Self-compacting concrete additive and subway precast slab track self-compacting concrete
By using mica powder, talc powder and other components in self-solid concrete, the problems of insufficient strength, poor impact resistance and insufficient durability in the early stages of the construction of prefabricated subway tracks are solved, and high electrical insulation is achieved Improved performance and comprehensive performance, suitable for engineering applications in complex environments.
Patent Information
- Application Number
- CN202410896904.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-05
AI Technical Summary
Traditional self-finished concrete is insufficient in the early stages of the construction of prefabricated panel tracks of subways, poor impact resistance, poor electrical insulation performance and insufficient durability, making it difficult to meet the composite needs of the construction and use environment at the same time.
A self-finished concrete additive is used, which consists of mica powder, talc powder, silica fume, carboxymethyl cellulose, styrene butadiene glue powder, paraffin powder, lignin fiber, polypropylene fiber and triisopropyl alcohol amines improve the early strength, impact resistance, electrical insulation properties and durability of concrete through the coordinated action of each component.
It significantly improves the resistivity, early strength, impact resistance and durability of concrete, reduces water leakage and segregation phenomena, and is suitable for subway prefabricated plate tracks and other high-performance self-contained concrete engineering projects.
Smart Images

Figure BDA0004929238320000121 
Figure BDA0004929238320000131
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and more specifically, relates to a self-compacting concrete additive and a subway prefabricated slab track self-compacting concrete. Background Art
[0002] Urban rail transit has developed rapidly in major cities due to its advantages of speed, comfort and large passenger capacity. Prefabricated prefabricated track has been widely used in subways or trams in cities such as Shanghai, Shenzhen, Guangzhou, Chengdu, Xi'an and Qingdao due to its advantages of low cost, high durability and low maintenance requirements. Self-compacting concrete is widely used as the filling layer material of prefabricated prefabricated track in subways due to its high cost-effectiveness, self-leveling ability and high durability. However, traditional self-compacting concrete still faces some technical challenges when applied to the construction of subway prefabricated track, such as insufficient early strength, poor impact resistance, poor electrical insulation performance and insufficient durability.
[0003] During the construction of subway precast track, insufficient early strength will lead to an extension of the construction period, affect the progress of the project, and even affect the overall stability of the structure. The early strength of traditional self-compacting concrete mainly depends on the hydration reaction of cement, and the speed and effect of the hydration reaction are affected by many factors, such as water-cement ratio, type and amount of admixtures, etc. During the use of subway precast track, it is often subjected to dynamic loads and impact loads during train operation, which requires concrete to have good impact resistance. Due to the brittleness of its own materials, traditional self-compacting concrete is prone to cracks and even damage when impacted. During the construction and use of subway precast track, the electrical insulation performance of concrete is also an important indicator. Good electrical insulation performance can prevent the occurrence of leakage accidents and ensure the safe operation of the track system. The electrical insulation performance of traditional self-compacting concrete is affected by its composition and structure, and it is usually difficult to meet high electrical insulation requirements. Subway precast track is exposed to complex environments for a long time, such as moisture, salt spray, chemical corrosion, etc., which requires concrete to have excellent durability. Traditional self-compacting concrete is easily affected by environmental factors during long-term use, and cracking, peeling and other phenomena may occur, which will affect its service life. Therefore, how to improve the durability of self-compacting concrete in complex environments while ensuring safety is an urgent problem that needs to be solved.
[0004] Adding additives to self-compacting concrete is a common method for changing the properties of self-compacting concrete. However, traditional additives usually only improve one property of concrete, such as enhancing fluidity or improving early strength, but under complex working conditions, the improvement of a single property is often not enough to meet actual needs. For example, in the construction of subway precast slab tracks, concrete is required to have good fluidity, high early strength, impact resistance and durability, and traditional additives are difficult to take into account these requirements at the same time. In addition, the interactions between different additives in concrete are complex and prone to unpredictable side effects. For example, although some water reducers can significantly improve the fluidity of concrete, they may also cause the early strength of concrete to decrease, and even segregation and bleeding. Chinese patent CN104003641A discloses a self-compacting concrete additive for slab ballastless track, which uses slag powder to improve the anti-segregation ability of self-compacting concrete, and combines solid sulfur ash, fly ash and water reducer to reduce the shrinkage of concrete, and the effect is relatively single.
