Preparation method of sewage oxidation treatment material based on magnetothermal effect

By forming a specific organic compound layer on the surface of the foam copper matrix and loading manganese magnesium gadolinium oxide nanocrystals, using magnetothermal effect to treat the materials, the 2,2',5,5'-tetrachlorobenzine sewage in the prior art is solved by using the magnetic and thermal effect to decompose 2,2',5,5'-tetrachlorobenzine sewage in the prior art. The problem of efficient degradation and reusing stability is achieved.

CN118894589AActive Publication Date: 2024-11-05SONGZI SHANGCHUAN ENVIRONMENTAL TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411165187.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-05
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

In the prior art, when treating organic wastewater containing 2,2',5,5'-tetrachlorobenzidine, the physical treatment method can only be transferred rather than decomposed, and the chemical oxidation and degradation effect is not ideal, resulting in secondary pollution and environmental threats.

Method used

Using the preparation method of wastewater oxidation treatment material based on magnetothermal effect, the organic compound layer of trimethylamine and maleamide iron oxide is formed on the surface of the foam copper matrix, and the manganese magnesium gadolinium oxide nanocrystals are loaded, and the magnetothermal effect is promoted by using alternating magnetic field. Promote the oxidative degradation of 2,2',5,5'-tetrachlorobenzidine.

Benefits of technology

The degradation rate of 2,2',5,5'-tetrachlorobenzidine is significantly improved, and the reusability stability of the treated materials is maintained, avoiding secondary contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894589A_ABST
    Figure CN118894589A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a sewage oxidation treatment material based on a magnetothermal effect. The preparation method sequentially comprises the following steps: (1) forming a Fe (C3H9NO) 3 organic compound layer on the surface of a foamy copper matrix; (2) converting the trimethylamine iron oxide Fe (C3H9NO) 3 organic compound layer into a maleic amide / trimethylamine iron oxide Fe (C4H3NO2) 2 (C3H9NO) organic compound layer; and (3) loading manganese magnesium gadolinium oxide Mn < 1-x > Mg < x > Gd < 2 > O < 4 > nanocrystals on the maleic amide / trimethylamine iron oxide Fe (C4H3NO2) 2 (C3H9NO) organic compound layer to obtain the sewage oxidation treatment material. The oxidation treatment material prepared by the method disclosed by the invention has excellent degradation rate of 2, 2 ', 5, 5'-tetrachlorobenzidine and excellent reuse stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of organic wastewater treatment technology, and in particular to a method for preparing wastewater oxidation treatment materials based on the magnetocaloric effect. Background Technology

[0002] Benzidine yellow organic pigments possess excellent coloring properties, vibrant colors, and outstanding solvent and heat resistance, making them widely used in coatings, plastics, and printing. The synthesis of benzidine yellow organic pigments involves diazotization followed by coupling. Because the diazotized component in the intermediate synthesis process is 2,2',5,5'-tetrachlorobenzidine, the synthesis of benzidine yellow organic pigments generates a large amount of organic wastewater containing 2,2',5,5'-tetrachlorobenzidine. 2,2',5,5'-tetrachlorobenzidine is an organic compound of benzidine with chlorine substitution at the 2,2',5,5' position. It exhibits high chemical stability and carcinogenic toxicity, is easily accumulated, and is difficult to degrade and treat, posing a serious threat to the Earth's ecological environment.

[0003] Current technologies for treating organic wastewater containing 2,2',5,5'-tetrachlorobenzidine include physical treatment processes such as adsorption and membrane exchange adsorption, as well as chemical processes involving oxidation and decomposition. Physical treatment processes like adsorption and membrane treatment only transfer 2,2',5,5'-tetrachlorobenzidine; they do not decompose it into harmless substances, thus causing secondary pollution. Meanwhile, the effectiveness of oxidation and degradation chemical processes for treating organic wastewater containing 2,2',5,5'-tetrachlorobenzidine is currently unsatisfactory.

[0004] Alternating magnetic fields can induce a significant magnetocaloric effect in superparamagnetic materials, which can significantly promote the kinetic rate of chemical reactions. This invention synergizes the magnetocaloric effect of superparamagnetic materials with the oxidative degradation chemical reaction process of 2,2',5,5'-tetrachlorobenzidine, which has played an important role in promoting the treatment technology of 2,2',5,5'-tetrachlorobenzidine organic wastewater. Summary of the Invention

[0005] To overcome the shortcomings of the prior art, the present invention provides a method for preparing wastewater oxidation treatment materials based on the magnetocaloric effect. The oxidation treatment materials prepared by this method have excellent degradation rate of 2,2',5,5' tetrachlorobenzidine and excellent reusability.

[0006] The technical solution adopted by this invention to solve its technical problem is:

[0007] This invention provides a method for preparing a wastewater oxidation treatment material based on the magnetocaloric effect, comprising the following steps performed in sequence:

[0008] Step [1]: A layer of trimethylamine iron oxide Fe(C3H9NO)3 organic compound is formed on the surface of the copper foam substrate;

[0009] Step [2] converts the trimethylamine oxide iron Fe(C3H9NO)3 organic compound layer into a maleamide / trimethylamine oxide iron Fe(C4H3NO2)2(C3H9NO) organic compound layer by substitution with maleimide group C4H3NO2;

[0010] Step [3] loads manganese magnesium gadolinium oxide Mn 1-x Mg x Gd2O4 (0 < x ≤ 0.3) nanocrystals on the maleamide / trimethylamine oxide iron Fe(C4H3NO2)2(C3H9NO) organic compound layer to obtain the sewage oxidation treatment material.

