Low-residual-alkali high-nickel ternary positive electrode material and preparation method thereof

By cleaning and coating the high-nickel ternary positive electrode material with boric acid, nano-alumina and cobalt hydroxyoxide in a sand bath rotary evaporator, the residual alkali problem in the preparation of high-nickel ternary materials is solved and the material is improved Cycling performance and capacitance avoid the time consumption of electric furnace sintering.

CN118894557APending Publication Date: 2024-11-05HEFEI GUOXUAN HIGH TECH POWER ENERGY CO LTD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410936087.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

High nickel ternary cathode material is sensitive to the environment during the preparation process and is easy to react with CO2 and H2O in the air to form residual alkali, which affects the safety performance and cycle life of the battery. Existing removal methods such as water washing and acid-base neutralization lead to degradation of material properties. .

Method used

The high-nickel ternary positive electrode material was cleaned and coated with boric acid, nano-alumina and cobalt hydroxyoxide in a non-aqueous environment using a sand bath rotary evaporator. The residual alkali was removed through acid-base neutralization reaction, and at 400 The surface cladding layer is generated by heat treatment of -600°C, eliminating the secondary sintering step of the electric furnace.

Benefits of technology

It effectively reduces the residual alkali on the surface of the material, improves the cycling performance and capacitance, solves the problems of degradation of material properties after pickling and poor uniformity of solid-phase coating dispersion, and saves heat treatment time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894557A_ABST
    Figure CN118894557A_ABST
Patent Text Reader

Abstract

The invention relates to a low-residual alkali high-nickel ternary positive electrode material and a preparation method thereof, and the preparation method comprises the following steps: S1, uniformly stirring and mixing nickel-cobalt-manganese hydroxide ternary precursor solid powder and LiOH.H2O, calcining, and naturally cooling to room temperature to obtain a high-nickel ternary positive electrode material; s2, adding boric acid and a derivative thereof into ethanol, and stirring until the boric acid and the derivative are completely dissolved, so as to obtain an ethanol solution containing boric acid radicals; adding the high-nickel ternary positive electrode material into an ethanol solvent containing borate radicals, uniformly stirring and mixing, and washing with ethanol to obtain a suspension; and S3, adding the turbid liquid, hydroxyl cobalt oxide and nano aluminum oxide into a sand bath rotary evaporator, carrying out rotary evaporation until the powder is completely dried, then carrying out heat treatment, and naturally cooling to room temperature, so as to obtain the high-nickel ternary positive electrode material with a coating layer on the surface. The method effectively solves the problems of material circulation, capacitance and other performance reduction caused by loss of part of active substances and damage of a crystal structure of the acid-washed ternary material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a low-residual-alkali-high-nickel ternary positive electrode material and a preparation method thereof. Background Art

[0002] With the continuous advancement of science and technology and the continuous improvement of the national economic level, lithium-ion batteries have been widely used in consumer electronics, energy storage devices and new energy vehicles in my country. In particular, in recent years, with the strong support of relevant national policies and the demand driven by national consumption, the requirements for battery energy density in electric vehicles have also continued to increase. High-nickel ternary positive electrode materials have gradually become one of the most widely used and most promising positive electrode materials on the market. However, with the increase of nickel content, the environmental requirements of ternary positive electrode materials during preparation become higher and they are very sensitive to environmental humidity. High-nickel ternary materials can easily react with CO2 and H2O in the air to generate LiOH and Li2CO3 on the surface of the material. LiOH reacts with lithium hexafluorophosphate in the electrolyte to generate HF, while Li2CO3 decomposes at high temperatures to produce gas expansion, both of which will seriously damage the overall safety performance of the battery; secondly, the continuous increase in nickel content will also increase the probability of Li / Ni mixing inside the material, shortening the cycle life of the positive electrode material, which has become the key to restricting the application of high-nickel ternary materials in high-energy-density power batteries for vehicles.

