Inorganic calcium salt doped modified silicon dioxide aerogel composite fiber felt heat insulation material and preparation method thereof

By introducing inorganic calcium salts into silica aerogels, it solves the problems of low efficiency and poor compatibility of modifiers in high-temperature environments, and achieves low density , low thermal conductivity and high strength thermal insulation effect, suitable for high temperature thermal insulation and energy saving fields.

CN118908692AInactive Publication Date: 2024-11-08TIANJIN UNIV

Patent Information

Application Number
CN202411156653.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional thermal insulation materials exhibit low efficiency and instability in high temperature environments, and the introduced modifiers have poor compatibility and corrosive ion problems, which limits their application in the field of high temperature insulation.

Method used

The silica aerogel composite fiber felt material modified with inorganic calcium salt doping, and the introduction of inorganic calcium salts such as calcium sulfate, calcium phosphate, calcium oxalate or calcium carbonate into the silica aerogel to form high temperature and stable Low thermal conductivity insulating material uses refractory fiber support and mesoporous silica aerogel filler to maintain the nanomesoporous structure of the aerogel and improve high temperature stability.

Benefits of technology

The material that achieves the thermal insulation performance at a high temperature of 800℃ has low density, low thermal conductivity and high strength, significantly reduces the weight of the thermal insulation layer, and adopts low-cost and environmentally friendly processes, suitable for high-temperature thermal insulation and energy-saving fields. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908692A_ABST
    Figure CN118908692A_ABST
Patent Text Reader

Abstract

The invention relates to an inorganic calcium salt doped modified silicon dioxide aerogel composite fiber felt thermal insulation material and a preparation method thereof. The fiber-reinforced aerogel thermal insulation material is formed by taking refractory fibers as a supporting body and inorganic calcium salt doped and modified mesoporous silica aerogel as a filling body. Taking water glass as a silicon source, and carrying out ion exchange to obtain acidic silicon dioxide sol; the inorganic calcium salt is added into the silica sol, and the inorganic calcium salt doped modified silica aerogel composite fiber felt thermal insulation material is obtained through the steps of pH adjustment, fiber felt dipping, aging, solvent replacement, ethanol supercritical drying and the like. The prepared material has the advantages of low density, low thermal conductivity and better high-temperature stability, the aerogel microstructure in fiber pores is better maintained after the material is subjected to heat treatment at 800 DEG C for 2 hours, and the material still has a complete gel network and a good nano mesoporous structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation technology of nano porous materials, and relates to an inorganic calcium salt doped modified silica aerogel composite fiber felt thermal insulation material and a preparation method thereof. Background Art

[0002] Thermal insulation materials are widely used in aerospace, building energy conservation, chemical metallurgy, industrial pipeline insulation and many other fields, and play a significant role in equipment thermal protection, energy saving and consumption reduction. However, as the application environment becomes more and more harsh (working conditions change from short-term, low temperature to long-term, high temperature), traditional thermal insulation materials (such as aluminum silicate fiber felt, glass fiber, rock wool, foam materials, etc.) have gradually failed to meet new usage requirements due to their high dead weight, poor long-term thermal insulation performance, and thermal conductivity that increases significantly with increasing temperature. It is necessary to develop new high-temperature resistant insulation materials with low density and low thermal conductivity.

