Low-temperature sealing glass powder material with self-repairing function
By introducing shape memory alloy fibers, microcapsule repair agents and nanoreinforced materials into the low-temperature sealing glass powder material, the problem of easy damage of existing low-temperature sealing materials is solved, and self-repairing ability and excellent sealing under low-temperature conditions are achieved Connection performance, suitable for electronic packaging and optical component manufacturing and other fields.
Patent Information
- Application Number
- CN202410856880.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-05
AI Technical Summary
During use, existing low-temperature sealing glass powder materials are prone to microcracks or damage due to external environment or mechanical stress, resulting in sealing failure. Traditional high-temperature sealing technology consumes a lot of energy and may cause thermal damage to the substrate.
Using low-temperature sealed glass powder material with self-healing function, the formed materials can be repaired by introducing shape memory alloy fibers, microcapsule repair agents and nanoreinforced materials into the glass powder, including nickel-titanium alloy fibers, Microcapsules for polyurea formaldehyde resins and epoxy resin repair agents and nanoreinforced materials for nanosilicon dioxide or nanoalumina.
It realizes the self-healing ability of the material under low temperature conditions, improves the mechanical strength and heat resistance of the seal, extends the service life and reliability of the material, and provides excellent sealing performance and wide application prospects.
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of glass powder, and more particularly to a low-temperature sealing glass powder material with self-repairing function. Background Art
[0002] In modern industrial production, glass materials are widely used in electronics, optics, construction and other fields due to their excellent physical and chemical properties. In particular, in electronic packaging technology, glass powder materials, as an important sealing material, play a vital role. Traditional glass powder materials usually need to be sealed under high temperature conditions, which not only consumes a lot of energy, but also easily causes thermal damage to the substrate under high temperature conditions, thus affecting the sealing effect and product quality.
[0003] The emergence of low-temperature sealing technology provides an effective way to solve the above problems. However, the existing low-temperature sealing glass powder materials still have some shortcomings in practical applications. For example, the sealing material may produce microcracks or breakage due to the influence of the external environment or mechanical stress during use, resulting in sealing failure. Summary of the invention
[0004] In order to solve the problems existing in the prior art, a low-temperature sealing glass powder material with self-repairing function is provided. The specific scheme is as follows:
[0005] A low-temperature sealing glass powder material with self-repairing function, the glass powder material comprises the following components: a borosilicate glass composition: SiO2 70-75%, B2O3 15-20%, Na2O 2-5%, Al2O3 1-3%, CaO 1-3%; a microcapsule repairing agent; a nano-reinforced material; and a shape memory alloy fiber.
[0006] Furthermore, the size of the microcapsule repair agent is 10 to 50 μm; the microcapsule repair agent includes polyurea formaldehyde resin and epoxy resin repair agent.
[0007] Furthermore, the nano-reinforcement material is nano-silicon dioxide or nano-aluminum oxide, or a mixture of the two.
[0008] Furthermore, the preparation method of the microcapsule repair agent comprises the following steps:
[0009] S1: Mix the epoxy resin repair agent and the initiator evenly to form a uniform liquid core material;
[0010] S2: under stirring conditions, dropping the core material into the polyurea formaldehyde resin solution to form microcapsules;
[0011] S3: Curing of microcapsules: Curing at 60°C for 2 hours to ensure the shell strength of the microcapsules.
[0012] A method for preparing a low-temperature sealing glass powder material with a self-repairing function comprises the following steps:
[0013] S501: crushing the borosilicate glass block to 100-200 mesh to form a uniform glass powder;
[0014] S502: using an ultrasonic disperser to disperse the nano-reinforced material in the ethanol solution, and then mixing the nano-reinforced material with the glass powder to obtain a mixture A;
[0015] S503: mixing the shape memory alloy fiber into the mixture A obtained in S502 to obtain a mixture B;
[0016] S504: The microcapsule repairing agent is uniformly mixed into the mixture B, and the mixed glass powder material is placed in a drying oven, and dried at 120° C. for 4 hours to obtain the glass powder material.