[0005] Therefore, the present invention proposes a self-compacting concrete additive that can be used for the preparation of subway precast track. By optimizing the ratio of components and the synergistic effect of each component, the comprehensive performance of concrete, such as early strength, impact resistance, electrical insulation and durability, is significantly improved. The additive is not only suitable for the construction of subway precast track, but can also be widely used in other engineering projects that require high-performance self-compacting concrete, providing a new idea and solution for solving existing problems. Summary of the invention
[0006] Based on the above technical problems existing in the prior art, the purpose of the present invention is to provide a self-compacting concrete additive and a subway precast track self-compacting concrete. The coordinated effect of the various components in the additive has the advantages of micro-expansion, anti-segregation, early strength, impact resistance, electrical insulation, strong water repellency, reinforcement protection, high durability, etc. It can be used as a subway precast track self-compacting concrete additive, and can also be used as an additive for ordinary self-compacting concrete.
[0007] In order to achieve the above object, the technical solution of the present invention is as follows:
[0008] A self-compacting concrete additive, the raw material components of which are calculated by weight:
[0009] 100 parts of mica powder, 50-100 parts of talc, 100-250 parts of silica fume, 1-2 parts of carboxymethyl cellulose, 20-50 parts of propylene benzene rubber powder, 25-50 parts of styrene butadiene rubber powder, 10-20 parts of paraffin powder, 20-50 parts of lignin fiber, 10-20 parts of polypropylene fiber, and 10-50 parts of triisopropanolamine.
[0010] The self-compacting concrete additive of the present invention can also be composed of the above components.
[0011] A preferred embodiment, the self-compacting concrete additive is composed of the following components by weight: 100 parts of mica powder, 50-80 parts of talc, 110-220 parts of silica fume, 1-2 parts of carboxymethyl cellulose, 20-45 parts of propylene benzene rubber powder, 30-45 parts of styrene-butadiene rubber powder, 10-20 parts of paraffin powder, 20-40 parts of lignin fiber, 10-20 parts of polypropylene fiber, and 20-40 parts of triisopropanolamine.
[0012] Further preferably, the self-compacting concrete additive is composed of the following components by weight: 100 parts of mica powder, 55-75 parts of talc, 110-200 parts of silica fume, 1-2 parts of carboxymethyl cellulose, 20-40 parts of propylene benzene rubber powder, 30-40 parts of styrene-butadiene rubber powder, 10-15 parts of paraffin powder, 25-35 parts of lignin fiber, 10-15 parts of polypropylene fiber, and 20-35 parts of triisopropanolamine.
[0013] The additive of the present invention adopts mica powder, and the fine particles of mica powder can fill the tiny gaps inside the concrete, increase the density and mechanical properties of the concrete. In addition, the flaky structure of the mica powder helps to improve workability, reduce the water absorption rate of the concrete, improve its durability, and reduce the shrinkage and cracking of the concrete. The mica powder can be evenly distributed and hold the stones, increase the bonding force between the particles inside the concrete, and reduce the segregation and bleeding of the concrete mixture. The mica powder has high electrical insulation, can improve the resistivity of the self-compacting concrete, and has good electrical insulation performance under high pressure environment.
[0014] In a preferred embodiment, the mica powder is fine powder extracted from natural ore, with a particle size of ≤10 μm, a SiO2 content of 50% to 55%, an Al2O3 content of 30% to 35%, and a K2O and Na2O content of 5% to 10%.
[0015] The present invention adds a certain amount of talcum powder, and utilizes the smooth flaky structure, large specific surface area, low water absorption and chemical inertness of the talcum powder to improve the fluidity of the concrete, effectively reduce the viscosity of the concrete and reduce water bleeding. In addition, the filling effect of the fine particles of the talcum powder helps to improve the early strength, durability and shrinkage of the concrete.