[0003] Silica (SiO2) aerogel is a three-dimensional amorphous porous solid material. Due to its special structure with high specific surface area, high porosity and low volume density, it has extremely low thermal conductivity and has broad application prospects in the fields of thermal insulation, energy-saving materials, etc. However, the high-temperature stability of silica aerogel is poor, making it difficult to use in high-temperature environments above 800°C, limiting its application in the field of high-temperature thermal insulation. The patent with publication number CN116791358A adds aluminum sources such as aluminum sec-butoxide to silica sol, and obtains a silicon-aluminum binary hydrolyzate after stirring and mixing. The introduction of the aluminum source causes part of the Si atoms in the Si-O-Si bond in the silica-based aerogel felt to be replaced by Al atoms, forming a Si-O-Al bond with better high-temperature resistance, effectively improving the high-temperature stability of silica aerogel. After heat treatment at 800°C for 2h, the size shrinkage rate of the sample is 10-14%. The patent with publication number CN116692881A adds rare earth salt solution to organosilane precursor, hydrolyzes it in ethanol solvent to obtain rare earth doped silica sol, and then obtains silica aerogel with good high temperature stability through gelation, aging, solvent exchange, drying and other steps. After heat treatment at 1000℃ for 2h, it can still maintain 180m 2 In his 2018 doctoral dissertation "Controllable Preparation and Multifunctionalization of ZrO2-SiO2 Composite Aerogels", He Jian studied the effect of Ca(NO3)2 alcohol solution immersion modification on the high temperature stability of ZrO2-SiO2 aerogels. The results showed that Ca 2+ The modified aerogel reacts with the surface hydroxyl groups of the wet gel to form Si-O-Ca bonds and Zr-O-Ca bonds, which reduces the number of hydroxyl groups on the aerogel surface and the surface activity of the gel particles. The specific surface area of ​​the modified aerogel after heat treatment at 1000°C is 223 m 2 / g, which is significantly higher than the specific surface area of ​​the unmodified aerogel after heat treatment under the same conditions (146m 2 / g), and the high temperature stability was significantly improved.

[0004] From the above, it can be seen that introducing a second phase into silica aerogel for doping modification can effectively improve the high-temperature stability of aerogel and broaden its application field. However, this method also has some problems: on the one hand, the introduced second phase has poor compatibility with silica and high cost; on the other hand, chloride or nitrate solution of the corresponding metal is usually used as a modifier, and corrosive ions will be introduced during the modification, which is not conducive to environmental friendliness and equipment maintenance. Therefore, it is very important to find a second phase modifier that is compatible with silica, low-cost and environmentally friendly to improve the high-temperature stability of silica aerogel. Summary of the invention

[0005] The present invention provides an inorganic calcium salt doped modified silica aerogel composite fiber felt thermal insulation material and a preparation method thereof. The material has the characteristics of good high temperature stability, low thermal conductivity and high strength, and the introduction of the inorganic calcium salt second phase does not affect the three-dimensional network porous structure of the silica aerogel, and effectively improves the high temperature stability of the aerogel fiber felt composite thermal insulation material without affecting the thermal insulation performance thereof. The material has potential application prospects in the field of high temperature thermal insulation and energy saving.

[0006] The specific technical solutions of the present invention are as follows:

[0007] An inorganic calcium salt doped modified silica aerogel composite fiber felt thermal insulation material; a fiber-reinforced aerogel thermal insulation material is formed by using refractory fiber as a support and inorganic calcium salt doped modified mesoporous silica aerogel as a filler.

[0008] The inorganic calcium salt is selected from one of calcium sulfate, calcium phosphate, calcium oxalate or calcium carbonate.

[0009] The fiber felt is one of mullite fiber felt, glass fiber felt, aluminum silicate fiber felt or quartz fiber felt.

[0010] The present invention provides a method for preparing an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material, comprising the following steps:

[0011] (1) Preparation of inorganic calcium salt-doped silica sol

[0012] Using water glass as a raw material, diluting the water glass with deionized water, obtaining an acidic silica sol after ion exchange, adding an inorganic calcium salt to the silica sol, stirring at room temperature for 1 to 24 hours, and obtaining an inorganic calcium salt-doped silica sol;

[0013] (2) Impregnation and gelation

[0014] Adding ammonia water to the sol obtained in step (1) to adjust the pH value to 4-7, impregnating the adjusted sol into the fiber felt, and obtaining a wet gel composite fiber felt after gelation;