[0011] Preferably, the step [1] specifically includes the following operations:

[0012] a1. Add carbonyl iron powder, ferric chloride, diethylamine and acetic acid to deionized water and mix to form a base solution; add methyl formate to methanol and mix to form an additive solution; add a certain amount of the additive solution to the base solution and mix to form a synthesis solution;

[0013] a2. Immerse the copper foam sample in the synthesis solution, heat to 60 - 90 °C, and react for 4 - 6 hours to obtain copper foam with a trimethylamine oxide iron Fe(C3H9NO)3 organic compound layer formed on its surface, denoted as intermediate A.

[0014] Preferably, in step a1, the concentration of carbonyl iron powder in the base solution is 160 g / L - 220 g / L, the concentration of ferric chloride is 50 g / L - 90 g / L, the concentration of diethylamine is 90 mL / L - 160 mL / L, and the concentration of acetic acid is 90 mL / L - 140 mL / L; the concentration of methyl formate in the additive solution is 110 mL / L - 130 mL / L; the volume ratio of the additive solution to the base solution in the synthesis solution is 1 - 3:3 - 5.

[0015] Preferably, in step a2, the weight of copper foam immersed in each liter of the synthesis solution is 260 - 290 g.

[0016] Preferably, the step [2] specifically includes the following operations:

[0017] b1. Add N - methylaniline and phenylhydrazine to ethanol and mix to form a first intermediate solution; add glyoxal and potassium permanganate to deionized water and mix to form a second intermediate solution; add a certain amount of the second intermediate solution to the first intermediate solution and mix to form a substitution solution;

[0018] b2. Immerse intermediate A in the substitute solution and react at room temperature for 1.5-3 hours to obtain copper foam with a layer of maleamide / trimethylammonium oxide Fe(C4H3NO2)2(C3H9NO) organic compound formed on the surface, denoted as intermediate B.

[0019] Preferably, in step b1, the concentration of N-methylaniline in the first intermediate solution is 160 mL / L-190 mL / L, and the concentration of phenylhydrazine is 210 mL / L-240 mL / L; the concentration of glyoxal in the second intermediate solution is 150 g / L-210 g / L, and the concentration of potassium permanganate is 40 g / L-70 g / L; the volume ratio between the first intermediate solution and the second intermediate solution in the substitute solution is 3-7:1-2.

[0020] Preferably, in step b2, the weight of intermediate A immersed in each liter of the substitute liquid is 270-310g.

[0021] Preferably, step [3] specifically includes the following operations:

[0022] c1. Add magnesium chloride, manganese nitrate, gadolinium nitrate, allyl alcohol and 2-hydroxysuccinic acid to deionized water to form an intermediate product forming solution. Immerse intermediate B in the intermediate product forming solution and place it in a microwave reactor. Microwave heat to 90℃-140℃ at a rate of 10-30℃ / min and react for 0.5-2 hours to load manganese magnesium gadolinium oxide intermediate on the maleamide / trimethylammonium trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer on the surface of the copper foam substrate to finally obtain intermediate C.

[0023] c2. The intermediate C is placed in a low-temperature box furnace and kept at 150℃-300℃ for 3-5 hours to convert the manganese magnesium gadolinium oxide intermediate into manganese magnesium gadolinium oxide nanocrystals, and finally obtain the wastewater oxidation treatment material.

[0024] Preferably, the concentration of magnesium chloride in the intermediate product forming solution in step c1 is 40 g / L-60 g / L, the concentration of manganese nitrate is 120 g / L-170 g / L, the concentration of gadolinium nitrate is 230 g / L-270 g / L, the concentration of allyl alcohol is 60 mL / L-90 mL / L, and the concentration of 2-hydroxysuccinic acid is 110 g / L-150 g / L.

[0025] Preferably, the weight of intermediate B immersed in each liter of the intermediate product forming liquid in step c1 is 220-270g.

[0026] The positive effects of this invention: The wastewater oxidation treatment material (foamed copper-based maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic matter supported manganese magnesium gadolinium oxide Mn) prepared according to the method described in this invention1-x Mg x Gd2O4 nanocrystals), and its structural characteristics are as follows: The Fe(C4H3NO2)2(C3H9NO) structure is an organic compound in which iron ions are the central ions and form a planar triangular structure with trimethylamine oxide C3H9NO and maleimide C4H3NO2. The structure of Fe(C4H3NO2)2(C3H9NO) is as shown in Figure 3 shown, with the iron ion located at the centroid of the planar triangle and the trimethylamine oxide C3H9NO and maleimide C4H3NO2 ligands located at the vertices of the planar triangle; Mn 1-x Mg x Gd2O4(0 < x ≤ 0.3) nanocrystals have a spinel structure (the structure is as shown in Figure 4 shown), with oxygen ions arranged in a cubic close-packed manner, gadolinium ions located in octahedral voids, and manganese ions and magnesium ions located in tetrahedral voids. Based on the above structural characteristics, among them, iron maleamide / trimethylamine oxide Fe(C4H3NO2)2(C3H9NO) has superparamagnetism. Under the action of an alternating magnetic field, due to Brown relaxation and Neel relaxation, a magnetothermal effect is generated. This magnetothermal effect is concentrated locally and is closely related to the iron ions of iron maleamide / trimethylamine oxide Fe(C4H3NO2)2(C3H9NO), which can cause the temperature of the Mn 1- x Mg x Gd2O4 nanocrystals to increase significantly, oxidize the divalent manganese ions of the Mn 1-x Mg x Gd2O4 nanocrystals to form tetravalent manganese ions. The tetravalent manganese ions undergo an electrophilic reaction with the aromatic ring of 2,2',5,5'-tetrachlorobenzidine and break, causing the degradation of 2,2',5,5'-tetrachlorobenzidine; in addition, the alternating magnetic field thermal effect of Fe(C4H3NO2)2(C3H9NO) also reduces the stability of the bond between the atoms of 2,2',5,5'-tetrachlorobenzidine adsorbed on the copper foam-based treatment material, further promoting the degradation of 2,2',5,5'-tetrachlorobenzidine.

