7 parts by weight of activator.
[0017] Furthermore, in step (2), the rubber sample weighed in step S1 is placed in an oven at a temperature of 115-125° C. and dried for 1 hour, then taken out and placed in a desiccator to cool to room temperature, and its mass is weighed as M2.
[0018] Furthermore, in step (3), the volatile matter content W is the average value of the results of three sets of parallel tests.
[0019] Furthermore, in step S3, the measures taken include checking whether the rubber raw materials involved are damp, whether the rubber cooling system operates normally, or whether the internal mixer is leaking.
[0020] Furthermore, if the rubber raw materials are damp, the volatile content of the rubber can be reduced by re-refining the rubber, drying the raw rubber, and replacing the carbon black.
[0021] Furthermore, the raw rubber is dried at a temperature of 50° C. and for a drying time of 8 to 24 hours.
[0022] Furthermore, the specific method of replacing carbon black is as follows:
[0023] S1. Check the carbon black before use. If the heating loss of carbon black is ≤1.5%, then the batch of carbon black can be used to produce rubber compound normally.
[0024] S2. If the heating loss of carbon black is greater than 1.5%, this batch of carbon black shall not be used and should be replaced with other batches of carbon black.
[0025] The principle of the present invention is as follows:
[0026] The source of the porosity of the extruded parts is mainly the thermal expansion of the volatile small molecules in the rubber. Therefore, controlling the volatile content in the rubber can control the porosity of the tire extruded parts.
[0027] Compared with the prior art, the present invention has the following advantages:
[0028] (1) The method for controlling the porosity of an extruded part provided by the present invention is simple, easy to operate, and takes little time;
[0029] (2) The test data of the test method for the volatile content in the rubber provided by the present invention is directly related to the porosity of the extruded part. When the volatile content of the rubber is controlled within 0.3%, the porosity can be well maintained below 4%. When the volatile content in the rubber is greater than 0.30%, the porosity of the extruded part is greater than 4%, which is a defective product. By controlling the volatile content of the rubber, the phenomenon of excessive porosity of the parts can be effectively reduced, thereby reducing the incidence of defective products. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a schematic diagram of the volatile matter of the rubber material in the all-natural tread and the porosity of its extruded part in Example 1 of the present invention, wherein A is a qualified product and B is an unqualified product;
[0031] Figure 2 Schematic diagram of the volatile matter of the rubber material in the tread containing synthetic rubber and the porosity of the extruded part thereof in Example 2 of the present invention, wherein A is a qualified product and B is an unqualified product. DETAILED DESCRIPTION
[0032] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0033] Example 1
[0034] This embodiment provides a method for controlling the porosity of an extruded component, and the specific steps are as follows:
[0035] S1. Detect the volatile content in the rubber:
[0036] (1) Take 10 g of the rubber sample of the actual all-natural tire tread, cut it into 2 mm pieces, place it in a watch glass and weigh it. The weighed mass is M1, accurate to 1 mg;
[0037] (2) The rubber sample weighed in step (1) is placed in an oven at a temperature of 115 to 125° C. and dried for 1 hour. The sample is then taken out and placed in a desiccator to cool to room temperature. The mass thereof is weighed as M2.
[0038] (3) Calculate the volatile content W, expressed as mass fraction (%): W = (M1-M2)÷M1×100%. The volatile content W is the average value of the results of three parallel tests.
[0039] S2. If the volatile matter content in the rubber obtained in step S1 is ≤ 0.3%, the rubber is used to extrude the tread component.
[0040] S3, if the volatile content of the rubber obtained in step S1 is greater than 0.30%, taking measures to control the volatile content of the rubber to ≤ 0.3%, and then using the rubber to extrude the tread component,
[0041] Check whether the rubber raw materials are damp, whether the rubber cooling system is operating normally or whether the internal mixer is leaking to control the volatile content of the rubber. If the rubber raw materials are damp, reduce the volatile content of the rubber by re-refining the rubber, drying the raw rubber (drying temperature is 50°C, drying time is 8 to 24 hours) and replacing carbon black.
[0042] The volatile matter of the rubber in the all-natural tread and the porosity of its extruded parts were tested. The results are as follows: Figure 1 As shown in Table 1, when the porosity of the extruded part in B is greater than 4%, the volatile matter of the corresponding rubber compound is greater than 0.3%.