[0015] (3) Aging

[0016] An aging solution is prepared using deionized water and the same inorganic calcium salt as in step (1), and the wet gel composite fiber felt obtained in step (2) is placed in the aging solution for aging for 24 to 72 hours;

[0017] (4) Solvent replacement

[0018] After aging, the wet gel composite fiber felt was subjected to solvent replacement with ethanol to replace the water in the pores with ethanol;

[0019] (5) Supercritical drying of ethanol

[0020] After the solvent replacement is completed, the wet gel composite fiber felt is subjected to ethanol supercritical drying to obtain an inorganic calcium salt-doped modified silica aerogel composite fiber felt insulation material.

[0021] The pH of the acidic silica sol in step (1) is 2-4; the concentration of silica in the silica sol is 4-7 wt %; and the amount of inorganic calcium salt added is 0.1-10 mol % of the silica content in the silica sol.

[0022] In the step (2), the concentration of the ammonia water is 0.5 to 1 mol / L.

[0023] In the step (3), the aging liquid is one of a saturated calcium sulfate solution, a saturated calcium phosphate solution, a saturated calcium oxalate solution or a saturated calcium carbonate solution, and the pH value of the aging liquid is 5-10.

[0024] In the step (3), the aging temperature is 30 to 180°C.

[0025] In the step (4), the ethanol solvent is replaced by replacing ethanol every 6 to 12 hours, for 3 to 6 times.

[0026] In the step (5), the supercritical drying conditions of ethanol are: temperature 250-270° C., pressure 7-9 MPa, and the temperature and pressure are maintained under supercritical conditions for 0.5-1 h before releasing the pressure.

[0027] The specific instructions are as follows

[0028] The present invention discloses an inorganic calcium salt doped modified silica aerogel composite fiber felt thermal insulation material; the material is a fiber-reinforced aerogel thermal insulation material with good high-temperature stability, using refractory fiber as a support and inorganic calcium salt doped modified mesoporous silica aerogel as a filler. The present invention reduces the number of active groups on the surface of gel particles and improves the high-temperature stability of the aerogel without changing the nano-mesoporous structure of the aerogel by doping modified silica aerogel with inorganic calcium salt; the material is a refractory fiber as a support and mesoporous silica aerogel as a filler to prepare the inorganic calcium salt doped modified aerogel composite fiber felt thermal insulation material.

[0029] The present invention provides a method for preparing an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material, comprising the following steps:

[0030] (1) Preparation of inorganic calcium salt-doped silica sol

[0031] Using water glass (Na2O·nSiO2) as a raw material, diluting the water glass with deionized water, and obtaining an acidic silica sol after ion exchange, the ion exchange process is shown in formula (1); adding an inorganic calcium salt to the silica sol, stirring at room temperature for 1 to 24 hours, obtaining an inorganic calcium salt-doped silica sol;

[0032] Na2O·nSiO2 + 2H-R → 2Na-R +H2O + nSiO2 (1)

[0033] Wherein, R is an ion exchange resin.

[0034] (2) Impregnation and gelation

[0035] Adding ammonia water to the sol obtained in step (1) to adjust the pH value to 4-7, impregnating the pH-adjusted sol into the fiber felt, and obtaining a wet gel composite fiber felt after gelation;

[0036] (3) Aging

[0037] Deionized water and an inorganic calcium salt are used to prepare an aging solution, wherein the inorganic calcium salt used here is the same as that in step (1), and the wet gel composite fiber felt obtained in step (2) is placed in the aging solution and aged for 24 to 72 hours;

[0038] (4) Solvent replacement

[0039] After aging, the wet gel composite fiber felt was subjected to solvent replacement with ethanol to replace the water in the pores with ethanol;

[0040] (5) Supercritical drying of ethanol

[0041] After the solvent replacement is completed, the wet gel composite fiber felt is subjected to ethanol supercritical drying to obtain an inorganic calcium salt-doped modified silica aerogel composite fiber felt insulation material.