[0003] At present, the industry mainly uses water washing to remove the residual alkali on the surface of high-nickel ternary materials. Although this process has the characteristics of simple operation and low cost, from the perspective of material performance after water washing, the loss of active lithium in the water washing process will generally greatly reduce the specific capacity, and the internal resistance of the battery will increase, affecting the cycle life and safety performance of the material. The patent with publication number CN110054226B provides a method for preparing a nickel-cobalt-manganese ternary positive electrode material with low surface residual alkali, which adopts the acid-base neutralization principle and utilizes the free H in a non-aqueous phase (ethanol) environment. + The acid-base neutralization reaction occurs with the residual alkali on the surface of the material, and the reaction intensity is regulated by the stirring time, which effectively reduces the residual alkali on the surface of the material and lowers the pH value of the material. However, this method will cause a certain degree of dissolution of the ternary positive electrode material crystals after the acid reaction is introduced, destroying the material structure and causing some active component loss. However, this method only repairs this by performing a low-temperature secondary calcination process, which is not enough to solve the poor cycle performance and rapid capacity decay problems shown in the subsequent testing of the pickled material. Summary of the invention

[0004] Based on this, in view of the technical problems existing in the prior art, the purpose of the present invention is to provide a low residual alkali and high nickel ternary positive electrode material and a preparation method thereof, to improve the above-mentioned problems, the positive electrode material after acid washing to remove the residual alkali, the coating agent and an appropriate amount of ethanol are placed together in a sand bath rotary evaporator and stirred and mixed, and the uniformity of the coating material dispersion is optimized by regulating the rotation time and evaporation temperature of the rotary evaporator, and the surface-coated ternary positive electrode material is directly generated at a heat treatment temperature of 400-600°C, eliminating the secondary sintering step in an electric furnace, and saving processing time compared to electric furnace sintering (10-15h). The obtained ternary positive electrode material has low residual alkali, good cycle performance, and can improve the capacitance of the material to a certain extent, and its performance is significantly better than the positive electrode material directly coated by the solid phase method.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for preparing a low-residual-alkali-high-nickel ternary positive electrode material, which comprises the following steps:

[0007] S1. The nickel-cobalt-manganese hydroxide ternary precursor solid powder is stirred and mixed with LiOH·H2O, and then calcined, and naturally cooled to room temperature to obtain a high-nickel ternary positive electrode material;

[0008] S2. Add boric acid and its derivatives to ethanol and stir until completely dissolved to obtain an ethanol solution containing borate; add the high-nickel ternary cathode material to the ethanol solvent containing borate and stir to mix evenly, rinse with ethanol to obtain a suspension;

[0009] S3. Add the suspension, cobalt hydroxide oxide and nano-alumina into a sand bath rotary evaporator, and rotary evaporate until the powder is completely dry. After heat treatment, naturally cool to room temperature to obtain a high-nickel ternary positive electrode material with a coating layer on the surface, wherein the coating layer contains Li3BO3, LiCoO2 and Al2O3.

[0010] The present invention uses an ethanol phase solution doped with boric acid and its derivatives, nano-aluminum oxide and cobalt hydroxide oxide to clean and coat the high-nickel ternary positive electrode material. On the one hand, the residual alkali generated on the surface of the material is removed by an acid-base neutralization reaction. On the other hand, a sand bath rotary evaporator is used to add a cobalt source and an aluminum source as a coating agent in a non-aqueous phase environment, and the cobalt source and the aluminum source continue to react with Li precipitated on the surface of the positive electrode material to generate LiCoO2 to improve the specific capacity of the material. At the same time, an Al2O3 coating layer is generated on the surface of the positive electrode material to isolate the electrolyte corrosion and improve its cycle performance. The problems of decreased material performance after pickling and poor dispersion uniformity of the coated material compared with the solid phase method are solved, the electric furnace secondary sintering step is omitted, and the heat treatment time is saved compared with the electric furnace sintering (10 to 15 hours). The obtained ternary positive electrode material has low residual alkali content and good cycle performance, and can improve the capacitance of the material to a certain extent. Its performance is significantly better than that of the positive electrode material directly coated by the solid phase method.