[0017] Furthermore, the method for using the glass powder material comprises the following steps:
[0018] S601: pre-treating the substrate to be sealed;
[0019] S602: evenly coating the dried glass powder on the contact surface of the substrate;
[0020] S603: placing the substrate coated with glass powder in a sealed furnace and heating at 300-400° C. for 0.5 h;
[0021] S604: gradually cooling the substrate to room temperature.
[0022] Furthermore, the shape memory alloy fiber is a nickel-titanium alloy fiber, the fiber diameter is 5 to 20 μm, the length is 0.1 to 5 mm, and the mass percentage content is 0.5% to 3% of the total mass of the glass powder material.
[0023] Furthermore, the mass percentage content of the nano-reinforced material is 0.1% to 5% of the total mass of the glass powder material.
[0024] Beneficial effects:
[0025] The present invention provides a low-temperature sealing glass powder material with self-repairing function, which specifically includes the following advantages:
[0026] First, by introducing shape memory alloy fibers, microcapsule repair agents and nano-reinforced materials into the glass matrix, the self-repairing ability of the material after damage is achieved. The shape memory alloy fibers can restore their original shape when the temperature changes, thereby closing the cracks; the microcapsule repair agent releases the repair agent when the cracks occur to fill the cracks; the nano-reinforced materials can improve the mechanical strength and heat resistance of the matrix material.
[0027] Among them, the shape memory alloy fiber is made of nickel-titanium alloy fiber, which can respond to temperature changes and self-repair when the material is damaged, greatly improving the service life and reliability of the material.
[0028] In summary, by organically combining shape memory alloy fibers, microcapsule repair agents and nano-reinforced materials, a new type of material with excellent sealing performance and self-repairing ability under low temperature conditions is provided. This material has broad application prospects in electronic packaging, optical component manufacturing and other fields that require low-temperature sealing technology. DETAILED DESCRIPTION
[0029] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0030] Embodiment 1:
[0031] (1) Component preparation:
[0032] Borosilicate glass composition: SiO272%, B2O318%, Na2O 4%, Al2O32%, CaO 2% Microcapsule repair agent: size 20μm, including polyurea formaldehyde resin and epoxy resin repair agent
[0033] Nano-reinforced material: Nano-silicon dioxide, 2% by mass
[0034] Shape memory alloy fiber: NiTi alloy fiber, diameter 10 μm, length 1 mm, mass percentage 1%
[0035] (2) Preparation steps:
[0036] ① Preparation of microcapsule repair agent:
[0037] Mix the epoxy resin repair agent and initiator evenly to form a uniform liquid core material.
[0038] Under stirring conditions, the core material is dropped into the polyurea formaldehyde resin solution to form microcapsules.
[0039] Curing was performed at 60°C for 2 hours to ensure the shell strength of the microcapsules.
[0040] ② Preparation of glass powder materials:
[0041] The borosilicate glass block was crushed to 150 mesh to form a uniform glass powder.
[0042] Nano-silica was dispersed in an ethanol solution using an ultrasonic disperser, and then the nano-reinforcement material was mixed with glass powder to obtain a mixture A.
[0043] The shape memory alloy fiber is mixed into the mixture A to obtain the mixture B.
[0044] The microcapsule repairing agent was uniformly mixed into the mixture B, and the mixed glass powder material was placed in a drying oven and dried at 120° C. for 4 hours to obtain the glass powder material.
[0045] (3) Usage:
[0046] The substrate to be sealed is pretreated.
[0047] The dried glass powder is evenly coated on the contact surface of the substrate.
[0048] The glass powder coated substrate was placed in a sealed furnace and heated at 350°C for 0.5 h.
[0049] The substrate was gradually cooled to room temperature.