[0042] The present invention uses water glass as a silicon source, obtains an acidic silica sol after ion exchange, adds an inorganic calcium salt to the silica sol, and obtains an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material after the steps of adjusting pH, impregnating fiber felt, aging, solvent replacement, and ethanol supercritical drying. The prepared material has a low density (0.14-0.18 g / cm 3 ), low thermal conductivity (0.017-0.020 W / m·K) and good high-temperature stability. After heat treatment at 800°C for 2h, the aerogel microstructure in the fiber pores remains well maintained, and it still has a complete gel network and good nano-mesoporous structure.

[0043] Beneficial effects of the present invention:

[0044] (1) The present invention introduces inorganic calcium salt into the silica aerogel system for doping modification, which effectively improves the high-temperature stability of the silica aerogel without affecting the nano-mesoporous structure of the aerogel. After heat treatment at 800°C for 2 hours, the aerogel microstructure in the fiber pores is well maintained, and it still has a complete gel network and a good nano-mesoporous structure.

[0045] (2) The inorganic calcium salt doped modified silica aerogel composite fiber felt insulation material of the present invention has a low density (0.14-0.18 g / cm 3 ) and low thermal conductivity (0.017-0.020 W / m·K), excellent thermal insulation effect, and can significantly reduce the weight of the insulation layer.

[0046] (3) The modified aerogel thermal insulation material preparation process provided by the present invention adopts low-cost inorganic silicon source and inorganic calcium salt, and has the advantages of low cost, easy operation, short preparation cycle, and environmental friendliness. It meets the requirements of energy saving, economy, and environmental protection, has potential economic value and application value, and is of great significance for expanding the application scope of high-performance thermal insulation materials, and can meet the requirements of thermal insulation fields such as aviation, aerospace, military and civil use. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a real photo of the inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material prepared by the method of the present invention (Example 1);

[0048] Figure 2 This is a scanning electron microscope image of an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material prepared by the method of the present invention (Example 1);

[0049] Figure 3 This is a scanning electron microscope image of aerogel in an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material prepared by the method of the present invention (Example 2);

[0050] Figure 4 The nitrogen adsorption-desorption curve and pore size distribution curve of the aerogel in the inorganic calcium salt-doped modified silica aerogel composite fiber felt insulation material prepared by the method of the present invention (Example 3);

[0051] Figure 5 The microscopic morphology of aerogel in the fiber pores of the inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material prepared by the method of the present invention (Example 4) after heat treatment at 800° C. for 2 hours;

[0052] Figure 6 The figure is a graph showing the change in specific surface area of ​​the inorganic calcium salt-doped modified silica aerogel composite fiber felt insulation material prepared by the method of the present invention (Example 4) before and after high-temperature heat treatment. DETAILED DESCRIPTION

[0053] The present invention will be further described below in conjunction with the embodiments.

[0054] Example 1

[0055] (1) Using water glass as a raw material, diluting the water glass with deionized water, and obtaining an acidic silica sol after ion exchange, adjusting the pH of the sol to 2, and adjusting the concentration of silica in the sol to 7 wt %; weighing calcium sulfate according to 0.1 mol % of the silica content in the sol and adding it to the sol, stirring at room temperature for 1 hour to make it uniformly mixed, to obtain a calcium sulfate-doped silica sol;

[0056] (2) adding ammonia water to the calcium sulfate-doped silica sol obtained in step (1) to adjust the solution pH to 4, wherein the ammonia concentration is 0.5 mol / L, and impregnating the pH-adjusted sol into the mullite fiber felt, and obtaining a wet gel composite fiber felt after gelation;

[0057] (3) placing the wet gel composite fiber felt in a saturated calcium sulfate solution with a pH of 5 and aging it at 30° C. for 60 h;

[0058] (4) placing the wet gel composite fiber felt in ethanol for solvent replacement, replacing the ethanol every 6 hours for 4 times;

[0059] (5) The wet gel composite fiber felt is subjected to supercritical drying with ethanol. The temperature in the supercritical drying kettle is 250° C. and the pressure is 7 MPa. The temperature and pressure are maintained for 0.5 h and then the pressure is released to obtain a calcium sulfate-doped modified silica aerogel composite mullite fiber felt insulation material.