[0027] In summary, the sewage oxidation treatment material prepared according to the present invention has excellent 2,2',5,5'-tetrachlorobenzidine degradation rate and excellent reusability stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a schematic diagram of the preparation process of the sewage oxidation treatment material described in the present invention;

[0029] Figure 2 is a schematic diagram of the structure of Fe(C3H9NO)3 described in the present invention;

[0030] Figure 3It is the structural schematic diagram of Fe(C4H3NO2)2(C3H9NO) described in the present invention;

[0031] Figure 4 is Mn described in the present invention 1-x Mg x It is the structural schematic diagram of Gd2O4(0<x≤0.3) described in the present invention;

[0032] Figure 5a It is the removal rate of 2,2',5,5'-tetrachlorobenzidine under different pH conditions when an alternating magnetic field is applied in Example 1, Comparative Example 1, and Comparative Example 2 of the present invention;

[0033] Figure 5b It is the removal rate of 2,2',5,5'-tetrachlorobenzidine under different pH conditions without an applied magnetic field in Example 1, Comparative Example 1, and Comparative Example 2 of the present invention;

[0034] Figure 6a It is the removal rate of 2,2',5,5'-tetrachlorobenzidine when reused for the 5th time under different pH conditions when an alternating magnetic field is applied in Example 1, Comparative Example 1, and Comparative Example 2 of the present invention;

[0035] Figure 6b It is the removal rate of 2,2',5,5'-tetrachlorobenzidine when reused for the 5th time under different pH conditions without an applied magnetic field in Example 1, Comparative Example 1, and Comparative Example 2 of the present invention. Specific embodiments

[0036] Refer to Figure 1 , the present invention provides a preparation method of a sewage oxidation treatment material based on the magnetothermal effect, comprising the following steps carried out in sequence:

[0037] Step [1] Form an organic compound layer of trimethylamine iron oxide Fe(C3H9NO)3 on the surface of the copper foam substrate, specifically including the following operations:

[0038] a1. Add carbonyl iron powder, ferric chloride, diethylamine, and acetic acid to deionized water, and mix to form a base solution with a carbonyl iron powder concentration of 160 g / L - 220 g / L, a ferric chloride concentration of 50 g / L - 90 g / L, a diethylamine concentration of 90 mL / L - 160 mL / L, and an acetic acid concentration of 90 mL / L - 140 mL / L; add methyl formate to methanol, and mix to form an additive solution with a methyl formate concentration of 110 mL / L - 130 mL / L; add the additive solution to the base solution in a volume ratio of 1 - 3:3 - 5, and mix to form a synthesis solution;

[0039] a2. Immerse the copper foam sample in the synthetic liquid (the weight of the copper foam immersed in each liter of the synthetic liquid is 260 - 290 g), heat it to 60 - 90 °C, and react for 4 - 6 hours to obtain copper foam with an organic compound layer of trimethylamine iron oxide Fe(C3H9NO)3 (the structure is as shown in Figure 2 ), which is denoted as intermediate A.

[0040] Step [2] converts the organic compound layer of trimethylamine iron oxide Fe(C3H9NO)3 into an organic compound layer of maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) by substituting the maleimide group C4H3NO2. The specific operations are as follows:

[0041] b1. Add N-methylaniline and phenylhydrazine to ethanol to form a first intermediate liquid with an N-methylaniline concentration of 160 mL / L - 190 mL / L and a phenylhydrazine concentration of 210 mL / L - 240 mL / L; add glyoxal and potassium permanganate to deionized water to form a second intermediate liquid with a glyoxal concentration of 150 g / L - 210 g / L and a potassium permanganate concentration of 40 g / L - 70 g / L; add the second intermediate liquid to the first intermediate liquid according to a volume ratio of 3 - 7:1 - 2 between the first intermediate liquid and the second intermediate liquid to form a substitution liquid;

[0042] b2. Immerse intermediate A in the substitution liquid (the weight of intermediate A immersed in each liter of the substitution liquid is 270 - 310 g), and react at room temperature for 1.5 - 3 hours to obtain copper foam with an organic compound layer of maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO), which is denoted as intermediate B.

[0043] Step [3] Load manganese magnesium gadolinium oxide Mn 1-x Mg x Gd2O4 (0 < x ≤ 0.3) nanocrystals on the organic compound layer of maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO). The specific operations are as follows:

[0044] c1. Magnesium chloride, manganese nitrate, gadolinium nitrate, allyl alcohol, and 2-hydroxysuccinic acid are added to deionized water to form an intermediate product forming solution with magnesium chloride concentration of 40 g / L-60 g / L, manganese nitrate concentration of 120 g / L-170 g / L, gadolinium nitrate concentration of 230 g / L-270 g / L, allyl alcohol concentration of 60 mL / L-90 mL / L, and 2-hydroxysuccinic acid concentration of 110 g / L-150 g / L. Intermediate B is then immersed in this intermediate product forming solution. The intermediate product is placed in a microwave reactor and heated to 90°C-140°C at a rate of 10-30°C / min for 0.5-2 hours. This process loads the intermediate product, manganese magnesium gadolinium oxide, onto the maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer on the surface of the copper foam matrix, thus finally obtaining intermediate product C.

[0045] c2. The intermediate C is placed in a low-temperature box furnace and kept at 150℃-300℃ for 3-5 hours to convert the manganese magnesium gadolinium oxide intermediate into manganese magnesium gadolinium oxide nanocrystals, ultimately obtaining the wastewater oxidation treatment material (foamed copper-based maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic matter-supported manganese magnesium gadolinium oxide Mn). 1-x Mg x Gd2O4 nanocrystals).