[0011] As a further improvement of the above scheme of the present invention, in step S1, the molar ratio of the nickel-cobalt-manganese hydroxide ternary precursor solid powder to LiOH·H2O is 1:1.05-1.10;

[0012] And / or, in step S1, the calcination is carried out in an oxygen atmosphere at 750°C to 900°C for 18-25h, and the heating rate during the calcination stage is 3-7°C / min;

[0013] And / or, in step S1, the molecular formula of the high nickel ternary positive electrode material is Li(Ni 1-x-y Co x Mn y )O2, where 0.07≤x≤0.1, 0.05≤y≤0.15.

[0014] As a further improvement of the above scheme of the present invention, in step S2, the boric acid and its derivatives are at least one of boric acid, metaboric acid, tetraboric acid, and ammonium borate;

[0015] And / or, in step S2, the mass of the boron element in the boric acid and its derivatives is 500-1000ppm of the mass of the high-nickel ternary positive electrode material.

[0016] As a further improvement of the above scheme of the present invention, in step S2, the volume ratio of the high-nickel ternary positive electrode material and the ethanol solution containing borate is 1:1.2-1.5; the solution acid concentration configured in this ratio is moderate. When the acid concentration is too low, the reaction of the residual alkali on the surface is incomplete and the expected effect cannot be achieved. When the concentration is too high, the positive electrode material itself will be corroded, resulting in the adverse consequence of material performance degradation.

[0017] As a further improvement of the above scheme of the present invention, in step S3, the added amount of the cobalt hydroxide oxide is 3000-9000ppm of the mass of the high-nickel ternary positive electrode material, and the added amount of the nano-alumina is 500-3000ppm of the mass of the high-nickel ternary positive electrode material; so as to optimize the comprehensive performance of the materials.

[0018] As a further improvement of the above scheme of the present invention, in step S3, the heating medium of the sand bath rotary evaporator is high-purity quartz sand. The maximum operating temperature of the sand bath rotary evaporator is 600°C, so the heating medium is selected as high-purity quartz sand. In this temperature range, the quartz sand can maintain stable properties.

[0019] As a further improvement of the above scheme of the present invention, in step S3, the drying is carried out in a sand bath rotary evaporator at 40°C-80°C for 0.5h-1h; the ethanol is first slowly evaporated, and during this process, the coating agent (cobalt hydroxide oxide, nano-aluminum oxide, boric acid and its derivatives) can be evenly distributed on the surface of the high-nickel ternary positive electrode material, waiting for the reaction in the high-temperature calcination stage.

[0020] As a further improvement of the above scheme of the present invention, in step S3, the heat treatment is carried out in a sand bath rotary evaporator at 400°C-600°C for 6h-12h. Preferably, the heat treatment temperature is 550°C and the time is 8h to ensure the reaction is carried out effectively.

[0021] As a further improvement of the above solution of the present invention, in step S3, the particle size D50 of the high nickel ternary positive electrode material with a coating layer on the surface is 2.0-10 μm;

[0022] And / or, in step S3, the particle size D50 of the cobalt oxyhydroxide and nano-aluminum oxide is 80-300 nm; the nano-crystallization of the coating agent can increase its own reaction activity, and the degree of reaction participation is higher when calcined with the positive electrode material.

