Lanthanum zirconate / silicon dioxide composite aerogel and preparation method thereof
Through the preparation of lanthanum zirconate/silica composite aerogel, the use of calcinedite structure and fiber reinforcement, the problem of limited service life of existing thermal barrier coating materials at high temperatures is solved, and the range from 1200°C to melting point is achieved The thermal stability and excellent thermal insulation performance are suitable for thermal barrier coatings.
Patent Information
- Application Number
- CN202410951748.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-05
AI Technical Summary
The existing thermal barrier coating materials have limited service life at high temperatures, and the limit temperature of the aerogel is not enough to meet future technical needs, especially materials such as ZrO2 and SiO2 fail at above 1200°C.
The composite aerogel with calcined chlorophylate structure was prepared by using lanthanum nitrate hexahydrate and zirconium nitrate pentahydrate as precursors, combined with fiber reinforcement, and sol-gel method and supercritical drying technology. Aerogel ensures thermal stability and excellent thermal insulation performance from 1200°C to melting point.
It achieves excellent thermal insulation and mechanical properties at high temperatures, is suitable for thermal barrier coatings, extends service life and reduces costs, and is suitable for large-scale production.
Smart Images

Figure CN118894713A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aerogel preparation, and in particular to a lanthanum zirconate / silicon dioxide composite aerogel and a preparation method thereof. Background Art
[0002] Thermal barrier coatings (TBCs) are a layer of ceramic coatings that are deposited on the surface of high-temperature resistant metals or superalloys. The TBCs act as a heat insulator for the substrate material, lowering the substrate temperature so that devices made of them (such as engine turbine blades) can operate at high temperatures and can increase the thermal efficiency of devices (engines, etc.) by more than 60%.
[0003] Thermal barrier coatings can significantly reduce the temperature of the substrate, have high hardness and good chemical stability, and have the advantages of preventing high-temperature corrosion, extending the service life of hot end components, increasing engine power and reducing fuel consumption. Currently, the most commonly used thermal barrier coating material is 8mol% Y2O3-ZrO2 (8YSZ), but the long-term use temperature of this material is lower than 1200°C, which can no longer meet the needs of future technological development. Research and search for materials that can replace ZrO2 and are suitable for thermal barrier coatings is the key.
[0004] Aerogel is a new type of three-dimensional nanoporous material with the characteristics of low density, high specific surface area, high porosity and low thermal conductivity. It is widely used in aerospace turbine guide vanes, building insulation and petrochemical industries. However, the maximum operating temperature of aerogels such as SiO2 and Al2O3 is below 900°C, which is not suitable for use in the field of thermal barrier coatings. Summary of the invention
[0005] In order to solve the problems in the prior art, the present invention provides a lanthanum zirconate / silicon dioxide composite aerogel and a preparation method thereof to obtain a fiber-reinforced lanthanum zirconate / silicon dioxide composite aerogel, which has a unique pyrochlore structure as well as good thermal insulation performance and mechanical strength, and has excellent application prospects in the field of thermal insulation.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0007] The present invention aims to provide a method for preparing a lanthanum zirconate / silicon dioxide composite aerogel, comprising the following steps:
[0008] S1: Using lanthanum nitrate hexahydrate and zirconium nitrate pentahydrate as precursors and propylene oxide as catalyst, LZ sol was obtained in anhydrous ethanol solvent;
[0009] S2: Using tetraethyl orthosilicate as a precursor and hydrochloric acid as a catalyst, hydrolysis is carried out in ethanol and water solvents to obtain SiO2 sol;
[0010] S3: dropping the obtained SiO2 sol into the LZ sol to obtain a mixed solution, and dropping the mixed solution dropwise into a propylene oxide gel accelerator to obtain an LZS sol;
[0011] S4: immersing the pretreated fiber in the LZS sol or evenly dropping the prepared LZS sol on the fiber until it is fully soaked, and applying a certain pressure to the fiber through a mold, and then standing in an oven to obtain FLZS gel;
[0012] S5: FLZS gel is aged and supercritically dried to obtain FLZS composite aerogel.
[0013] Lanthanum zirconate has a unique pyrochlore structure and will not undergo phase change between 1200°C and the melting point. However, the pyrochlore structure has oxygen vacancy defects. The applicant has found that the amorphous structure of SiO2 can inhibit the growth of pyrochlore crystals and improve the thermal stability of single-phase lanthanum zirconate aerogel. In addition, the lanthanum zirconate / silicon dioxide composite aerogel prepared by using fiber as a reinforcement has excellent thermal insulation and mechanical properties and can be used as a high-temperature thermal insulation material.