[0046] The preferred embodiments of the present invention will be described below by way of example.

[0047] Example 1

[0048] Preferred embodiment 1 of the present invention provides a method for preparing a wastewater oxidation treatment material based on the magnetocaloric effect, comprising the following steps performed in sequence:

[0049] Step [1] involves forming a layer of ferric trimethylamine oxide (Fe(C3H9NO)3) organic compound on the surface of a copper foam substrate, specifically including the following operations:

[0050] a1. Carbonyl iron powder, ferric chloride, diethylamine, and acetic acid are added to deionized water and mixed to form a base solution with a carbonyl iron powder concentration of 190 g / L, a ferric chloride concentration of 70 g / L, a diethylamine concentration of 150 mL / L, and an acetic acid concentration of 120 mL / L; methyl formate is added to methanol and mixed to form an additive solution with a methyl formate concentration of 120 mL / L; the additive solution is added to the base solution at a volume ratio of 2:5 and mixed to form a synthesis solution;

[0051] a2. Immerse the copper foam sample in the synthetic liquid (the weight of the copper foam immersed in each liter of the synthetic liquid is 280 g), heat it to 80 °C, and react for 5 hours to obtain copper foam with an iron trimethylamine oxide Fe(C3H9NO)3 organic compound layer formed on its surface, denoted as intermediate A.

[0052] Step [2] converts the iron trimethylamine oxide Fe(C3H9NO)3 organic compound layer into an N - maleoyl / iron trimethylamine oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer through the substitution of maleimide groups C4H3NO2, specifically including the following operations:

[0053] b1. Add N - methylaniline and phenylhydrazine to ethanol to form a first intermediate liquid with an N - methylaniline concentration of 180 mL / L and a phenylhydrazine concentration of 230 mL / L; add glyoxal and potassium permanganate to deionized water to form a second intermediate liquid with a glyoxal concentration of 200 g / L and a potassium permanganate concentration of 60 g / L; add the second intermediate liquid to the first intermediate liquid according to a volume ratio of 5:2 between the first intermediate liquid and the second intermediate liquid to form a substitution liquid;

[0054] b2. Immerse intermediate A in the substitution liquid (the weight of intermediate A immersed in each liter of the substitution liquid is 300 g), react at room temperature for 3 hours to obtain copper foam with an N - maleoyl / iron trimethylamine oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer formed on its surface, denoted as intermediate B.

[0055] Step [3] loads manganese - magnesium - gadolinium oxide Mn 1-x Mg x Gd2O4 (0 < x ≤ 0.3) nanocrystals on the N - maleoyl / iron trimethylamine oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer, specifically including the following operations:

[0056] c1. Add magnesium chloride, manganese nitrate, gadolinium nitrate, allyl alcohol, and 2 - hydroxybutyric acid to deionized water to form an intermediate product formation liquid with a magnesium chloride concentration of 50 g / L, a manganese nitrate concentration of 160 g / L, a gadolinium nitrate concentration of 260 g / L, an allyl alcohol concentration of 80 mL / L, and a 2 - hydroxybutyric acid concentration of 140 g / L. Immerse intermediate B in the intermediate product formation liquid (the weight of intermediate B immersed in each liter of the intermediate product formation liquid is 260 g), put it into a microwave reactor, and microwave - heat it to 130 °C at a rate of 25 °C / min and react for 1.5 hours to load the manganese - magnesium - gadolinium oxide intermediate product on the N - maleoyl / iron trimethylamine oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer on the copper foam matrix surface, and finally obtain intermediate C;

[0057] c2. The intermediate C is placed in a low-temperature box furnace and kept at 260°C for 4 hours to convert the manganese magnesium gadolinium oxide intermediate into manganese magnesium gadolinium oxide nanocrystals, ultimately obtaining the wastewater oxidation treatment material (foamed copper-based maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic matter-supported manganese magnesium gadolinium oxide Mn). 1-x Mg x Gd2O4 nanocrystals, referred to as Example 1.

[0058] Comparative Example 1

[0059] Comparative Example 1 provides a method for preparing a wastewater treatment material, comprising the following steps performed in sequence:

[0060] Step [1] involves forming a layer of ferric trimethylamine oxide (Fe(C3H9NO)3) organic compound on the surface of a copper foam substrate, specifically including the following operations:

[0061] a1. Add carbonyl iron powder, ferric chloride, diethylamine, and acetic acid to deionized water to form a base solution with a carbonyl iron powder concentration of 170 g / L, a ferric chloride concentration of 60 g / L, a diethylamine concentration of 100 mL / L, and an acetic acid concentration of 100 mL / L; add methyl formate to methanol to form an additive solution with a methyl formate concentration of 115 mL / L; add the additive solution to the base solution at a volume ratio of 1:3 and mix to form a synthesis solution;

[0062] a2. Immerse the copper foam sample in the synthesis solution (the weight of the copper foam immersed in each liter of the synthesis solution is 270g), heat to 70°C, and react for 5 hours to obtain copper foam with a layer of trimethylamine iron Fe(C3H9NO)3 organic compound formed on the surface, which is denoted as intermediate A.

[0063] Step [2] involves replacing the maleimide group C4H3NO2 to convert the Fe(C3H9NO)3 organic compound layer of maleamide / Fe(C4H3NO2)2(C3H9NO) organic compound layer, specifically including the following operations:

[0064] b1. N-methylaniline and phenylhydrazine are added to ethanol and mixed to form a first intermediate solution with an N-methylaniline concentration of 180 mL / L and a phenylhydrazine concentration of 220 mL / L; glyoxal and potassium permanganate are added to deionized water and mixed to form a second intermediate solution with an glyoxal concentration of 160 g / L and a potassium permanganate concentration of 50 g / L; the second intermediate solution is added to the first intermediate solution at a volume ratio of 3:2 to form a substitute solution;

[0065] b2. Immerse intermediate A in the substitution liquid (the weight of intermediate A immersed in each liter of the substitution liquid is 280 g), react at room temperature for 2 hours to obtain copper foam with an organic compound layer of maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) formed on the surface, denoted as Comparative Example 1.