[0023] The present invention provides a low-residual-alkali high-nickel ternary positive electrode material, which is prepared by the preparation method as described above.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention uses an ethanol phase solution doped with borate, nano-aluminum oxide and cobalt hydroxide oxide to clean and coat the high-nickel ternary positive electrode material. On the one hand, the residual alkali generated on the surface of the material is removed by an acid-base neutralization reaction. On the other hand, a sand bath rotary evaporator is used to add a cobalt source and an aluminum source as a coating agent in a non-aqueous phase environment, and the cobalt source and the aluminum source continue to react with Li precipitated on the surface of the positive electrode material to generate LiCoO2 to improve the specific capacity of the material. At the same time, an Al2O3 coating layer is generated on the surface of the positive electrode material to isolate the electrolyte corrosion and improve its cycle performance. The problems of decreased material performance after pickling and poor dispersion uniformity of the coated material compared with the solid phase method are solved, the electric furnace secondary sintering step is omitted, and the heat treatment time is saved compared with the electric furnace sintering (10 to 15 hours). The obtained ternary positive electrode material has low residual alkali content and good cycle performance, and can improve the capacitance of the material to a certain extent. Its performance is significantly better than that of the positive electrode material directly coated by the solid phase method.

[0026] The present invention effectively solves the problem of degradation of material circulation, capacitance and other performances of the ternary material after pickling due to the loss of some active substances and destruction of the crystal structure. At the same time, compared with the solid phase coating method, it improves the uniformity of the dispersion of the coating material and enhances the coating effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 These are electron microscope images of NCM-1 to NCM-6 materials;

[0028] Figure 2 XRD diffraction patterns of NCM-0, NCM-1 and NCM-2 materials;

[0029] Figure 3 This is the result of 100 cycle tests of CR2025 button batteries made of NCM-0 to NCM-6 materials. DETAILED DESCRIPTION

[0030] For ease of understanding of the present invention, the present invention will be described more fully below in conjunction with specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0032] The instrument information used in the following examples and comparative examples is as follows:

[0033] Rotary evaporator: instrument model is R-1050, Zhengzhou, China;

[0034] Digital constant temperature sand bath: The instrument model is SY-2 sand bath, Shanghai, China;

[0035] Multipotential titrator, instrument model T5, Shanghai, China;

[0036] Scanning electron microscope: The instrument model is Phenom Nano G2, Phenom Nano, the Netherlands;

[0037] X-ray diffractometer, instrument model is MiniFlex 600, Rigaku Corporation, Japan;

[0038] Inductively coupled plasma atomic emission spectrometer, instrument model is Lab ICP 1000, Beijing, China.

[0039] The above-mentioned instruments are only for illustrating the sources and models of the instruments used in the experiments of the present invention so as to fully disclose the information, and do not mean that the present invention cannot be realized by using other similar instruments or instruments provided by other suppliers.

[0040] Preparation of high nickel ternary positive electrode material: Ni, cobalt, manganese ternary positive electrode material precursor Ni 0.90 Co 0.06 Mn 0.04 (OH)2 and LiOH·H2O solid powders were put into a high-speed mixer at a molar ratio of 1:1.05, stirred evenly in the high-speed mixer, placed in a tubular furnace and calcined at 840°C for 12 h under an oxygen atmosphere. The heating rate in the calcination stage was 5°C / min. After naturally cooling to room temperature, the powder was crushed through a 300-mesh sieve to obtain a nickel-cobalt-manganese ternary positive electrode material, recorded as NCM-0.

[0041] The NCM-0 was tested by inductively coupled plasma atomic emission spectrometry (ICP-AES) using an inductively coupled plasma atomic emission spectrometer. The ICP-AES test results showed that the elemental composition of NCM-0 was LiNi 0.88 Co 0.07 Mn 0.05 , the presence of C and H elements was not detected.

[0042] The XRD results of NCM-0 material are as follows Figure 2 As shown, it can be seen that its crystal structure is a typical α-NaFeO2 layered structure, belonging to the R-3m space group.

[0043] Comparative Example 1

[0044] This comparative example proposes a high-nickel ternary positive electrode material, and its preparation method comprises the following steps:

[0045] S1. Boric acid, cobalt oxyhydroxide, nano-alumina and NCM-0 were added to a high-speed mixer and mechanically stirred for 50 min to obtain a blended powder; wherein the addition amounts of boric acid, cobalt oxyhydroxide and nano-alumina were 1000ppm, 4000ppm and 800ppm of the mass of NCM-0, respectively;

[0046] S2. The blended powder obtained in step S1 is placed in an oxidizing atmosphere and calcined at 550°C for 14 hours. The heating rate during the calcination stage is 5°C / min. After naturally cooling to room temperature, a high-nickel ternary positive electrode material coated with Li3BO3 and LiCoO2 is obtained, which is marked as NCM-1.