[0016] In a preferred embodiment, the talc powder is a fine powder extracted from talc ore, with a particle size of ≤10 μm, a SiO2 content of 50% to 60%, and a MgO content of 30% to 40%.
[0017] The present invention adds a certain amount of silica fume, and the large specific surface area of silica fume is conducive to improving the fluidity and pumpability of self-compacting concrete, and helps to improve the water retention of concrete. In addition, the fine particles and high activity of silica fume can accelerate the hydration reaction of cement, increase the density of cement paste, and thus improve the early strength of concrete. In the later stage of hydration, silica fume further fills the pores in concrete through volcanic ash reaction, significantly improving the strength, durability, resistivity and other properties of concrete.
[0018] In the preferred embodiment, the silicon ash is the product of the fumes released from the exhaust gas during the smelting of ferrosilicon and industrial silicon (metallic silicon) in the ferroalloy plant, which is collected and treated by a special capture device, and its surface area should be ≥20000m 2 / kg, the activity index should be ≥100%.
[0019] The present invention incorporates a certain amount of carboxymethyl cellulose, propylene styrene rubber powder and styrene butadiene rubber powder, and these polymers significantly improve the rheological properties and workability of self-compacting concrete, enhance adhesion, and reduce bleeding and segregation. Unlike carboxymethyl cellulose, propylene styrene rubber powder and styrene butadiene rubber powder aggregate and deposit on cement particles and pore surfaces, gradually cross-linking to form a continuous polymer film structure. The formation of the polymer film helps to further improve the bonding force of the self-compacting concrete, reduce bleeding and segregation. In addition, the polymer film can disperse and conduct stress, inhibit the generation and diffusion of cracks, and improve the durability, toughness and impact resistance of the mortar. Compared with propylene styrene rubber powder, styrene butadiene rubber powder performs better in improving the impact resistance of concrete, but performs slightly worse in improving the bonding strength and durability of concrete.
[0020] In the preferred embodiment, the density of the carboxymethyl cellulose is 1.050 g / cm 3 , molecular weight is 180.
[0021] In a preferred embodiment, the bulk density of the propylene-styrene rubber powder is 350-550 g / L, the pH value is 7.5-9.5, and the minimum film-forming temperature is 0°C.
[0022] In a preferred embodiment, the density of the styrene-butadiene rubber powder is 1.04 g / mL, and the powder is soluble in a solvent having a solubility parameter between 7.7 and 9.4.
[0023] In a more preferred embodiment, the mass ratio of the propylene benzene rubber powder to the styrene butadiene rubber powder is 1:1 to 1.5. More preferably, the mass ratio of the propylene benzene rubber powder to the styrene butadiene rubber powder is 1:1.2.
[0024] The present invention adds a certain amount of paraffin powder, and utilizes the high insulation and hydrophobicity of the paraffin powder to improve the water absorption, durability and resistivity of the self-compacting concrete. Among them, the improvement of the resistivity of the self-compacting concrete can reduce the electrochemical corrosion of the steel bars. However, since the paraffin powder has hydrophobicity, its addition will have a negative impact on the working performance and strength of the self-compacting concrete, and it needs to be used in coordination with other admixtures.
[0025] In the preferred embodiment, the density of the paraffin powder is 0.8-1.0 g / cm 3 , the melting point is 50℃~70℃.
[0026] The present invention incorporates a certain amount of lignin fiber and polypropylene fiber, which can effectively prevent the development and expansion of micro cracks in concrete, help improve the internal structure of concrete, and then improve the crack resistance of concrete, and reduce segregation and water bleeding in concrete. Compared with polypropylene fiber, lignin fiber can absorb and retain more water, and has better performance in water retention and adhesion. Compared with lignin fiber, polypropylene fiber is more outstanding in improving the toughness and impact resistance of concrete. Under the coordinated effect of the two fibers, the performance of self-compacting concrete is better.
[0027] In a preferred embodiment, the length of the lignin fiber is about 6 mm, the pH value is about 7, and the gray content does not exceed 18%.