[0066] Comparative Example 2

[0067] This Comparative Example 2 provides a preparation method of a sewage treatment material, comprising the following steps carried out in sequence:

[0068] Step [1] Form an organic compound layer of trimethylamine iron oxide Fe(C3H9NO)3 on the surface of the copper foam substrate, specifically including the following operations:

[0069] a1. Add carbonyl iron powder, ferric chloride, diethylamine and acetic acid to deionized water, and mix to form a base liquid with a carbonyl iron powder concentration of 20 g / L, a ferric chloride concentration of 60 g / L, a diethylamine concentration of 140 mL / L, and an acetic acid concentration of 130 mL / L; add methyl formate to methanol, and mix to form an additive liquid with a methyl formate concentration of 120 mL / L; add the additive liquid to the base liquid in a volume ratio of 3:5, and mix to form a synthetic liquid;

[0070] a2. Immerse the copper foam sample in the synthetic liquid (the weight of the copper foam immersed in each liter of the synthetic liquid is 280 g), heat to 80 °C, and react for 5 hours to obtain copper foam with an organic compound layer of trimethylamine iron oxide Fe(C3H9NO)3 formed on the surface, denoted as intermediate A.

[0071] Step [2] Load manganese-magnesium-gadolinium oxide Mn 1- x Mg x Gd2O4 (0 < x ≤ 0.3) nanocrystals on the organic compound layer of trimethylamine iron oxide Fe(C3H9NO)3, specifically including the following operations:

[0072] c1. Add magnesium chloride, manganese nitrate, gadolinium nitrate, allyl alcohol and 2-hydroxybutyric acid to deionized water to form an intermediate product formation liquid with a magnesium chloride concentration of 50 g / L, a manganese nitrate concentration of 150 g / L, a gadolinium nitrate concentration of 252 g / L, an allyl alcohol concentration of 80 mL / L, and a 2-hydroxybutyric acid concentration of 130 g / L. Immerse intermediate A in the intermediate product formation liquid (the weight of intermediate A immersed in each liter of the intermediate product formation liquid is 260 g), put it into a microwave reactor, and microwave heat to 130 °C at a rate of 20 °C / min, and react for 1.5 hours to load an intermediate product of manganese-magnesium-gadolinium oxide on the organic compound layer of trimethylamine iron oxide Fe(C3H9NO)3 on the surface of the copper foam substrate, and finally obtain intermediate D;

[0073] c2. The intermediate D is placed in a low-temperature box furnace and kept at 200°C for 4 hours to convert the manganese magnesium gadolinium oxide intermediate into manganese magnesium gadolinium oxide nanocrystals, ultimately obtaining the wastewater treatment material (foamed copper-based trimethylamine iron oxide Fe(C3H9NO)3 organic matter-supported manganese magnesium gadolinium oxide Mn). 1-x Mg x Gd2O4 nanocrystals), denoted as Comparative Example 2.

[0074] To analyze the degradation performance of wastewater containing 2,2',5,5'-tetrachlorobenzidine in Examples 1, 1, and 2, solutions with a 2,2',5,5'-tetrachlorobenzidine concentration of 40 mg / L were prepared using deionized water as simulated wastewater. The pH of the prepared simulated wastewater was adjusted with hydrochloric acid and sodium hydroxide to obtain simulated wastewater with pH values ​​of 4, 5, 6, 7, and 8. 40 g of wastewater treatment material (i.e., Examples 1, 1, and 2) was placed in each liter of simulated wastewater for 2,2',5,5'-tetrachlorobenzidine degradation treatment for 40 min. The treatment conditions were an alternating magnetic field with an applied frequency of 500 kHz and a magnetic field strength of 0.05 T, and no applied magnetic field (0 T), respectively. The concentration of 2,2',5,5'-tetrachlorobenzidine in the corresponding simulated wastewater after degradation treatment was measured using high-performance liquid chromatography (HPLC), and the corresponding degradation rate of 2,2',5,5'-tetrachlorobenzidine was calculated. The results are as follows: Figure 5a -b is shown. Furthermore, to compare and analyze the repeated use stability of Example 1, Comparative Example 1, and Comparative Example 2, the degradation rate of 2,2',5,5'-tetrachlorobenzidine in the corresponding simulated wastewater was studied when Example 1, Comparative Example 1, and Comparative Example 2 were reused for the fifth time under the same conditions. The results are shown in Figure 1. Figure 6a -b is shown.

[0075] The experimental results show that under the action of an alternating magnetic field, the magnetocaloric effect can promote the degradation of 2,2',5,5'-tetrachlorobenzidine in Example 1. Compared with the condition without the alternating magnetic field thermal effect, the degradation performance of wastewater containing 2,2',5,5'-tetrachlorobenzidine is significantly improved by the alternating magnetic field thermal effect oxidation treatment. In contrast, the degradation performance of 2,2',5,5'-tetrachlorobenzidine wastewater in Comparative Examples 1 and 2 is not ideal, whether under the condition with or without the alternating magnetic field. Furthermore, when Example 1 was used for the fifth time, the 2,2',5,5'-tetrachlorobenzidine under the alternating magnetic field thermal effect oxidation treatment condition could still be degraded by more than 83%, while the degradation rate of 2,2',5,5'-tetrachlorobenzidine in Comparative Examples 1 and 2 was significantly reduced when used for the fifth time.