[0050] Embodiment 2:
[0051] (1) Component preparation:
[0052] Borosilicate glass composition: SiO273%, B2O317%, Na2O 3%, Al2O33%, CaO 2% Microcapsule repair agent: size 30μm, including polyurea formaldehyde resin and epoxy resin repair agent
[0053] Nano-reinforced material: Nano-alumina, 3% by mass
[0054] Shape memory alloy fiber: NiTi alloy fiber, diameter 15 μm, length 2 mm, mass percentage 2%
[0055] (2) Preparation steps:
[0056] ① Preparation of microcapsule repair agent:
[0057] Mix the epoxy resin repair agent and initiator evenly to form a uniform liquid core material.
[0058] Under stirring conditions, the core material is dropped into the polyurea formaldehyde resin solution to form microcapsules.
[0059] Curing was performed at 60°C for 2 hours to ensure the shell strength of the microcapsules.
[0060] ② Preparation of glass powder materials:
[0061] The borosilicate glass block was crushed to 120 mesh to form a uniform glass powder.
[0062] Nano-alumina was dispersed in an ethanol solution using an ultrasonic disperser, and then the nano-reinforcement material was mixed with glass powder to obtain a mixture A.
[0063] The shape memory alloy fiber is mixed into the mixture A to obtain the mixture B.
[0064] The microcapsule repairing agent was uniformly mixed into the mixture B, and the mixed glass powder material was placed in a drying oven and dried at 120° C. for 4 hours to obtain the glass powder material.
[0065] (3) Usage:
[0066] The substrate to be sealed is pretreated.
[0067] The dried glass powder is evenly coated on the contact surface of the substrate.
[0068] The glass powder coated substrate was placed in a sealed furnace and heated at 370°C for 0.5 h.
[0069] The substrate was gradually cooled to room temperature.
[0070] Embodiment 3:
[0071] (1) Component preparation:
[0072] Borosilicate glass composition: SiO271%, B2O319%, Na2O 3%, Al2O31%, CaO 2% Microcapsule repair agent: size 40μm, including polyurea formaldehyde resin and epoxy resin repair agent
[0073] Nano-reinforced material: a mixture of nano-silicon dioxide and nano-alumina, with a mass percentage of 4%
[0074] Shape memory alloy fiber: nickel titanium alloy fiber, diameter 20μm, length 3mm, mass percentage 3%
[0075] (2) Preparation steps:
[0076] ① Preparation of microcapsule repair agent:
[0077] Mix the epoxy resin repair agent and initiator evenly to form a uniform liquid core material.
[0078] Under stirring conditions, the core material is dropped into the polyurea formaldehyde resin solution to form microcapsules.
[0079] Curing was performed at 60°C for 2 hours to ensure the shell strength of the microcapsules.
[0080] ② Preparation of glass powder materials:
[0081] The borosilicate glass block was crushed to 180 mesh to form a uniform glass powder.
[0082] The mixture of nano-silica and nano-alumina was dispersed in an ethanol solution using an ultrasonic disperser, and then the nano-reinforcement material was mixed with glass powder to obtain a mixture A.
[0083] The shape memory alloy fiber is mixed into the mixture A to obtain the mixture B.
[0084] The microcapsule repairing agent was uniformly mixed into the mixture B, and the mixed glass powder material was placed in a drying oven and dried at 120° C. for 4 hours to obtain the glass powder material.
[0085] (3) Usage:
[0086] The substrate to be sealed is pretreated.
[0087] The dried glass powder is evenly coated on the contact surface of the substrate.
[0088] The glass powder coated substrate was placed in a sealed furnace and heated at 380°C for 0.5 h.
[0089] The substrate was gradually cooled to room temperature.
[0090] Comparative Example 1:
[0091] The preparation method is the same as that of Example 1, except that no microcapsule repair agent is added;
[0092] Comparative Example 2:
[0093] The preparation method is the same as that of Example 1, except that no nickel-titanium alloy fiber is added;
[0094] Comparative Example 3:
[0095] The preparation method is the same as that of Example 1, except that no nano-reinforcement material is added.