[0028] In the preferred embodiment, the density of the polypropylene fiber is 0.9 to 0.92 g / cm 3 , diameter is 22-50μm and length is 12-19mm.
[0029] In a more preferred embodiment, the mass ratio of the lignin fiber to the polypropylene fiber is 2 to 3:1. More preferably, the mass ratio of the lignin fiber to the polypropylene fiber is 2 to 2.5:1.
[0030] The present invention adds a certain amount of triisopropanolamine to promote cement hydration reaction and improve early mechanical properties. Triisopropanolamine (TIPA) can accelerate the Fe 3+ and Al 3+ The dissolution of ions shortens the induction period, promotes the overall silicate reaction to a certain extent, and improves the early mechanical properties.
[0031] In a preferred embodiment, the triisopropanolamine has a density of 0.99-1 g / ml, an industrial grade purity, and a fineness of ≤10 μm.
[0032] The present invention also provides a subway prefabricated track self-compacting concrete, which comprises the self-compacting concrete additive. The addition amount of the self-compacting concrete additive in the self-compacting concrete is 10% to 30% of the cementitious material.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The self-compacting concrete additive provided by the present invention has synergistic effects among the components, and has the advantages of micro-expansion, anti-segregation, early strength, impact resistance, electrical insulation, strong water repellency, reinforcement protection, high durability, etc. When added to concrete, the resistivity of the self-compacting concrete can be improved, so that it has good electrical insulation performance under high pressure environment. It can significantly improve the strength and durability of concrete, reduce bleeding and segregation. It can be used in the preparation of self-compacting concrete for subway prefabricated tracks, and has high practical application value. DETAILED DESCRIPTION
[0035] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. It should be noted that the reagents used in the present embodiment are all common commercial products.
[0037] A self-compacting concrete additive is prepared by mixing mica powder, talcum powder, silica fume, carboxymethyl cellulose, propylene benzene rubber powder, styrene butadiene rubber powder, paraffin powder, lignin fiber, polypropylene fiber and triisopropanolamine.
[0038] Among them, the weight proportion of each component is: 100 parts of mica powder, 50-100 parts of talc powder, 100-250 parts of silica fume, 1-2 parts of carboxymethyl cellulose, 20-50 parts of propylene benzene rubber powder, 25-50 parts of styrene butadiene rubber powder, 10-20 parts of paraffin powder, 20-50 parts of lignin fiber, 10-20 parts of polypropylene fiber, and 10-50 parts of triisopropanolamine.
[0039] Furthermore, the mica powder is a fine powder extracted from natural ore, with a particle size of ≤10 μm, a SiO2 content of 50% to 55%, an Al2O3 content of 30% to 35%, and a K2O and Na2O content of 5% to 10%.
[0040] Furthermore, the talcum powder is a fine powder extracted from talc ore, with a particle size of ≤10 μm, a SiO2 content of 50% to 60%, and a MgO content of 30% to 40%.
[0041] Furthermore, the silica ash is a product obtained by collecting and treating the smoke and dust emitted from the exhaust gas during the smelting of ferrosilicon and industrial silicon (metallic silicon) in ferroalloy plants through a special capture device, and its surface area should be ≥20,000 m 2 / kg, the activity index should be ≥100%.
[0042] Furthermore, the carboxymethyl cellulose has a density of 1.050 g / cm 3 , molecular weight is 180; the bulk density of the propylene benzene rubber powder is 350-550g / L, the pH value is 7.5-9.5, and the minimum film-forming temperature is 0°C; the density of the styrene-butadiene rubber powder is 1.04g / mL, and it is soluble in a solvent with a solubility parameter between 7.7 and 9.4; the mass ratio of the propylene benzene rubber powder to the styrene-butadiene rubber powder is 1:1~1.5.
[0043] Furthermore, the density of the paraffin powder is 0.8-1.0 g / cm 3 , the melting point is 50℃~70℃.
[0044] Furthermore, the length of the lignin fiber is about 6 mm, the pH value is about 7, and the gray content does not exceed 18%; the density of the polypropylene fiber is 0.9-0.92 g / cm 3 , diameter is 22-50μm, length is 12-19mm; the mass ratio of the lignin fiber to the polypropylene fiber is 2-3:1; the density of the triisopropanolamine is 0.99-1g / ml, the purity is industrial grade, and the fineness needs to be ≤10μm.