[0076] In summary, the wastewater oxidation treatment material prepared according to the present invention has excellent degradation rate of 2,2',5,5'-tetrachlorobenzidine and excellent stability for repeated use.

[0077] To illustrate this further in detail, three more embodiments are provided below.

[0078] Example 2

[0079] Preferred embodiment 2 of the present invention provides a method for preparing a wastewater oxidation treatment material based on the magnetocaloric effect, comprising the following steps performed in sequence:

[0080] Step [1] involves forming a layer of ferric trimethylamine oxide (Fe(C3H9NO)3) organic compound on the surface of a copper foam substrate, specifically including the following operations:

[0081] a1. Add carbonyl iron powder, ferric chloride, diethylamine, and acetic acid to deionized water to form a base solution with a carbonyl iron powder concentration of 160 g / L, a ferric chloride concentration of 50 g / L, a diethylamine concentration of 90 mL / L, and an acetic acid concentration of 90 mL / L; add methyl formate to methanol to form an additive solution with a methyl formate concentration of 130 mL / L; add the additive solution to the base solution at a volume ratio of 1:3 and mix to form a synthesis solution;

[0082] a2. Immerse the copper foam sample in the synthesis solution (the weight of the copper foam immersed in each liter of the synthesis solution is 260g), heat to 60°C, and react for 6 hours to obtain copper foam with a layer of trimethylamine iron Fe(C3H9NO)3 organic compound formed on the surface, which is denoted as intermediate A.

[0083] Step [2] involves replacing the maleimide group C4H3NO2 to convert the Fe(C3H9NO)3 organic compound layer of maleamide / Fe(C4H3NO2)2(C3H9NO) organic compound layer, specifically including the following operations:

[0084] b1. N-methylaniline and phenylhydrazine are added to ethanol and mixed to form a first intermediate solution with an N-methylaniline concentration of 190 mL / L and a phenylhydrazine concentration of 210 mL / L; glyoxal and potassium permanganate are added to deionized water and mixed to form a second intermediate solution with an glyoxal concentration of 210 g / L and a potassium permanganate concentration of 40 g / L; the second intermediate solution is added to the first intermediate solution at a volume ratio of 7:2 to form a substitute solution;

[0085] b2. Immerse the intermediate A in the replacement liquid (the weight of the intermediate A immersed in each liter of the replacement liquid is 270 g), react at room temperature for 1.5 hours to obtain copper foam with an organic compound layer of maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) formed on the surface, denoted as intermediate B.

[0086] Step [3] Load manganese magnesium gadolinium oxide Mn 1-x Mg x Gd2O4 (0 < x ≤ 0.3) nanocrystals, specifically including the following operations:

[0087] c1. Add magnesium chloride, manganese nitrate, gadolinium nitrate, allyl alcohol and 2-hydroxybutyric acid to deionized water to form an intermediate product forming solution with a magnesium chloride concentration of 40 g / L, a manganese nitrate concentration of 120 g / L, a gadolinium nitrate concentration of 270 g / L, an allyl alcohol concentration of 60 mL / L, and a 2-hydroxybutyric acid concentration of 150 g / L. Immerse the intermediate B in the intermediate product forming solution (the weight of the intermediate B immersed in each liter of the intermediate product forming solution is 220 g), place it in a microwave reactor, microwave heat it to 90 °C at a rate of 10 °C / min, and react for 2 hours to load the intermediate product of manganese magnesium gadolinium oxide on the organic compound layer of maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) on the surface of the copper foam matrix, and finally obtain intermediate C;

[0088] c2. Place the intermediate C in a low-temperature box furnace and keep it at 300 °C for 3 hours to convert the intermediate product of manganese magnesium gadolinium oxide into manganese magnesium gadolinium oxide nanocrystals, and finally obtain the sewage oxidation treatment material (copper foam-based maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic matter loaded with manganese magnesium gadolinium oxide Mn 1-x Mg x Gd2O4 nanocrystals).

[0089] Example 3

[0090] The preferred embodiment 3 of the present invention provides a preparation method of a sewage oxidation treatment material based on the magnetothermal effect, including the following steps carried out in sequence:

[0091] Step [1] Form an organic compound layer of trimethylamine iron oxide Fe(C3H9NO)3 on the surface of the copper foam matrix, specifically including the following operations:

[0092] a1. Add carbonyl iron powder, ferric chloride, diethylamine and acetic acid to deionized water, and mix to form a base solution with a carbonyl iron powder concentration of 220 g / L, a ferric chloride concentration of 90 g / L, a diethylamine concentration of 160 mL / L, and an acetic acid concentration of 140 mL / L; add methyl formate to methanol, and mix to form an additive solution with a methyl formate concentration of 110 mL / L; add the additive solution to the base solution in a volume ratio of 3:5, and mix to form a synthesis solution.

[0093] a2. Immerse the copper foam sample in the synthesis solution (the weight of copper foam immersed in each liter of the synthesis solution is 290 g), heat to 90 °C, and react for 4 hours to obtain copper foam with a layer of trimethylamine iron oxide Fe(C3H9NO)3 organic compound formed on the surface, denoted as intermediate A.

[0094] Step [2] converts the trimethylamine iron oxide Fe(C3H9NO)3 organic compound layer into a maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer by substitution of the maleimide group C4H3NO2, and the specific operations are as follows:

[0095] b1. Add N-methylaniline and phenylhydrazine to ethanol, and mix to form a first intermediate solution with a N-methylaniline concentration of 160 mL / L and a phenylhydrazine concentration of 240 mL / L; add glyoxal and potassium permanganate to deionized water, and mix to form a second intermediate solution with a glyoxal concentration of 150 g / L and a potassium permanganate concentration of 70 g / L; add the second intermediate solution to the first intermediate solution in a volume ratio of 3:1 between the first intermediate solution and the second intermediate solution, and mix to form a substitution solution.