[0047] The SEM results of NCM-1 material are as follows Figure 1 As shown, from Figure 1 It can be seen that the NCM-1 material is a secondary particle composed of multiple primary particles, and the surface of the secondary particles is clean without obvious impurities.

[0048] The XRD results of NCM-1 material are shown in Figure 2 As shown, it can be seen that its crystal structure is a typical α-NaFeO2 layered structure, belonging to the R-3m space group.

[0049] Example 1

[0050] This embodiment provides a low residual alkali high nickel ternary positive electrode material, and the preparation method thereof comprises the following steps:

[0051] S1. Add boric acid to the ethanol solvent and stir until completely dissolved to obtain a boric acid ethanol solution with a concentration of 0.01 mol / L; then slowly add NCM-0 to the boric acid ethanol solution in batches and stir for 10 to 20 minutes, wherein the solid-liquid volume ratio of NCM-0 to the boric acid ethanol solution is 1:1.5; rinse with ethanol 2 to 5 times to remove excess borate to obtain a uniformly mixed suspension;

[0052] S2. Slowly add cobalt hydroxide oxide and nano-alumina to the suspension obtained in step S1 in batches, and the addition amounts of cobalt hydroxide oxide and nano-alumina are 4000ppm and 800ppm of the mass of NCM-0, respectively; add ethanol to 100mL, and then pour the obtained mixed solution into the rotary bottle of a sand bath rotary evaporator, and rotary evaporate at 70°C until the positive electrode material powder is completely dry; then gradually heat up to 550°C at 3°C / min and continue heat treatment for 10h, and naturally cool to room temperature to obtain a high nickel ternary positive electrode material coated with Li3BO3, LiCoO2 and Al2O3, marked as NCM-2.

[0053] The SEM results of NCM-2 material are as follows Figure 1 As shown, from Figure 1It can be seen that the NCM-2 material is a secondary particle composed of multiple primary particles, and the surface of the secondary particles is clean without obvious impurities.

[0054] The XRD results of NCM-2 material are as follows Figure 2 As shown, it can be seen that its crystal structure is a typical α-NaFeO2 layered structure, belonging to the R-3m space group.

[0055] Example 2

[0056] This embodiment provides a low residual alkali high nickel ternary positive electrode material, and the preparation method thereof comprises the following steps:

[0057] S1. Add boric acid and tetraboric acid to an ethanol solvent and stir until completely dissolved to obtain a boric acid ethanol solution with a concentration of 0.02 mol / L; then slowly add NCM-0 to the boric acid ethanol solution in batches and stir for 10 to 20 minutes, wherein the solid-liquid volume ratio of NCM-0 to the boric acid ethanol solution is 1:1.5; rinse with ethanol 2 to 5 times to remove excess borate to obtain a uniformly mixed suspension;

[0058] S2. Slowly add cobalt hydroxide oxide and nano-alumina to the suspension obtained in step S1 in batches, and the addition amounts of cobalt hydroxide oxide and nano-alumina are 2500ppm and 500ppm of the mass of NCM-0, respectively; add ethanol to 100mL, and then pour the obtained mixed solution into the rotary bottle of a sand bath rotary evaporator, and rotary evaporate at 80°C until the positive electrode material powder is completely dry; then gradually heat up to 550°C at 3°C / min and continue heat treatment for 10h, and naturally cool to room temperature to obtain a high nickel ternary positive electrode material coated with Li3BO3, LiCoO2 and Al2O3, marked as NCM-3.

[0059] The SEM results of NCM-3 material are as follows Figure 1 As shown, from Figure 1 It can be seen that the NCM-3 material is a secondary particle composed of multiple primary particles, and the surface of the secondary particles is clean without obvious impurities.