[0043] Table 1 Volatile matter of rubber and porosity of extruded parts
[0044]
[0045]
[0046] Example 2
[0047] This embodiment provides a method for controlling the porosity of an extruded component, and the specific steps are as follows:
[0048] S1. Detect the volatile content in the rubber:
[0049] (1) Take 10 g of a rubber sample of a tire tread containing synthetic rubber, cut it into 2 mm pieces, place it in a watch glass and weigh it. The weighed mass is M1, accurate to 1 mg;
[0050] (2) The rubber sample weighed in step (1) is placed in an oven at a temperature of 115 to 125° C. and dried for 1 hour. The sample is then taken out and placed in a desiccator to cool to room temperature. The mass thereof is weighed as M2.
[0051] (3) Calculate the volatile content W, expressed as mass fraction (%): W = (M1-M2)÷M1×100%. The volatile content W is the average value of the results of three parallel tests.
[0052] S2. If the volatile matter content in the rubber obtained in step S1 is ≤ 0.3%, the rubber is used to extrude the tread component.
[0053] S3. If the volatile content of the rubber obtained in step S1 is greater than 0.30%, measures are taken to control the volatile content of the rubber to be ≤ 0.3%, and the rubber is then used to extrude the tread component.
[0054] Check whether the rubber raw materials are damp, whether the rubber cooling system is operating normally or whether the internal mixer is leaking to control the volatile content of the rubber. If the rubber raw materials are damp, reduce the volatile content of the rubber by re-refining the rubber, drying the raw rubber (drying temperature is 50°C, drying time is 8 to 24 hours) and replacing carbon black.
[0055] The volatile matter of the rubber in the all-natural tread and the porosity of its extruded parts were tested. The results are as follows: Figure 2 As shown in Table 2, when the porosity of the extruded part in B is greater than 4%, the volatile matter of the corresponding rubber compound is greater than 0.3%.
[0056] Table 2 Volatile matter of rubber and porosity of extruded parts
[0057]
[0058]
[0059] Example 3
[0060] This embodiment provides a method for controlling the porosity of an extruded component, and the specific steps are as follows:
[0061] S1. Detect the volatile content in the rubber:
[0062] (1) Take 10 g of a rubber sample of a tire tread containing synthetic rubber, cut it into 2 mm pieces, place it in a watch glass and weigh it. The weighed mass is M1, accurate to 1 mg;
[0063] (2) The rubber sample weighed in step (1) is placed in an oven at a temperature of 115 to 125° C. and dried for 1 hour. The sample is then taken out and placed in a desiccator to cool to room temperature. The mass thereof is weighed as M2.
[0064] (3) Calculate the volatile content W, expressed as mass fraction (%): W = (M1-M2)÷M1×100%. The volatile content W is the average value of the results of three parallel tests.
[0065] S2. If the volatile matter content in the rubber obtained in step S1 is ≤ 0.3%, the rubber is used to extrude the tread component.
[0066] S3. If the volatile content of the rubber obtained in step S1 is greater than 0.30%, take measures for the batch of rubber:
[0067] (1) Return the batch of rubber to the internal mixing workshop and mix it in an internal mixer at a temperature of 80-110°C;
[0068] (2) After mixing for 2 minutes, the mixture is passed through an open mixing mill for 5 passes and then collected;
[0069] (3) The volatile content of the rubber material is detected again, the steps are the same as S1, the volatile content of the rubber material is ≤ 0.30%, and the rubber material is then used to extrude the tread component.
[0070] Example 4
[0071] This embodiment provides a method for controlling the porosity of an extruded component, and the specific steps are as follows:
[0072] S1. Detect the volatile content in the rubber:
[0073] (1) Take 10 g of a rubber sample of a tire tread containing synthetic rubber, cut it into 2 mm pieces, place it in a watch glass and weigh it. The weighed mass is M1, accurate to 1 mg;
[0074] (2) The rubber sample weighed in step (1) is placed in an oven at a temperature of 115 to 125° C. and dried for 1 hour. The sample is then taken out and placed in a desiccator to cool to room temperature. The mass thereof is weighed as M2.
[0075] (3) Calculate the volatile content W, expressed as mass fraction (%): W = (M1-M2)÷M1×100%. The volatile content W is the average value of the results of three parallel tests.
[0076] S2. If the volatile content of the rubber obtained in step S1 is greater than 0.30%, the volatile content of the raw rubber is tested before production:
[0077] (1) If the volatile matter of the raw rubber before use is ≤ 0.5% according to step S1, the raw rubber is used to produce rubber compound;
[0078] (2) Similarly, if the volatile matter of the raw rubber before use is greater than 0.5% according to step S1, the raw rubber is dried in a drying room before use. The drying temperature is 50° C. and the drying time is 8 to 24 hours.