[0060] The material is intact in appearance, as shown in the attached Figure 1 The combination of fiber and aerogel in this material is shown in the attached Figure 2 As shown in the figure, the microstructure of the aerogel in the material is a porous structure formed by the accumulation of spherical nanoparticles; the density of the composite material is 0.16g / cm 3 The room temperature thermal conductivity is 0.018 W / m·K. After heat treatment at 800℃ for 2h, the aerogel micro-mesoporous structure in the fiber pores remains good, and the specific surface area of ​​the composite material is 198m 2 / g.

[0061] Example 2

[0062] (1) Using water glass as a raw material, diluting the water glass with deionized water, and obtaining an acidic silica sol after ion exchange, adjusting the pH of the sol to 3, and the concentration of silica in the sol to 6 wt %; weighing calcium phosphate according to 1 mol % of the silica content in the sol and adding it to the sol, stirring at room temperature for 24 h to uniformly mix, to obtain a calcium phosphate-doped silica sol;

[0063] (2) adding ammonia water to the calcium phosphate-doped silica sol obtained in step (1) to adjust the pH of the solution to 5, wherein the concentration of ammonia water is 0.7 mol / L, and impregnating the sol after the pH adjustment into the glass fiber mat, and obtaining a wet gel composite fiber mat after gelation;

[0064] (3) placing the wet gel composite fiber felt in a saturated calcium phosphate solution with a pH of 7 and aging it at 80° C. for 72 h;

[0065] (4) placing the wet gel composite fiber felt in ethanol for solvent replacement, replacing the ethanol every 8 hours for 6 times;

[0066] (5) The wet gel composite fiber felt is subjected to supercritical ethanol drying. The temperature in the supercritical drying kettle is 260°C and the pressure is 9 MPa. After maintaining the temperature and pressure for 1 hour, the pressure is released to obtain a calcium phosphate-doped modified silica aerogel composite glass fiber felt insulation material.

[0067] The material has a complete appearance, and the internal fibers are tightly combined with the aerogel; the microstructure of the aerogel is a porous structure formed by the accumulation of spherical nanoparticles. Figure 3 As shown; the density of the composite material is 0.14g / cm 3 The room temperature thermal conductivity is 0.020 W / m·K. After heat treatment at 800℃ for 2h, the aerogel micro-mesoporous structure in the fiber pores remains good, and the specific surface area of ​​the composite material is 216 m 2 / g.

[0068] Example 3

[0069] (1) Using water glass as a raw material, diluting the water glass with deionized water, and obtaining an acidic silica sol after ion exchange, wherein the pH of the sol is 3.5, and the concentration of silica in the sol is 5 wt %; weighing calcium oxalate according to 5 mol % of the silica content in the sol and adding it to the sol, stirring at room temperature for 12 h to uniformly mix, thereby obtaining a calcium oxalate-doped silica sol;

[0070] (2) adding ammonia water to the calcium oxalate-doped silica sol obtained in step (1) to adjust the solution pH to 6, wherein the ammonia concentration is 0.9 mol / L, and impregnating the pH-adjusted sol into aluminum silicate fiber felt, and obtaining a wet gel composite fiber felt after gelation;

[0071] (3) placing the wet gel composite fiber felt in a saturated calcium oxalate solution with a pH of 9 and aging it at 130° C. for 24 h;

[0072] (4) placing the wet gel composite fiber felt in ethanol for solvent replacement, replacing the ethanol every 10 hours for 3 times;

[0073] (5) The wet gel composite fiber felt is subjected to supercritical ethanol drying. The temperature in the supercritical drying kettle is 270°C and the pressure is 8 MPa. After maintaining the temperature and pressure for 0.6 h, the pressure is released to obtain a calcium oxalate-doped modified silica aerogel composite aluminum silicate fiber felt insulation material.