[0060] Example 3

[0061] This embodiment provides a low residual alkali high nickel ternary positive electrode material, and the preparation method thereof comprises the following steps:

[0062] S1. Add boric acid and metaboric acid to an ethanol solvent and stir until completely dissolved to obtain a boric acid / tetraboric acid ethanol solution with a concentration of 0.005 mol / L; then slowly add NCM-0 to the boric acid ethanol solution in batches and stir for 20 to 40 minutes, wherein the solid-liquid volume ratio of NCM-0 to the boric acid ethanol solution is 1:1.5; rinse with ethanol 2 to 5 times to remove excess borate to obtain a uniformly mixed suspension;

[0063] S2. Slowly add cobalt hydroxide oxide and nano-alumina to the suspension obtained in step S1 in batches, and the addition amounts of cobalt hydroxide oxide and nano-alumina are 6000ppm and 3000ppm of the mass of NCM-0, respectively; add ethanol to 100mL, and then pour the obtained mixed solution into the rotary bottle of a sand bath rotary evaporator, and rotary evaporate at 60°C until the positive electrode material powder is completely dry; then gradually heat up to 550°C at 3°C / min and continue heat treatment for 10h, and naturally cool to room temperature to obtain a high nickel ternary positive electrode material coated with Li3BO3, LiCoO2 and Al2O3, marked as NCM-4.

[0064] The SEM results of NCM-4 material are as follows Figure 1 As shown in the figure, it can be seen that the NCM-4 material is a secondary particle composed of multiple primary particles, and the surface of the secondary particles is clean without obvious impurities.

[0065] Example 4

[0066] This embodiment provides a low residual alkali high nickel ternary positive electrode material, and the preparation method thereof comprises the following steps:

[0067] S1. Add boric acid to the ethanol solvent and stir until completely dissolved to obtain a boric acid ethanol solution with a concentration of 0.01 mol / L; then slowly add NCM-0 to the boric acid ethanol solution in batches and stir for 10 to 20 minutes, wherein the solid-liquid volume ratio of NCM-0 to the boric acid ethanol solution is 1:1.5; rinse with ethanol 2 to 5 times to remove excess borate to obtain a uniformly mixed suspension;

[0068] S2. Slowly add cobalt hydroxide oxide and nano-alumina to the suspension obtained in step S1 in batches, and the addition amounts of cobalt hydroxide oxide and nano-alumina are 4000ppm and 800ppm of the mass of NCM-0, respectively; add ethanol to 100mL, and then pour the obtained mixed solution into the rotary bottle of a sand bath rotary evaporator, and rotary evaporate at 70°C until the positive electrode material powder is completely dry; then gradually heat up to 400°C at 3°C / min and continue heat treatment for 10h, and naturally cool to room temperature to obtain a high nickel ternary positive electrode material coated with Li3BO3, LiCoO2 and Al2O3, marked as NCM-5.

[0069] The SEM results of NCM-5 material are as follows Figure 1 As shown, from Figure 1 It can be seen that the NCM-5 material is a secondary particle composed of multiple primary particles, and the surface of the secondary particles is clean without obvious impurities.

[0070] Example 5

[0071] This embodiment provides a low residual alkali high nickel ternary positive electrode material, and the preparation method thereof comprises the following steps:

[0072] S1. Add boric acid to the ethanol solvent and stir until completely dissolved to obtain a boric acid ethanol solution with a concentration of 0.01 mol / L; then slowly add NCM-0 to the boric acid ethanol solution in batches and stir for 10 to 20 minutes, wherein the solid-liquid volume ratio of NCM-0 to the boric acid ethanol solution is 1:1.5; rinse with ethanol 2 to 5 times to remove excess borate to obtain a uniformly mixed suspension;

[0073] S2. Slowly add cobalt hydroxide oxide and nano-alumina to the suspension obtained in step S1 in batches, and the addition amounts of cobalt hydroxide oxide and nano-alumina are 4000ppm and 800ppm of the mass of NCM-0, respectively; add ethanol to 100mL, and then pour the obtained mixed solution into the rotary bottle of a sand bath rotary evaporator, and rotary evaporate at 70°C until the positive electrode material powder is completely dry; then gradually heat up to 600°C at 3°C / min and continue heat treatment for 12h, and naturally cool to room temperature to obtain a high nickel ternary positive electrode material coated with Li3BO3, LiCoO2 and Al2O3, marked as NCM-6.