[0014] Furthermore, in step S1, the molar ratio of lanthanum nitrate hexahydrate, zirconium nitrate pentahydrate, propylene oxide and ethanol is 1:1:2:50.
[0015] Furthermore, in step S2, the molar ratio of ethyl orthosilicate, ethanol and water is 1:35:2; the molar ratio of ethyl orthosilicate and hydrochloric acid is 5:10. -4 , the mass fraction of the hydrochloric acid is 0.05wt%.
[0016] Furthermore, the molar ratio of propylene oxide to lanthanum nitrate hexahydrate added in step S3 is 1:1; and the molar fraction of SiO2 added to the mixed solution is 0% to 20%.
[0017] Furthermore, the fiber in step S4 can be any one of glass fiber, quartz fiber, basalt fiber and the like; the size of the fiber is 6cm×6cm×5mm, and the mass fraction of the fiber is 40% to 80%.
[0018] Furthermore, the fiber pretreatment method in step S4 is:
[0019] The fiber was immersed in 0.2 mol / L hydrochloric acid and subjected to ultrasonic oscillation for 2 h, repeated 2 to 3 times, and then taken out and rinsed with ethanol for 2 to 3 times and dried.
[0020] Furthermore, in step S4, the pressure applied is less than 0.5 MPa.
[0021] Furthermore, the supercritical drying method in step S5 is: using ethanol as the supercritical drying medium, pre-filling nitrogen so that the pressure in the kettle is not less than 2MPa, raising the temperature in the kettle to 270°C at a heating rate of 1°C / min, keeping warm for 2h until the pressure in the kettle is 8-10Mpa, turning on the water cooling device, slowly releasing the pressure in the kettle to normal pressure, passing N2 into the kettle for purge, and cooling to room temperature to obtain FLZS aerogel.
[0022] Furthermore, the preparation method of the lanthanum zirconate / silicon dioxide composite aerogel specifically comprises the following steps:
[0023] 1) Add lanthanum nitrate hexahydrate, zirconium nitrate pentahydrate and ethanol into a beaker in proportion, stir in a stirring pot at 60° C. until clear and transparent, and let stand at room temperature to obtain a mixed solution;
[0024] 2) adding propylene oxide dropwise into the mixed sol obtained in step 1), and stirring evenly to obtain LZ sol;
[0025] 3) Add tetraethyl orthosilicate, ethanol and water in a three-necked flask in proportion, stir mechanically for 15 minutes, add hydrochloric acid dropwise through a constant pressure funnel, stir for 120 minutes, and after stirring, seal and stand at room temperature for 24 hours to allow the hydrolysis reaction to proceed fully and slowly, thereby obtaining SiO2 sol;
[0026] 4) adding the SiO2 sol obtained in step 3) dropwise into the LZ sol obtained in step 2), and stirring evenly to obtain a mixed solution;
[0027] 5) adding propylene oxide dropwise into the mixed solution obtained in step 4), and stirring to obtain LZS sol;
[0028] 6) completely immersing the pretreated fiber in the LZS sol obtained in step 5) or evenly dropping the prepared LZS sol on the fiber until it is fully soaked, and applying a certain pressure to the fiber through a mold, and then standing in an oven at 60° C. to obtain FLZS gel;
[0029] 7) The FLZS gel obtained in step 6) is sealed and aged at room temperature for 72 hours and then supercritically dried to obtain a block FLZS composite aerogel.
[0030] The present invention also provides a lanthanum zirconate / silicon dioxide composite aerogel, which is prepared by the preparation method of the lanthanum zirconate / silicon dioxide composite aerogel.
[0031] The beneficial effects of the present invention are as follows:
[0032] 1) The present invention uses rare earth nitrate and tetraethyl orthosilicate as raw materials, fiber as reinforcement, ethanol as solvent, acid and alkali as catalyst, and uses a sol-gel method to prepare silicon-modified lanthanum zirconate wet gel, and obtains fiber-reinforced lanthanum zirconate / silicon dioxide composite aerogel after supercritical drying with ethanol. The obtained composite material has a low thermal conductivity and excellent thermal insulation and mechanical properties.