[0074] The material has a complete appearance, and the internal fibers are tightly combined with the aerogel. The microstructure of the aerogel in the material is a porous structure formed by the accumulation of spherical nanoparticles. The nitrogen adsorption and desorption curves and pore size distribution of the aerogel are shown in the attached figure. Figure 4 As shown; the density of the composite material is 0.18g / cm 3 The room temperature thermal conductivity is 0.019 W / m·K. After heat treatment at 800℃ for 2h, the aerogel micro-mesoporous structure in the fiber pores remains good, and the specific surface area of ​​the composite material is 237m 2 / g.

[0075] Example 4

[0076] (1) Using water glass as a raw material, diluting the water glass with deionized water, and obtaining an acidic silica sol after ion exchange, wherein the pH of the sol is 4, and the concentration of silica in the sol is 4 wt %; weighing calcium carbonate according to 10 mol % of the silica content in the sol and adding it to the sol, stirring at room temperature for 6 h to make it uniformly mixed, to obtain a calcium carbonate-doped silica sol;

[0077] (2) adding ammonia water to the calcium carbonate-doped silica sol obtained in step (1) to adjust the pH of the solution to 7, with the ammonia concentration being 1.0 mol / L, and impregnating the pH-adjusted sol into a quartz fiber felt, and obtaining a wet gel composite fiber felt after gelation;

[0078] (3) placing the wet gel composite fiber felt in a saturated calcium carbonate solution with a pH of 10 and aging it at 180°C for 48 hours;

[0079] (4) placing the wet gel composite fiber felt in ethanol for solvent replacement, replacing the ethanol every 12 hours for 5 times;

[0080] (5) The wet gel composite fiber felt is subjected to supercritical drying with ethanol. The temperature in the supercritical drying kettle is 265°C and the pressure is 8.5 MPa. After the temperature and pressure are maintained for 0.8 h, the pressure is released to obtain a calcium carbonate-doped modified silica aerogel composite quartz fiber felt insulation material.

[0081] The appearance of the material is complete, and the internal fibers are tightly combined with the aerogel. The microstructure of the aerogel in the material is a porous structure formed by the accumulation of spherical nanoparticles. The microstructure of the aerogel in the fiber pores after heat treatment at 800℃ for 2h is shown in the attached figure. Figure 5 The specific surface area changes of the composite materials before and after high temperature heat treatment are shown in the attached Figure 6 As shown; the density of the composite material is 0.15g / cm 3 The room temperature thermal conductivity is 0.017 W / m·K. After heat treatment at 800℃ for 2h, the aerogel micro-mesoporous structure in the fiber pores remains good, and the specific surface area of ​​the composite material is 242m 2 / g.

[0082] The present invention proposes an inorganic calcium salt doped modified silica aerogel composite fiber felt insulation material and a preparation method thereof, which has been described through preferred embodiments. It is obvious that relevant technical personnel can modify or appropriately change and combine the technical methods described herein without departing from the content, spirit and scope of the present invention to realize the technology of the present invention. It should be particularly pointed out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all deemed to be included in the spirit, scope and content of the present invention.

Claims

1. An inorganic calcium salt doped modified silica aerogel composite fiber felt thermal insulation material; characterized in that: The fiber-reinforced aerogel thermal insulation material is formed by taking refractory fiber as a support and mesoporous silica aerogel doped and modified by inorganic calcium salt as a filler.

2. The inorganic calcium salt doped modified silica aerogel composite fiber felt thermal insulation material according to claim 1; characterized in that: The inorganic calcium salt is selected from one of calcium sulfate, calcium phosphate, calcium oxalate or calcium carbonate.