[0079] Example 5
[0080] This embodiment provides a method for controlling the porosity of an extruded component, and the specific steps are as follows:
[0081] S1. Detect the volatile content in the rubber:
[0082] (1) Take 10 g of a rubber sample of a tire tread containing synthetic rubber, cut it into 2 mm pieces, place it in a watch glass and weigh it. The weighed mass is M1, accurate to 1 mg;
[0083] (2) The rubber sample weighed in step (1) is placed in an oven at a temperature of 115 to 125° C. and dried for 1 hour. The sample is then taken out and placed in a desiccator to cool to room temperature. The mass thereof is weighed as M2.
[0084] (3) Calculate the volatile content W, expressed as mass fraction (%): W = (M1-M2)÷M1×100%. The volatile content W is the average value of the results of three parallel tests.
[0085] S2. If the volatile content of the rubber obtained in step S1 is greater than 0.30%, the carbon black heating loss is detected before production:
[0086] (1) Take 2 g of carbon black sample and weigh it in a weighing bottle. The weighed mass is M1 and the accuracy is 0.1 mg;
[0087] (2) Place the rubber sample weighed in step (1) in an oven at 125±1°C for 30 min, take it out, place it in a desiccator and cool it to room temperature, and weigh its mass as M2;
[0088] (3) Calculate the heating loss W in mass fraction (%): W = (M1-M2)÷M1×100%, and the volatile content W is the average value of the results of three parallel tests.
[0089] (4) If the heating loss of carbon black is ≤1.5%, then this batch of carbon black is used to produce rubber compound;
[0090] (5) If the heating loss of carbon black is greater than 1.5%, the carbon black in this batch shall not be used and other batches of carbon black shall be replaced;
[0091] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for controlling the porosity of an extruded part, characterized in that: The specific steps are as follows: S1. Detect the volatile content in the rubber; S2, if the volatile matter content in the rubber obtained in step S1 is ≤0.3%, using the rubber to extrude the tread component; S3. If the volatile content of the rubber obtained in step S1 is greater than 0.30%, measures are taken to control the volatile content of the rubber to be ≤ 0.3%, and the rubber is then used to extrude the tread component.
2. A method for controlling the porosity of an extruded part according to claim 1, characterized in that: In step S1, the testing method of the volatile matter content in the rubber material is as follows: (1) Take a certain amount of rubber sample used to prepare tires and weigh its mass as M1; (2) drying the rubber sample weighed in step S1, cooling it to room temperature, and weighing its mass as M2; (3) Calculate the volatile matter content W in mass fraction (%): W = (M1-M2)÷M1×100%.
3. A method for controlling the porosity of an extruded part according to claim 2, characterized in that: In step (1), 10 g of a rubber sample for preparing a tire is taken, cut into 2 mm rubber sample pieces, placed in a watch glass and weighed, the weighed mass is M1, accurate to 1 mg.
4. A method for controlling the porosity of an extruded part according to claim 3, characterized in that: The rubber sample for preparing the tire comprises: 100 parts by weight of natural rubber or synthetic rubber, 25 to 35 parts by weight of carbon black, 15 to 25 parts by weight of white carbon black, 1 to 2 parts by weight of a vulcanizing agent, 1 to 2 parts by weight of an accelerator, 3 to 4 parts by weight of an antioxidant and 5 to 7 parts by weight of an activator.
5. A method for controlling the porosity of an extruded part according to claim 2, characterized in that: In step (2), the rubber sample weighed in step S1 is placed in an oven at a temperature of 115-125° C. and dried for 1 hour, then taken out and placed in a desiccator to cool to room temperature, and its mass is weighed as M2.
6. A method for controlling the porosity of an extruded part according to claim 2, characterized in that: In step (3), the volatile content W is the average value of the results of three parallel tests.
7. A method for controlling the porosity of an extruded part according to claim 1, characterized in that: In step S3, the measures taken include checking whether the rubber raw materials involved are damp, whether the rubber cooling system operates normally, or whether the internal mixer is leaking.
8. A method for controlling the porosity of an extruded part according to claim 7, characterized in that: If the rubber raw materials are damp, the volatile content of the rubber can be reduced by re-refining the rubber, drying the raw rubber, and replacing the carbon black.
9. A method for controlling the porosity of an extruded part according to claim 8, characterized in that: The raw rubber is dried at a temperature of 50° C. and for a drying time of 8 to 24 hours.
10. A method for controlling the porosity of an extruded part according to claim 8, characterized in that: The specific method of replacing carbon black is as follows: S1. Check the carbon black before use. If the heating loss of carbon black is ≤1.5%, then the batch of carbon black can be used to produce rubber compound normally. S2. If the heating loss of carbon black is greater than 1.5%, this batch of carbon black shall not be used and other batches of carbon black shall be replaced.