[0045] A self-compacting concrete for prefabricated subway tracks, wherein the amount of the self-compacting concrete additive added to the self-compacting concrete is 10% to 30% of the cementitious material.
[0046] Example 1
[0047] The invention discloses a subway prefabricated slab track self-compacting concrete with a self-compacting concrete additive. The self-compacting concrete additive is prepared from mica powder, talcum powder, silica fume, carboxymethyl cellulose, propylbenzene rubber powder, styrene-butadiene rubber powder, paraffin powder, lignin fiber, polypropylene fiber and triisopropanolamine. Under the condition that the amount of cement used is 2000 parts by mass, the component contents are as follows: 100 parts by mass of mica powder, 60 parts by mass of talcum powder, 200 parts by mass of silica fume, 1 part by mass of carboxymethyl cellulose, 30 parts by mass of propylbenzene rubber powder, 35 parts by mass of styrene-butadiene rubber powder, 15 parts by mass of paraffin powder, 30 parts by mass of lignin, 13 parts by mass of polypropylene fiber and 30 parts by mass of triisopropanolamine.
[0048] Example 2
[0049] The invention discloses a subway prefabricated slab track self-compacting concrete with a self-compacting concrete additive, which is prepared from mica powder, talcum powder, silica fume, carboxymethyl cellulose, propylene benzene rubber powder, styrene butadiene rubber powder, paraffin powder, lignin fiber, polypropylene fiber, triisopropanolamine and the like. Under the condition that the amount of cement used is 2000 parts by mass, the components of the concrete are as follows: 100 parts by mass of mica powder, 75 parts by mass of talcum powder, 180 parts by mass of silica fume, 1 part by mass of carboxymethyl cellulose, 40 parts by mass of propylene benzene rubber powder, 40 parts by mass of styrene butadiene rubber powder, 15 parts by mass of paraffin powder, 35 parts by mass of lignin, 15 parts by mass of polypropylene fiber and 35 parts by mass of triisopropanolamine.
[0050] Example 3
[0051] The invention discloses a subway prefabricated slab track self-compacting concrete with a self-compacting concrete additive, which is prepared from mica powder, talcum powder, silica fume, carboxymethyl cellulose, propylbenzene rubber powder, styrene-butadiene rubber powder, paraffin powder, lignin fiber, polypropylene fiber, triisopropanolamine and the like. Under the condition that the amount of cement used is 2000 parts by mass, the components of the concrete are as follows: 100 parts by mass of mica powder, 55 parts by mass of talcum powder, 120 parts by mass of silica fume, 2 parts by mass of carboxymethyl cellulose, 25 parts by mass of propylbenzene rubber powder, 30 parts by mass of styrene-butadiene rubber powder, 10 parts by mass of paraffin powder, 25 parts by mass of lignin, 10 parts by mass of polypropylene fiber and 20 parts by mass of triisopropanolamine.
[0052] Comparative Example 1
[0053] The difference from Example 1 is that no styrene-butadiene rubber powder is added.
[0054] Comparative Example 2
[0055] The difference from Example 1 is that no paraffin was added.
[0056] Comparative Example 3
[0057] The difference from Example 1 is that no triisopropanolamine was added.
[0058] Comparative Example 4
[0059] The difference from Example 1 is that 40 parts of wood cellulose and 10 parts of polypropylene fibers are used.
[0060] Comparative Example 5
[0061] The difference from Example 1 is that the propylene benzene rubber powder is 20 parts and the styrene butadiene rubber powder is 45 parts.
[0062] Performance Testing
[0063] (1) Fluidity test
[0064] Fluidity is one of the most critical indicators for evaluating the quality of self-compacting concrete. The test was conducted using a slump cone with a height of 60 mm, an upper inner diameter of 70 mm, a lower inner diameter of 100 mm, and a lower outer diameter of 120 mm. The test was performed in accordance with GB / T2419-2005 (2005). The results are shown in Table 1.