[0033] 2) The preparation process of the present invention is simple, low in cost, and suitable for large-scale production. By adding SiO2 to the single-phase lanthanum zirconate aerogel system, the thermal insulation performance of the material can be improved, and the process of the present invention controls the thermal conductivity and thermal insulation performance of the composite material by controlling the molar fraction of the added SiO2 and the molar fraction of the fiber. And the fiber is used for reinforcement, which is closer to practical application, improves the comprehensive performance of the composite material, and expands its application range.
[0034] 3) The pretreatment of the fiber increases the interfacial bonding strength between the fiber and the sol (such as the Fig.12 As shown), static electricity on the glass fiber surface is eliminated, clusters between fibers are reduced, and dust-free impregnation is achieved by slowly impregnating at a certain pressure (<0.5MPa).
[0035] 4) When the fiber is glass fiber or basalt fiber (mainly composed of SiO2), the surface of the gel skeleton is rich in lanthanum (III). Not only does the interaction between silicon (IV) and lanthanum improve the defects of the single-phase lanthanum zirconate, which has a higher defect tolerance and can effectively inhibit the growth of pyrochlore crystals, but also the mechanical properties are enhanced for application in high-temperature fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0037] Figure 1 This is a macroscopic image of the FLZS composite aerogel prepared in Example 1 of the present invention.
[0038] Figure 2 This is a macroscopic image of the FLZS composite aerogel prepared in Example 2 of the present invention.
[0039] Figure 3 This is a macroscopic image of the FLZ composite aerogel prepared in Comparative Example 1 of the present invention.
[0040] Figure 4This is a comparison chart of thermal conductivity of the FLZS composite aerogel prepared in Example 1 of the present invention and the FLZ composite aerogel prepared in Comparative Example 1 after heat treatment at different temperatures.
[0041] Figure 5 This is a macroscopic comparison diagram of the thickness of the FLZS composite aerogel prepared in Example 1 of the present invention and the FLZ composite aerogel prepared in Comparative Example 1 before and after heat treatment at 1000°C.
[0042] Figure 6 This is a macroscopic comparison diagram of the thickness of the FLZS composite aerogel prepared in Example 3 of the present invention and the FLZ composite aerogel prepared in Comparative Example 2 before and after heat treatment at 600, 800 and 1000°C.
[0043] Figure 7 The cold surface temperature of the FLZ composite aerogel prepared in Comparative Example 1 of the present invention after burning on a 1000°C flame for 30 seconds and 15 minutes.
[0044] Figure 8 It is the cold surface temperature of the FLZS composite aerogel prepared in Example 1 of the present invention after burning in a 1000° C. flame for 30 seconds and 15 minutes.
[0045] Fig. 9 High-temperature Raman images of the FLZS composite aerogel prepared in Example 3 of the present invention and the comparative example 2 after heat treatment at 1200°C.
[0046] Fig.10 This is a comparison chart of the compressive strength of the FLZS composite aerogel prepared in Example 3 of the present invention and the FLZ composite aerogel prepared in Comparative Examples 2 to 5 at 10%, 30%, and 50% strain.
[0047] Fig.11 This is an infrared comparison diagram of the FLZS composite aerogel prepared in Example 3 of the present invention and that of Comparative Example 6.
[0048] Fig.12 Electron micrographs of FLZS composite aerogels prepared before and after fiber pretreatment. DETAILED DESCRIPTION
[0049] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0050] Example 1
[0051] The preparation method of the lanthanum zirconate / silicon dioxide composite aerogel in this embodiment specifically includes the following steps:
[0052] 1) 2.598 g of lanthanum nitrate hexahydrate, 2.5759 g of zirconium nitrate pentahydrate and 13.821 g of anhydrous ethanol were added to a beaker in sequence, and stirred in a 60° C. heat-collecting magnetic stirring pot until clear and transparent, and allowed to stand at room temperature to obtain a mixed solution.
[0053] 2) 0.6969 g of propylene oxide was added dropwise into the mixed sol obtained in step 1), and the mixture was stirred to obtain LZ sol.
[0054] 3) Add 5 g TEOS, 38.64 g anhydrous ethanol and 0.864 g H2O into a three-necked flask, stir mechanically for 15 min, add 0.864 g of 0.05 wt% hydrochloric acid ethanol dilution solution dropwise at a rate of 6 s / drop through a constant pressure funnel, stir for 120 min, and after stirring, seal and let stand at room temperature for 24 h to allow the hydrolysis reaction to proceed fully and slowly to obtain SiO2 sol.