3. The inorganic calcium salt doped modified silica aerogel composite fiber felt thermal insulation material according to claim 1; characterized in that: The fiber felt is one of mullite fiber felt, glass fiber felt, aluminum silicate fiber felt or quartz fiber felt.

4. A method for preparing an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material according to claim 1, characterized in that: The steps include: (1) Preparation of inorganic calcium salt-doped silica sol Using water glass as a raw material, diluting the water glass with deionized water, obtaining an acidic silica sol after ion exchange, adding an inorganic calcium salt to the silica sol, stirring at room temperature for 1 to 24 hours, and obtaining an inorganic calcium salt-doped silica sol; (2) Impregnation and gelation Adding ammonia water to the sol obtained in step (1) to adjust the pH value to 4-7, impregnating the adjusted sol into the fiber felt, and obtaining a wet gel composite fiber felt after gelation; (3) Aging An aging solution is prepared using deionized water and the same inorganic calcium salt as in step (1), and the wet gel composite fiber felt obtained in step (2) is placed in the aging solution for aging for 24 to 72 hours; (4) Solvent replacement After aging, the wet gel composite fiber felt was subjected to solvent replacement with ethanol to replace the water in the pores with ethanol; (5) Supercritical drying of ethanol After the solvent replacement is completed, the wet gel composite fiber felt is subjected to ethanol supercritical drying to obtain an inorganic calcium salt-doped modified silica aerogel composite fiber felt insulation material.

5. A method for preparing an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material as claimed in claim 4, characterized in that: The pH of the acidic silica sol in step (1) is 2-4; the concentration of silica in the silica sol is 4-7 wt %; and the amount of inorganic calcium salt added is 0.1-10 mol % of the silica content in the silica sol.

6. A method for preparing an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material as claimed in claim 4, characterized in that: In the step (2), the concentration of the ammonia water is 0.5 to 1 mol / L.

7. A method for preparing an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material as claimed in claim 4, characterized in that: In the step (3), the aging liquid is one of a saturated calcium sulfate solution, a saturated calcium phosphate solution, a saturated calcium oxalate solution or a saturated calcium carbonate solution, and the pH value of the aging liquid is 5-10.

8. A method for preparing an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material as claimed in claim 4, characterized in that: In the step (3), the aging temperature is 30 to 180°C.

9. A method for preparing an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material as claimed in claim 4, characterized in that: In the step (4), the ethanol solvent is replaced by replacing ethanol every 6 to 12 hours, for 3 to 6 times.

10. A method for preparing an inorganic calcium salt-doped modified silica aerogel composite fiber felt thermal insulation material as claimed in claim 4, characterized in that: In the step (5), the supercritical drying conditions of ethanol are: temperature 250-270° C., pressure 7-9 MPa, and the temperature and pressure are maintained under supercritical conditions for 0.5-1 h before releasing the pressure.

Citation Information

Patent Citations

  • Silicon-dioxide aerogel heat insulation composite material and preparation method thereof

    CN103011745A

  • Preparation method of high-temperature-resistant aerogel and aerogel-type porous ceramics

    CN107098352A

  • Method for preparing modified silicon dioxide aerogel material through normal-pressure drying and by external circulation mode

    CN108793173A

  • Aerogel heat insulation composite material and preparation method thereof

    CN118479856A

  • Aerogel blanket and manufacturing method therefor

    WO2021054644A1

Cited By

  • Calcium carbonate thermal insulation material as well as preparation method and application thereof

    CN121202172A

  • A calcium carbonate thermal insulation material, its preparation method and application

    CN121202172B

  • Ultrathin SiO2 aerogel heat insulation composite material with extremely low heat conductivity coefficient as well as preparation method and application of ultrathin SiO2 aerogel heat insulation composite material

    CN122036314A