[0096] b2. Immerse intermediate A in the substitution solution (the weight of intermediate A immersed in each liter of the substitution solution is 310 g), and react at room temperature for 3 hours to obtain copper foam with a layer of maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound formed on the surface, denoted as intermediate B.

[0097] Step [3] Load manganese magnesium gadolinium oxide Mn 1-x Mg x Gd2O (0 <x ≤ 0.3) nanocrystals, and the specific operations are as follows:

[0098] c1. Magnesium chloride, manganese nitrate, gadolinium nitrate, allyl alcohol, and 2-hydroxysuccinic acid are added to deionized water to form an intermediate product forming solution with a magnesium chloride concentration of 60 g / L, a manganese nitrate concentration of 170 g / L, a gadolinium nitrate concentration of 230 g / L, an allyl alcohol concentration of 90 mL / L, and a 2-hydroxysuccinic acid concentration of 110 g / L. Intermediate B is immersed in the intermediate product forming solution (the weight of intermediate B immersed in each liter of the intermediate product forming solution is 270 g), placed in a microwave reactor, and microwave heated to 140°C at a rate of 30°C / min for 0.5 hours to obtain manganese magnesium gadolinium oxide intermediate product loaded on the maleamide / trimethylammonium trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer on the surface of the copper foam substrate, finally obtaining intermediate C;

[0099] c2. The intermediate C is placed in a low-temperature box furnace and kept at 150°C for 5 hours to convert the manganese magnesium gadolinium oxide intermediate into manganese magnesium gadolinium oxide nanocrystals, ultimately obtaining the wastewater oxidation treatment material (foamed copper-based maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic matter-supported manganese magnesium gadolinium oxide Mn). 1-x Mg x Gd2O4 nanocrystals).

[0100] Example 4

[0101] Preferred embodiment 4 of the present invention provides a method for preparing a wastewater oxidation treatment material based on the magnetocaloric effect, comprising the following steps performed in sequence:

[0102] Step [1] involves forming a layer of ferric trimethylamine oxide (Fe(C3H9NO)3) organic compound on the surface of a copper foam substrate, specifically including the following operations:

[0103] a1. Carbonyl iron powder, ferric chloride, diethylamine, and acetic acid are added to deionized water and mixed to form a base solution with a carbonyl iron powder concentration of 190 g / L, a ferric chloride concentration of 70 g / L, a diethylamine concentration of 126 mL / L, and an acetic acid concentration of 115 mL / L; methyl formate is added to methanol and mixed to form an additive solution with a methyl formate concentration of 120 mL / L; the additive solution is added to the base solution at a volume ratio of 2:4 and mixed to form a synthesis solution;

[0104] a2. Immerse the copper foam sample in the synthesis solution (the weight of the copper foam immersed in each liter of the synthesis solution is 275g), heat to 69°C, and react for 5 hours to obtain copper foam with a layer of trimethylamine iron Fe(C3H9NO)3 organic compound formed on the surface, which is denoted as intermediate A.

[0105] Step [2] converts the trimethylamine iron oxide Fe(C3H9NO)3 organic compound layer into a maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer through the substitution of maleimide group C4H3NO2. The specific operations are as follows:

[0106] b1. Add N-methylaniline and phenylhydrazine to ethanol to form a first intermediate solution with an N-methylaniline concentration of 175 mL / L and a phenylhydrazine concentration of 225 mL / L. Add glyoxal and potassium permanganate to deionized water to form a second intermediate solution with a glyoxal concentration of 190 g / L and a potassium permanganate concentration of 55 g / L. Add the second intermediate solution to the first intermediate solution according to a volume ratio of 5:2 between the first intermediate solution and the second intermediate solution to form a substitution solution.

[0107] b2. Immerse intermediate A in the substitution solution (the weight of intermediate A immersed in each liter of the substitution solution is 290 g), and react at room temperature for 2 hours to obtain copper foam with a maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer formed on its surface, denoted as intermediate B.

[0108] Step [3] loads manganese magnesium gadolinium oxide Mn 1-x Mg x Gd2O4 (0 < x ≤ 0.3) nanocrystals. The specific operations are as follows:

[0109] c1. Add magnesium chloride, manganese nitrate, gadolinium nitrate, allyl alcohol and 2-hydroxybutyric acid to deionized water to form an intermediate product forming solution with a magnesium chloride concentration of 50 g / L, a manganese nitrate concentration of 145 g / L, a gadolinium nitrate concentration of 246 g / L, an allyl alcohol concentration of 75 mL / L, and a 2-hydroxybutyric acid concentration of 130 g / L. Immerse intermediate B in the intermediate product forming solution (the weight of intermediate B immersed in each liter of the intermediate product forming solution is 245 g), place it in a microwave reactor, and microwave heat it to 120 °C at a rate of 20 °C / min and react for 1.2 hours to load the manganese magnesium gadolinium oxide intermediate product on the maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer on the copper foam matrix, and finally obtain intermediate C.

[0110] c2. Place intermediate C in a low-temperature box furnace and keep it at 210 °C for 4 hours to convert the manganese magnesium gadolinium oxide intermediate product into manganese magnesium gadolinium oxide nanocrystals, and finally obtain the sewage oxidation treatment material (copper foam-based maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic matter loaded with manganese magnesium gadolinium oxide Mn1-x Mg x Gd2O4 nanocrystals).