[0055] 4) 1.1342 g of the SiO2 sol obtained in step 3) was slowly dripped into the LZ sol obtained in step 2), and magnetically stirred for 30 min to obtain a mixed solution with a SiO2 doping amount of 10% by mole fraction.
[0056] 5) Add 0.3485 g of propylene oxide dropwise into the material obtained in step 4) and stir evenly to obtain LZS sol.
[0057] 6) 7.819 g of LZS sol was evenly dropped on the pretreated glass fiber (6 cm×6 cm×5 mm, 5.213 g), and a pressure of 0.02 MPa was applied to the fiber through a mold, and then allowed to stand in an oven to obtain a FLZS gel with a fiber molar fraction of 40%.
[0058] The pretreatment method of the glass fiber is as follows: immersing the glass fiber in 0.2 mol / L hydrochloric acid, ultrasonically oscillating for 2 hours, repeating 2 to 3 times, taking out and rinsing with ethanol for 2 to 3 times, and drying.
[0059] 7) The FLZS gel was sealed and aged for 72 hours before supercritical drying. Ethanol was used as the supercritical drying medium and N2 was pre-filled until the pressure in the kettle was 2MPa. The temperature in the kettle was raised to 270°C at a heating rate of 1°C / min and kept warm for 2 hours until the pressure in the kettle reached 10MPa. The water cooling device was turned on, and the pressure in the kettle was slowly released to normal pressure. N2 was then introduced into the kettle to purge it. After cooling to room temperature, the FLZS composite aerogel was obtained.
[0060] See attached Figure 1, is a macroscopic image of the FLZS composite aerogel obtained in this example, and Figure 4 FLZS10 is the thermal conductivity of this embodiment after heat treatment at different temperatures. Figure 5 FLZS10 in the figure is the thickness macrograph of this embodiment before and after heat treatment at 1000°C. Figure 8 The cold surface temperature of this embodiment after burning on a 1000°C flame for 30 seconds and 15 minutes is 71.4°C and 284.7°C respectively, indicating that the thermal insulation performance can be improved by adding SiO2 and composite glass fiber into the single-phase lanthanum zirconate system.
[0061] Example 2
[0062] The preparation method of the lanthanum zirconate / silicon dioxide composite aerogel in this embodiment specifically includes the following steps:
[0063] 1) 2.598 g of lanthanum nitrate hexahydrate, 2.5759 g of zirconium nitrate pentahydrate and 13.821 g of anhydrous ethanol were added to a beaker in sequence, and stirred in a 60° C. heat-collecting magnetic stirring pot until clear and transparent, and allowed to stand at room temperature to obtain a mixed solution.
[0064] 2) 0.6969 g of propylene oxide was added dropwise into the mixed sol obtained in step 1), and the mixture was stirred to obtain LZ sol.
[0065] 3) Add 5g TEOS, 38.64g anhydrous ethanol and 0.864g H2O into a three-necked flask, stir mechanically for 15min, add 0.864g of 0.05wt% hydrochloric acid ethanol dilution dropwise at a rate of 6s / drop through a constant pressure funnel, and stir for 120min. After stirring, seal and stand at room temperature for 24h to allow the hydrolysis reaction to proceed fully and slowly, and obtain SiO2 sol.
[0066] 4) 1.1342 g of the SiO2 sol obtained in step 3) was slowly dripped into the LZ sol obtained in step 2), and magnetic stirring was performed for 30 min to obtain a mixed solution with a Si doping amount of 10% by mole.
[0067] 5) 0.3485 g of propylene oxide was added dropwise into the material obtained in step 4), and the mixture was stirred to obtain LZS sol.
[0068] 6) 3.409 g of LZS sol was evenly dropped onto the pretreated glass fiber (6 cm×6 cm×5 mm, 5.113 g), and a pressure of 0.02 MPa was applied to the fiber through a mold, and then the fiber was allowed to stand in an oven to obtain a FLZS gel with a fiber molar fraction of 60%. The pretreatment method of the glass fiber in this embodiment is the same as that in Example 1.