[0074] The SEM results of NCM-6 material are as follows Figure 1 As shown, from Figure 1 It can be seen that the NCM-6 material is a secondary particle composed of multiple primary particles, and the surface of the secondary particles is clean without obvious impurities.

[0075] Test Case

[0076] (1) The residual alkali test on the surface of NCM-0, NCM-1, NCM-2, NCM-3, NCM-4, NCM-5 and NCM-6 was carried out using a multipotential titrator. The LiOH, Li2CO3 and free lithium content on the surface of NCM-0, NCM-1, NCM-2, NCM-3, NCM-4, NCM-5 and NCM-6 products measured by the multipotential titrator are shown in Table 1.

[0077] Table 1

[0078]

[0079] From the results in Table 1, it can be seen that compared with NCM-1, the residual alkali on the surface of high nickel ternary cathode materials NCM-2 to NCM-6 after liquid phase pickling is significantly reduced. This shows that compared with solid phase mixing, due to the addition of ethanol medium, the free H +It is easier to contact the residual alkali on the surface of the positive electrode material to undergo acid-base neutralization reaction; compared with Example 1, when Example 3 uses a lower concentration of pickling solution, even if the reaction and neutralization time is longer than that of Example 1, the residual alkali on the surface of the final finished product is greater than that of the finished product in Example 1. This is because the boric acid concentration is too low and is not enough to completely react with the residual alkali; when a higher concentration of pickling solution is used, such as Example 2, the residual alkali on the surface of the final finished product is not much different from that on the surface of the finished product in Example 2, and the higher concentration of pickling solution may cause more serious corrosion to the crystal structure of the positive electrode material. Therefore, the preferred pickling solution concentration in the present invention is 0.01 mol / L.

[0080] (2) NCM-n (NCM-0, NCM-1, NCM-2, NCM-3, NCM-4, NCM-5, NCM-6) were used to assemble CR2025 button cells. The assembly method of CR2025 button cells is as follows: NCM-n, acetylene black, and polyvinylidene fluoride (PVDF) dissolved in N-methylpyrrolidone (NMP) were prepared into a uniform slurry in a mass ratio of 8:1:1 and coated on an aluminum foil. After drying, the aluminum foil loaded with active materials was cut into small discs with a diameter of 11 mm using a cutting machine as the positive electrode, a metal lithium sheet was used as the half-cell negative electrode, Celgard2300 was used as a separator, and a 1M carbonate solution was used as the electrolyte (wherein the solvent was a mixed solution of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1, and the solvent was LiPF6). The CR2025 button cells were assembled in an argon glove box.

[0081] The assembled CR2025 button battery was charged and discharged for 100 cycles at 2.75V~4.3V and 0.2C rate using a CT2001ALAND battery tester (defined as 1C current density of 200mA / g, charge and discharge voltage range of 2.75V~4.3V, and test temperature of 25°C). The electrochemical performance results are shown in Figure 3 shown.

[0082] from Figure 3 The results show that, by comparing the cycle data of NCM-0 material with the cycle data of NCM-1 to NCM-6 materials, the use of cobalt oxyhydroxide and nano-aluminum oxide as coating agents can significantly improve the cycle stability of the ternary positive electrode material; from the cycle data of NCM-1 to NCM-6, it can be seen that the ternary positive electrode material coated by the solid phase method (NCM-1) has an obvious capacity decay trend after 60 cycles, and the capacity is 89% of the initial capacity after 100 cycles; while the material cycle stability measured by the liquid phase environment and sand bath rotary evaporator coating method (NCM-2 to NCM-6) is better, and the capacity is 95% of the initial capacity after 100 cycles, indicating that the method of the present invention can make the coating material more evenly dispersed and coated on the surface of the ternary material, and the performance of the raw materials is more significantly improved after coating.