[0111] The above description is only a preferred embodiment of the present invention. It should be understood that the above description of the embodiments is only for the purpose of helping to understand the method and core idea of ​​the present invention, and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, etc. made within the idea and principle of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a sewage oxidation treatment material based on magnetocaloric effect, characterized in that: It contains the following steps in order: Step [1] forming an organic compound layer of trimethylamine iron oxide Fe(C3H9NO)3 on the surface of the copper foam substrate; Step [2] converting the trimethylamine iron oxide Fe(C3H9NO)3 organic compound layer into a maleimide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer by replacing the maleimide group C4H3NO2; Step [3] Load manganese-magnesium-gadolinium oxide Mn 1-x Mg x Gd2O4 (0 < x ≤ 0.3) nanocrystals on the maleamide / trimethylamine oxide iron Fe(C4H3NO2)2(C3H9NO) organic compound layer to obtain the sewage oxidation treatment material.

2. The method for preparing a sewage oxidation treatment material based on magnetocaloric effect according to claim 1, characterized in that: The step [1] specifically includes the following operations: a1. Add carbonyl iron powder, ferric chloride, diethylamine and acetic acid to deionized water and mix to form a base liquid; add methyl formate to methanol and mix to form an additive liquid; add a certain amount of the additive liquid to the base liquid and mix to form a synthetic liquid; a2. Immerse the copper foam sample in the synthetic solution, heat to 60-90°C, react for 4-6 hours, and obtain a copper foam having an organic compound layer of trimethylamine iron oxide Fe(C3H9NO)3 formed on the surface, which is recorded as intermediate A.

3. The method for preparing a sewage oxidation treatment material based on magnetocaloric effect according to claim 2, characterized in that: In step a1, the concentration of carbonyl iron powder in the base liquid is 160g / L-220g / L, the concentration of ferric chloride is 50g / L-90g / L, the concentration of diethylamine is 90mL / L-160mL / L, and the concentration of acetic acid is 90mL / L-140mL / L; the concentration of methyl formate in the additive liquid is 110mL / L-130mL / L; and the volume ratio between the additive liquid and the base liquid in the synthetic liquid is 1-3:3-5.

4. The method for preparing a sewage oxidation treatment material based on magnetocaloric effect according to claim 2, characterized in that: In step a2, the weight of the foamed copper immersed in each liter of the synthetic solution is 260-290 g.

5. The method for preparing a sewage oxidation treatment material based on magnetocaloric effect according to claim 1, characterized in that: The step [2] specifically includes the following operations: b1. N-methylaniline and phenylhydrazine are added to ethanol and mixed to form a first intermediate solution; glyoxal and potassium permanganate are added to deionized water and mixed to form a second intermediate solution; a certain amount of the second intermediate solution is added to the first intermediate solution and mixed to form a replacement solution; b2. Immerse the intermediate A in the replacement solution and react at room temperature for 1.5-3 hours to obtain a copper foam having a maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer formed on the surface, which is recorded as intermediate B.

6. The method for preparing a sewage oxidation treatment material based on magnetocaloric effect according to claim 5, characterized in that: In step b1, the concentration of N-methylaniline in the first intermediate solution is 160mL / L-190mL / L, and the concentration of phenylhydrazine is 210mL / L-240mL / L; the concentration of glyoxal in the second intermediate solution is 150g / L-210g / L, and the concentration of potassium permanganate is 40g / L-70g / L; the volume ratio between the first intermediate solution and the second intermediate solution in the replacement solution is 3-7:1-2.

7. The method for preparing a sewage oxidation treatment material based on magnetocaloric effect according to claim 5, characterized in that: In step b2, the weight of the intermediate A immersed in each liter of the replacement liquid is 270-310 g.

8. The method for preparing a sewage oxidation treatment material based on magnetocaloric effect according to claim 1, characterized in that: The step [3] specifically includes the following operations: c1. Magnesium chloride, manganese nitrate, gadolinium nitrate, allyl alcohol and 2-hydroxysuccinic acid are added to deionized water to form an intermediate product forming liquid, intermediate B is immersed in the intermediate product forming liquid, placed in a microwave reactor, and microwave-heated to 90°C-140°C at a rate of 10-30°C / min, and reacted for 0.5-2 hours to load manganese magnesium gadolinium oxide intermediate product on the maleamide / trimethylamine iron oxide Fe(C4H3NO2)2(C3H9NO) organic compound layer on the surface of the foam copper substrate, and finally obtain intermediate C; c2. placing the intermediate C into a low-temperature box furnace and keeping it at 150°C-300°C for 3 to 5 hours to convert the manganese magnesium gadolinium oxide intermediate into manganese magnesium gadolinium oxide nanocrystals, and finally obtaining the sewage oxidation treatment material.

9. The method for preparing a sewage oxidation treatment material based on magnetocaloric effect according to claim 8, characterized in that: In step c1, the magnesium chloride concentration of the intermediate product forming liquid is 40g / L-60g / L, the manganese nitrate concentration is 120g / L-170g / L, the gadolinium nitrate concentration is 230g / L-270g / L, the allyl alcohol concentration is 60mL / L-90mL / L, and the 2-hydroxysuccinic acid concentration is 110g / L-150g / L.

10. The method for preparing a sewage oxidation treatment material based on magnetocaloric effect according to claim 8, characterized in that: In step c1, the weight of the intermediate B immersed in each liter of the intermediate product forming liquid is 220-270 g.

Citation Information

Patent Citations

  • Preparation method and application of alternating magnetic field-oriented auxiliary photo-Fenton catalyst

    CN116726943A

  • Method for producing oxide-based metal-organic framework materials by inserting oxides while controlling water content

    WO2011069541A1

  • Method for strengthening biogenic manganese oxidation by using magnetic field, and application thereof

    WO2022188834A1

Cited By

  • Preparation method of composite material for ozone photocatalysis cooperative treatment of unsymmetrical dimethylhydrazine sewage

    CN119702079A

  • Preparation method of composite material for ozone photocatalytic synergistic treatment of unsymmetrical dimethylhydrazine wastewater