[0069] 7) The FLZS gel was sealed and aged for 72 hours before supercritical drying. Ethanol was used as the supercritical drying medium and N2 was pre-filled until the pressure in the kettle was 2MPa. The temperature in the kettle was raised to 270°C at a heating rate of 1°C / min and kept warm for 2 hours until the pressure in the kettle reached 10MPa. The water cooling device was turned on, and the pressure in the kettle was slowly released to normal pressure. N2 was then introduced into the kettle to purge it. After cooling to room temperature, the FLZS composite aerogel was obtained.
[0070] See attached Figure 2 , which is a macroscopic picture of the FLZS composite aerogel obtained in this example, indicating that the mass fraction of the fibers can be adjusted as needed.
[0071] Example 3
[0072] The preparation method of the lanthanum zirconate / silicon dioxide composite aerogel in this embodiment specifically includes the following steps:
[0073] 1) 2.598 g of lanthanum nitrate hexahydrate, 2.5759 g of zirconium nitrate pentahydrate and 13.821 g of anhydrous ethanol were added to a beaker in sequence, and stirred in a 60° C. heat-collecting magnetic stirring pot until clear and transparent, and allowed to stand at room temperature to obtain a mixed solution.
[0074] 2) 0.6969 g of propylene oxide was added dropwise into the mixed sol obtained in step 1), and the mixture was stirred to obtain LZ sol.
[0075] 3) Add 5g TEOS, 38.64g anhydrous ethanol and 0.864g H2O into a three-necked flask, stir mechanically for 15min, add 0.864g of 0.05wt% hydrochloric acid ethanol dilution dropwise at a rate of 6s / drop through a constant pressure funnel, and stir for 120min. After stirring, seal and stand at room temperature for 24h to allow the hydrolysis reaction to proceed fully and slowly, and obtain SiO2 sol.
[0076] 4) 1.1342 g of the SiO2 sol obtained in step 3) was slowly dripped into the LZ sol obtained in step 2), and magnetic stirring was performed for 30 min to obtain a mixed solution with a Si doping amount of 10% by mole.
[0077] 5) 0.3485 g of propylene oxide was added dropwise into the material obtained in step 4), and the mixture was stirred to obtain LZS sol.
[0078] 6) 20g of LZS sol was evenly dripped onto the pretreated basalt fiber (6cm×6cm×5mm, 5.285g), and a pressure of 0.02MPa was applied to the fiber through a mold, and then the fiber was allowed to stand in an oven to obtain a FLZS gel with a fiber molar fraction of 60%. The pretreatment method of the basalt fiber in this embodiment is the same as the pretreatment method of the glass fiber in Example 1.
[0079] 7) The FLZS gel was sealed and aged for 72 hours before supercritical drying. Ethanol was used as the supercritical drying medium and N2 was pre-filled until the pressure in the kettle was 2MPa. The temperature in the kettle was raised to 270°C at a heating rate of 1°C / min and kept warm for 2 hours until the pressure in the kettle reached 10MPa. The water cooling device was turned on, and the pressure in the kettle was slowly released to normal pressure. N2 was then introduced into the kettle to purge it. After cooling to room temperature, the FLZS composite aerogel was obtained.
[0080] Comparative Example 1
[0081] The preparation method of the lanthanum zirconate / silicon dioxide composite aerogel in this comparative example specifically comprises the following steps:
[0082] 1) 2.598 g of lanthanum nitrate hexahydrate, 2.5759 g of zirconium nitrate pentahydrate and 13.821 g of anhydrous ethanol were added to a beaker in sequence, and stirred in a 60° C. heat-collecting magnetic stirring pot until clear and transparent, and allowed to stand at room temperature to obtain a mixed solution.
[0083] 2) 0.6969 g of propylene oxide was added dropwise into the mixed sol obtained in step 1), and the mixture was stirred to obtain LZ sol.
[0084] 3) 7.554 g of LZ sol was evenly dropped on the pretreated glass fiber (6 cm×6 cm×5 mm, 5.036 g), and a pressure of 0.02 MPa was applied to the fiber through a mold, and then the fiber was allowed to stand in an oven to obtain a FLZ gel with a fiber molar fraction of 40%. The pretreatment method of the glass fiber in this comparative example was the same as that in Example 1.