[0096] The glass powder materials obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were tested for performance, and the test data are as follows:
[0097] Flexural strength(MPa) Fracture toughness (MPa·m^0.5) Self-repair efficiency (%) Example 1 120 2.5 80 Example 2 125 2.8 85 Example 3 130 3.0 90 Comparative Example 1 110 2.0 10 Comparative Example 2 115 2.3 65 Comparative Example 3 118 2.4 60
[0098] It can be seen from the above test data that the glass powder material in the embodiment with the addition of microcapsule repair agent, nano-reinforcement material and shape memory alloy fiber has significantly improved flexural strength, fracture toughness and self-repair efficiency compared with the comparative material. In particular, in terms of self-repair efficiency, the embodiments all show a high self-repair ability, while the self-repair efficiency of comparative example 1 is low due to the absence of the addition of microcapsule repair agent. Although the self-repair efficiency of comparative example 2 is improved due to the absence of the addition of shape memory alloy fiber, the flexural strength and fracture toughness are still lower than those of the embodiment. Although the self-repair efficiency of comparative example 3 is improved due to the absence of the addition of nano-reinforcement material, the flexural strength and fracture toughness are still lower than those of the embodiment.
[0099] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A low-temperature sealing glass powder material with self-repairing function, characterized in that: The glass powder material comprises the following components: borosilicate glass composition: SiO2 70-75%, B2O3 15-20%, Na2O 2-5%, Al2O3 1-3%, CaO 1-3%; microcapsule repairing agent; nano-reinforced material; shape memory alloy fiber.
2. The low-temperature sealing glass powder material with self-repairing function according to claim 1, characterized in that: The size of the microcapsule repair agent is 10-50 μm; the microcapsule repair agent includes polyurea formaldehyde resin and epoxy resin repair agent.
3. The low-temperature sealing glass powder material with self-repairing function according to claim 1, characterized in that: The nano-enhanced material is nano-silicon dioxide or nano-aluminum oxide, or a mixture of the two.
4. The low-temperature sealing glass powder material with self-repairing function according to claim 1, characterized in that: The preparation method of the microcapsule repair agent comprises the following steps: S1: Mix the epoxy resin repair agent and the initiator evenly to form a uniform liquid core material; S2: under stirring conditions, dropping the core material into the polyurea formaldehyde resin solution to form microcapsules; S3: Curing of microcapsules: Curing at 60°C for 2 hours to ensure the shell strength of the microcapsules.
5. The method for preparing a glass powder material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S501: crushing the borosilicate glass block to 100-200 mesh to form a uniform glass powder; S502: using an ultrasonic disperser to disperse the nano-reinforced material in the ethanol solution, and then mixing the nano-reinforced material with the glass powder to obtain a mixture A; S503: mixing the shape memory alloy fiber into the mixture A obtained in S502 to obtain a mixture B; S504: The microcapsule repairing agent is uniformly mixed into the mixture B, and the mixed glass powder material is placed in a drying oven, and dried at 120° C. for 4 hours to obtain the glass powder material.
6. The low-temperature sealing glass powder material with self-repairing function according to claim 1, characterized in that: The method for using the glass powder material comprises the following steps: S601: pre-treating the substrate to be sealed; S602: evenly coating the dried glass powder on the contact surface of the substrate; S603: placing the substrate coated with glass powder in a sealed furnace and heating at 300-400° C. for 0.5 h; S604: gradually cooling the substrate to room temperature.
7. The low-temperature sealing glass powder material with self-repairing function according to claim 1, characterized in that: The shape memory alloy fiber is a nickel-titanium alloy fiber with a fiber diameter of 5 to 20 μm and a length of 0.1 to 5 mm. The mass percentage of the shape memory alloy fiber is 0.5% to 3% of the total mass of the glass powder material.
8. The low-temperature sealing glass powder material with self-repairing function according to claim 1, characterized in that: The mass percentage content of the nano-reinforced material is 0.1% to 5% of the total mass of the glass powder material.
Citation Information
Cited By
Reusable fire barrier and preparation method thereof
CN120698770A
Antifouling glaze with snow velvet effect and preparation method thereof
CN120903826A