[0065] (2) Compressive strength test
[0066] The strength of the self-compacting concrete is represented by its compressive strength at 3d, 7d, and 28d. According to the content of GB / T17671-1999, the compressive strength test was carried out on the examples and comparative examples. The size of the test piece was 100mm×100mm×100mm. It should be noted that after pouring the material into the mold, no vibration is required. The results are shown in Table 1.
[0067] (3) Resistivity test
[0068] The resistivity of the self-compacting concrete was measured using a 24-volt four-electrode method after 3, 7, and 28 days of curing. Four electrodes are usually arranged on the sample, the two inner electrodes are used to measure the voltage, and the two outer electrodes are used to measure the current. In order to avoid the influence of moisture content on the measurement results, the specimens were kept in a saturated dry state during the resistivity test. For each group of the embodiments and comparative examples, three cubic specimens were cast in a plastic mold to measure the average resistivity value of the samples, and the results are shown in Table 1.
[0069] (4) Drop weight impact test
[0070] The drop hammer impact test determines the average value of the impact energy corresponding to the initial and final cracks. The initial crack is the stage where the first crack appears on the concrete surface and a needle can be inserted into the crack, while the final crack is the stage where the sample disintegrates into fragments. The impact resistance is judged based on the absorbed energy. A hammer weighing 4.53 kg (10 lb) is used to apply the impact load to a cylindrical disk with a diameter of 100 mm and a height of 63.5 mm at a drop height of 457 mm. In this test, the hammer falls on the steel ball, through which the impact load is transmitted to the cylindrical disk. The results are shown in Table 1.
[0071] 5. Durability test
[0072] The durability of the self-compacting concrete prepared in the examples and comparative examples was tested with reference to the "Concrete Durability Test and Assessment Standard JGJ / T 193-2009", and the results are shown in Table 1.
[0073] Table 1
[0074]
[0075]
[0076] It can be seen from Examples 1-3 that the additive used in subway precast slab track self-compacting concrete of the present invention can increase the fluidity of concrete to meet the requirements of self-compacting. At the same time, the self-compacting concrete with the additive of the present invention has high resistivity, high early strength, and good impact resistance, and is suitable for subway precast slab track self-compacting concrete.
[0077] As can be seen from Example 1 and Comparative Example 1, adding styrene-butadiene rubber powder can improve the impact resistance of self-compacting concrete, and improve fluidity, so that it has better workability. The impact resistance of Comparative Example 1 is much lower than that of Examples 1-3, not only because styrene-butadiene rubber powder can promote the formation of polymer structure inside concrete and improve concrete density, but also because styrene-butadiene rubber powder can produce coupling effect with polypropylene fiber in the composition of the present invention, and jointly improve the impact resistance of self-compacting concrete. This is because adding polypropylene fiber and styrene-butadiene rubber powder at the same time leads to the formation of polymer structure, which makes concrete density increase and microstructure more solid. In addition, the presence of polypropylene fiber delays crack propagation, so impact resistance can be enhanced. And, styrene-butadiene rubber powder itself can play a water-reducing effect, improves the fluidity of self-compacting concrete, and makes it more fluid.
[0078] As can be seen from Example 1 and Comparative Example 2, adding paraffin powder can improve the resistivity of self-compacting concrete, but it has an impact on its fluidity. From the perspective of pore structure, although the hydrophobicity of paraffin causes the pore structure to become rough, its electrical insulation and hydrophobicity help to extend the conductive path, thereby improving the resistivity of cement-based materials. From the perspective of moisture content, the hydrophobicity of paraffin helps to increase the air content and reduce the moisture content of cement-based materials, thereby significantly increasing their resistivity. From the perspective of ionic strength, the addition of paraffin reduces the ionic strength of cement-based materials, thereby increasing their resistivity. This is because the hydrophobicity of paraffin covers the hydration products, inhibits their dissolution and ionization, thereby reducing the content of charged carriers. But at the same time, paraffin powder will cover the surface of cement particles during stirring, because its own good hydrophobic properties will cause some cement particles to be unable to contact with water, generate hydration products, and cause their fluidity to decrease. However, Examples 1-3 found that even if paraffin powder was added, because of other ingredients in the additive, such as styrene-butadiene rubber powder, the fluidity of the samples was also above 700mm, which can meet actual engineering needs.