[0085] 4) The FLZ gel was sealed and aged for 72 hours before supercritical drying. Ethanol was used as the supercritical drying medium and N2 was pre-filled until the pressure in the kettle was 2MPa. The temperature in the kettle was raised to 270°C at a heating rate of 1°C / min and kept warm for 2 hours until the pressure in the kettle reached 10MPa. The water cooling device was turned on, and the pressure in the kettle was slowly released to normal pressure. N2 was then introduced into the kettle to purge it. After cooling to room temperature, the FLZ composite aerogel was obtained.
[0086] See attached Figure 3 , is a macroscopic image of the FLZ composite aerogel obtained in this comparative example, Figure 4 The thermal conductivity of the comparative example (FLZS0) and the example 2 (FLZS10) after heat treatment at different temperatures is shown in the figure. Figure 5 FLZS0 is the thickness macrograph of this comparative example before and after heat treatment at 1000°C. Figure 7 For this comparative example, the cold surface temperatures after burning on a 1000°C flame for 30 seconds and 15 minutes are 86.0°C and 375.7°C, respectively.
[0087] Comparative Example 2
[0088] The preparation method of the lanthanum zirconate / silicon dioxide composite aerogel in this comparative example specifically comprises the following steps:
[0089] 1) 2.598 g of lanthanum nitrate hexahydrate, 2.5759 g of zirconium nitrate pentahydrate and 13.821 g of anhydrous ethanol were added to a beaker in sequence, and stirred in a 60° C. heat-collecting magnetic stirring pot until clear and transparent, and allowed to stand at room temperature to obtain a mixed solution.
[0090] 2) 0.6969 g of propylene oxide was added dropwise into the mixed sol obtained in step 1), and the mixture was stirred to obtain LZ sol.
[0091] 3) 20g of LZ sol was evenly dripped on the pretreated basalt fiber (6cm×6cm×5mm, 5.118g), and a pressure of 0.02MPa was applied to the fiber through a mold, and then it was allowed to stand in an oven to obtain a FLZ gel with a fiber molar fraction of 40%. The pretreatment method of the basalt fiber in this comparative example was the same as the pretreatment method of the glass fiber in Example 1.
[0092] 4) The FLZ gel was sealed and aged for 72 hours before supercritical drying. Ethanol was used as the supercritical drying medium and N2 was pre-filled until the pressure in the kettle was 2MPa. The temperature in the kettle was raised to 270°C at a heating rate of 1°C / min and kept warm for 2 hours until the pressure in the kettle reached 10MPa. The water cooling device was turned on, and the pressure in the kettle was slowly released to normal pressure. N2 was then introduced into the kettle to purge it. After cooling to room temperature, the FLZS composite aerogel was obtained.
[0093] The thickness macroscopic comparison diagram of the FLZS composite aerogel prepared in Example 3 of the present invention and the FLZ composite aerogel prepared in Comparative Example 2 before and after heat treatment at 600, 800 and 1000°C is shown in the attached figure. Figure 6 As shown in the figure, it can be seen that after the fiber and the aerogel are tightly combined, the silicon dioxide component added in the present invention can inhibit the collapse of the lanthanum zirconate nanopores at high temperature. After heat treatment, the sintering degree of Example 3 of the present invention is lower than that of the composite aerogel of Comparative Example 2.
[0094] The high temperature Raman comparison diagram of the FLZS composite aerogel prepared in Example 3 of the present invention and the FLZ composite aerogel prepared in Comparative Example 2 after heat treatment at 1200°C is shown in the attached figure. Fig. 9 As shown in the figure, at 302cm -1 The observed position is E g In addition, 520cm -1 A 1g The mode is closely related to the bending vibration of Zr-O6 octahedron. -1 and 400cm-1 F 2g The mode is directly related to the bending vibration of Zr-O and La-O bonds. Compared with Comparative Example 2, after adding SiO2, the crystal absorption peak of Example 3 of the present invention is reduced, which proves that the growth of pyrochlore crystals can be effectively inhibited.
[0095] Comparative Example 3
[0096] The difference between this comparative example and Example 3 is that the content of LZS sol in step 6) is 10 g, and the remaining steps are the same.
[0097] Comparative Example 4
[0098] The difference between this comparative example and Example 3 is that the content of LZS sol in step 6) is 15 g, and the remaining steps are the same.
[0099] Comparative Example 5
[0100] The difference between this comparative example and Example 3 is that the content of LZS sol in step 6) is 25 g, and the remaining steps are the same.