[0083] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0084] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a low residual alkali high nickel ternary positive electrode material, characterized in that: It includes the following steps: S1. The nickel-cobalt-manganese hydroxide ternary precursor solid powder is stirred and mixed with LiOH·H2O, and then calcined and naturally cooled to room temperature to obtain a high-nickel ternary positive electrode material; S2. Adding boric acid and its derivatives to ethanol and stirring until completely dissolved to obtain an ethanol solution containing borate; adding the high-nickel ternary cathode material to the ethanol solvent containing borate and stirring to mix evenly, washing with ethanol to obtain a suspension; S3. Add the suspension, cobalt hydroxide oxide and nano-alumina into a sand bath rotary evaporator, and rotary evaporate until the powder is completely dry, then heat treat and naturally cool to room temperature to obtain a high-nickel ternary positive electrode material with a coating layer on the surface, wherein the coating layer contains Li3BO3, LiCoO2 and Al2O3.

2. The method for preparing the low residual alkali high nickel ternary positive electrode material according to claim 1, characterized in that: In step S1, the molar ratio of the nickel-cobalt-manganese hydroxide ternary precursor solid powder to LiOH·H2O is 1:1.05-1.10: And / or, in step S1, the calcination is carried out in an oxygen atmosphere at 750°C to 900°C for 18-25h, and the heating rate during the calcination stage is 3-7°C / min; And / or, in step S1, the molecular formula of the high nickel ternary positive electrode material is Li(Ni 1-x-y Co x Mn y )O2, where 0.07≤x≤0.1, 0.05≤y≤0.

15.

3. The method for preparing the low residual alkali high nickel ternary positive electrode material according to claim 1, characterized in that: In step S2, the boric acid and its derivatives are at least one of boric acid, metaboric acid, tetraboric acid, and ammonium borate; And / or, in step S2, the mass of the boron element in the boric acid and its derivatives is 500-1000ppm of the mass of the high-nickel ternary positive electrode material.

4. The method for preparing the low residual alkali high nickel ternary positive electrode material according to claim 3, characterized in that: In step S2, the volume ratio of the high-nickel ternary positive electrode material and the ethanol solution containing borate is 1:1.2-1.

5.

5. The method for preparing the low residual alkali high nickel ternary positive electrode material according to claim 1, characterized in that: In step S3, the added amount of the cobalt oxyhydroxide is 3000-9000 ppm of the mass of the high-nickel ternary positive electrode material, and the added amount of the nano-aluminum oxide is 500-3000 ppm of the mass of the high-nickel ternary positive electrode material.

6. The method for preparing the low residual alkali high nickel ternary positive electrode material according to claim 1, characterized in that: In step S3, the heating medium of the sand bath rotary evaporator is high-purity quartz sand.

7. The method for preparing the low residual alkali high nickel ternary positive electrode material according to claim 1, characterized in that: In step S3, the drying is carried out in a sand bath rotary evaporator at 40°C-80°C for 0.5h-1h.

8. The method for preparing the low residual alkali high nickel ternary positive electrode material according to claim 1, characterized in that: In step S3, the heat treatment is carried out in a sand bath rotary evaporator at 400°C-600°C for 6h-12h.

9. The method for preparing the low residual alkali high nickel ternary positive electrode material according to claim 1, characterized in that: In step S3, the particle size D50 of the high nickel ternary positive electrode material with a coating layer on the surface is 2.0-10 μm; And / or, in step S3, the particle size D50 of the cobalt oxyhydroxide and nano-aluminum oxide is 80-300 nm.

10. A low residual alkali high nickel ternary positive electrode material, characterized in that: The invention is prepared by the preparation method described in any one of claims 1 to 9.