[0079] It can be seen from Example 1 and Comparative Example 3 that the 28-day compressive strength of the concrete with triisopropanolamine added is higher than that of the concrete without triisopropanolamine, indicating that the addition of triisopropanolamine can effectively improve the mechanical properties of self-compacting concrete. This is because triisopropanolamine (TIPA) can accelerate the degradation of F in C4AF.e 3+ and Al 3+ ions dissolve, promoting the formation of calcium aluminate. The main reason is the formation of TIPA-Fe compounds, which promotes the dissolution of the ferrite phase, makes other phases more easily dissolved, shortens the induction period, promotes the overall silicate reaction to a certain extent, and improves the early mechanical properties. It is worth noting that TIPA has almost no effect on the fluidity of self-compacting concrete while improving the mechanical properties of self-compacting concrete. Unlike other additives, it sacrifices its fluidity while improving the early strength, which has an adverse effect on the working performance of self-compacting concrete. It was found through experiments that compared with comparative example 3, the compressive strength of Examples 1-3 with the addition of TIPA was increased by 12.3%, 15.6% and 23.8% at 3d, 7d and 28d, respectively, and the increase exceeded the value of the existing research. This is because the other components in the additive and TIPA produce a coupling effect on the early strength of the self-compacting concrete, which illustrates the synergistic effect of the components of the present invention on the improvement of the mechanical properties of the self-compacting concrete.
[0080] From the results of Comparative Examples 4 and 5, it can be seen that the specific proportions of wood cellulose and polypropylene fibers, propylene benzene rubber powder and styrene butadiene rubber powder can improve the mechanical properties and durability of the self-compacting concrete as a whole, which indicates that the components in the present invention have a synergistic effect and jointly improve the performance of the self-compacting concrete, which meets the use requirements of the self-compacting concrete for subway prefabricated tracks.
[0081] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A self-compacting concrete additive, characterized in that: The raw material components include, by weight: 100 parts of mica powder, 50-100 parts of talc powder, 100-250 parts of silica fume, 1-2 parts of carboxymethyl cellulose, 20-50 parts of propylene benzene rubber powder, 25-50 parts of styrene-butadiene rubber powder, 10-20 parts of paraffin powder, 20-50 parts of lignin fiber, 10-20 parts of polypropylene fiber and 10-50 parts of triisopropanolamine.
2. The self-compacting concrete additive according to claim 1, characterized in that: The mica powder is fine powder extracted from natural ore, with a particle size of ≤10 μm, a SiO2 content of 50% to 55%, an Al2O3 content of 30% to 35%, and a K2O and Na2O content of 5% to 10%.
3. The self-compacting concrete additive according to claim 1, characterized in that: The talcum powder has a particle size of ≤10 μm, a SiO2 content of 50% to 60%, and a MgO content of 30% to 40%.
4. The self-compacting concrete additive according to claim 1, characterized in that: The surface area of silica fume is ≥20000m 2 / kg, activity index ≥100%.
5. The self-compacting concrete additive according to claim 1, characterized in that: The mass ratio of the propylene benzene rubber powder to the styrene butadiene rubber powder is 1:1-1.
5.
6. The self-compacting concrete additive according to claim 1, characterized in that: The density of the paraffin powder is 0.8-1.0 g / cm 3 , the melting point is 50℃~70℃.
7. The self-compacting concrete additive according to claim 1, characterized in that: The mass ratio of the lignin fiber to the polypropylene fiber is 2-3:
1.
8. A self-compacting concrete for subway prefabricated track, characterized in that: The self-compacting concrete additive comprises the self-compacting concrete additive according to any one of claims 1 to 7, wherein the addition amount thereof is 10% to 30% of the cementitious material.
Citation Information
Patent Citations
Plate type ballastless track self-compacting concrete additive
CN104003641A