[0101] The compressive strength comparison diagram of the FLZS composite aerogel prepared in Example 3 of the present invention and the FLZ composite aerogel prepared in Comparative Examples 2 to 5 at 10%, 30%, and 50% strain is shown in the attached figure. Fig.10 As shown in the figure, it can be seen that the maximum values are reached when the sol content is 20g, which are 0.76MPa and 2.51MPa respectively. As the sol content continues to increase, the compressive strength decreases. After adding Si, the bending stress increases, and the bearing capacity of the composite material is significantly improved. However, as the Si content changes, the bending strength of the composite material shows a trend of first increasing and then decreasing.
[0102] Comparative Example 6
[0103] The preparation method of lanthanum zirconate / silicon dioxide aerogel in this comparative example specifically comprises the following steps:
[0104] 1) 2.598 g of lanthanum nitrate hexahydrate, 2.5759 g of zirconium nitrate pentahydrate and 13.821 g of anhydrous ethanol were added to a beaker in sequence, and stirred in a 60° C. heat-collecting magnetic stirring pot until clear and transparent, and allowed to stand at room temperature to obtain a mixed solution.
[0105] 2) 0.6969 g of propylene oxide was added dropwise into the mixed sol obtained in step 1), and the mixture was stirred to obtain LZ sol.
[0106] 3) Add 5g TEOS, 38.64g anhydrous ethanol and 0.864g H2O into a three-necked flask, stir mechanically for 15min, add 0.864g of 0.05wt% hydrochloric acid ethanol dilution dropwise at a rate of 6s / drop through a constant pressure funnel, and stir for 120min. After stirring, seal and stand at room temperature for 24h to allow the hydrolysis reaction to proceed fully and slowly, and obtain SiO2 sol.
[0107] 4) 1.1342 g of the SiO2 sol obtained in step 3) was slowly dripped into the LZ sol obtained in step 2), and magnetic stirring was performed for 30 min to obtain a mixed solution with a Si doping amount of 10% by mole.
[0108] 5) 0.3485 g of propylene oxide was added dropwise into the material obtained in step 4), and the mixture was stirred to obtain LZS sol.
[0109] 6) Pour the mixed solution into a closed mold and let it stand at 60° C. for a period of time to obtain LZS gel.
[0110] 7) The FLZS gel was sealed and aged for 72 hours before supercritical drying. Ethanol was used as the supercritical drying medium and N2 was pre-filled until the pressure in the kettle was 2MPa. The temperature in the kettle was raised to 270°C at a heating rate of 1°C / min and kept warm for 2 hours until the pressure in the kettle reached 10MPa. The water cooling device was turned on, and the pressure in the kettle was slowly released to normal pressure. N2 was then introduced into the kettle to purge it. After cooling to room temperature, FLZS aerogel was obtained.
[0111] Specifically, steps 1) to 5) in this comparative example are the same as those in Example 3, except that there is no fiber in step 6). The infrared comparison diagram of the FLZS composite aerogel prepared in Example 3 of the present invention and that of Comparative Example 6 is shown in the attached figure. Fig.11 As shown in the figure, at 1123cm -1 The weak peak centered at 490cm is caused by the stretching vibration of Zr to O in Zr-O-Zr. -1 The weak band near is related to the vibration of the O-La-O bending mode. -1 The Si-O-Si bending vibration is exhibited nearby, which is attributed to the main component of the fiber, SiO2. Compared with the comparative example 6 without added fiber, it shows stronger vibration, indicating that the fiber has a stronger interaction with the gel skeleton surface.
[0112] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a lanthanum zirconate / silicon dioxide composite aerogel, characterized in that: The steps include: S1: Using lanthanum nitrate hexahydrate and zirconium nitrate pentahydrate as precursors and propylene oxide as catalyst, LZ sol was obtained in anhydrous ethanol solvent; S2: Using tetraethyl orthosilicate as a precursor and hydrochloric acid as a catalyst, hydrolysis is carried out in ethanol and water solvents to obtain SiO2 sol; S3: dropping the obtained SiO2 sol into the LZ sol to obtain a mixed solution, and dropping the mixed solution dropwise into a propylene oxide gel accelerator to obtain an LZS sol; S4: immersing the pretreated fiber in the LZS sol or evenly dropping the prepared LZS sol on the fiber until it is fully soaked, and applying a certain pressure to the fiber through a mold, and then standing in an oven to obtain FLZS gel; S5: FLZS gel is aged and supercritically dried to obtain FLZS composite aerogel.
2. The method for preparing the lanthanum zirconate / silicon dioxide composite aerogel according to claim 1, characterized in that: In step S1, the molar ratio of lanthanum nitrate hexahydrate, zirconium nitrate pentahydrate, propylene oxide and ethanol is 1:1:2:
50.
3. The method for preparing the lanthanum zirconate / silicon dioxide composite aerogel according to claim 1, characterized in that: In step S2, the molar ratio of ethyl orthosilicate, ethanol and water is 1:35:2; the molar ratio of ethyl orthosilicate and hydrochloric acid is 5:
10. -4 , the mass fraction of the hydrochloric acid is 0.05wt%.
4. The method for preparing the lanthanum zirconate / silicon dioxide composite aerogel according to claim 1, characterized in that: The molar ratio of propylene oxide to lanthanum nitrate hexahydrate added dropwise in step S3 is 1:1; the molar fraction of SiO2 added to the mixed solution is 0% to 20%.
5. The method for preparing the lanthanum zirconate / silicon dioxide composite aerogel according to claim 1, characterized in that: The fiber in step S4 is selected from any one of glass fiber, quartz fiber and basalt fiber; the size of the fiber is 6cm×6cm×5mm, and the mass fraction of the fiber is 40% to 80%.
6. The method for preparing the lanthanum zirconate / silicon dioxide composite aerogel according to claim 1, characterized in that: The fiber pretreatment method in step S4 is: The fiber was immersed in 0.2 mol / L hydrochloric acid and subjected to ultrasonic oscillation for 2 h, repeated 2 to 3 times, and then taken out and rinsed with ethanol for 2 to 3 times and dried.
7. The method for preparing the lanthanum zirconate / silicon dioxide composite aerogel according to claim 1, characterized in that: The pressure applied in step S4 is less than 0.5 MPa.
8. The method for preparing the lanthanum zirconate / silicon dioxide composite aerogel according to claim 1, characterized in that: The supercritical drying method in step S5 is as follows: using ethanol as the supercritical drying medium, pre-filling nitrogen so that the pressure in the kettle is not less than 2MPa, raising the temperature in the kettle to 270°C at a heating rate of 1°C / min, keeping warm for 2h until the pressure in the kettle is 8-10Mpa, turning on the water cooling device, slowly releasing the pressure in the kettle to normal pressure, passing N2 into the kettle for purge, and cooling to room temperature to obtain FLZS aerogel.
9. The method for preparing the lanthanum zirconate / silicon dioxide composite aerogel according to any one of claims 1 to 8, characterized in that: The specific steps include: 1) Add lanthanum nitrate hexahydrate, zirconium nitrate pentahydrate and ethanol into a beaker in proportion, stir in a stirring pot at 60° C. until clear and transparent, and let stand at room temperature to obtain a mixed solution; 2) adding propylene oxide dropwise into the mixed sol obtained in step 1), and stirring evenly to obtain LZ sol; 3) Add tetraethyl orthosilicate, ethanol and water in a three-necked flask in proportion, stir mechanically for 15 minutes, add hydrochloric acid dropwise through a constant pressure funnel, stir for 120 minutes, and after stirring, seal and stand at room temperature for 24 hours to allow the hydrolysis reaction to proceed fully and slowly, thereby obtaining SiO2 sol; 4) adding the SiO2 sol obtained in step 3) dropwise into the LZ sol obtained in step 2), and stirring evenly to obtain a mixed solution; 5) adding propylene oxide dropwise into the mixed solution obtained in step 4), and stirring to obtain LZS sol; 6) completely immersing the pretreated fiber in the LZS sol obtained in step 5) or evenly dropping the prepared LZS sol on the fiber until it is fully soaked, and applying a certain pressure to the fiber through a mold, and then standing in an oven at 60° C. to obtain FLZS gel; 7) The FLZS gel obtained in step 6) is sealed and aged at room temperature for 72 hours and then supercritically dried to obtain a block FLZS composite aerogel.
10. A lanthanum zirconate / silicon dioxide composite aerogel, characterized in that: The lanthanum zirconate / silicon dioxide composite aerogel is prepared by the preparation method of any one of claims 1 to 8.
Citation Information
Patent Citations
Rare earth-doped silicon dioxide aerogel, and preparation method therefor and use thereof
WO2023040965A1