Anti-oxidation impregnation process of graphite mold for 3d glass mobile phone backboard
Through vacuum and pressurized immersion processes, the impregnation liquid penetrates into the graphite mold to form an antioxidant film, which solves the problem of oxidation and weight loss of graphite mold at high temperatures, significantly improves its antioxidant performance and service life, and is suitable for the production of 3D glass mobile phone back panels. .
Patent Information
- Application Number
- CN202410927914.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
Graphite molds have severe oxidation and weight loss at high temperatures, resulting in a decrease in mechanical properties, limiting their application in an oxidative atmosphere. The existing antioxidant treatment methods are not perfect enough, especially the impregnation process on ultra-fine structural graphite materials has defects.
Using an antioxidant impregnation process, including pretreatment, vacuum impregnation, pressurized impregnation and high-temperature curing steps of graphite mold samples, using impregnation liquid containing phosphoric acid, aluminum dihydrogen phosphate, silica sol and alumina, through vacuum and pressurization The technology allows the impregnation liquid to penetrate deep into the graphite mold to form a mesh structure to prevent the invasion of the oxidation medium.
It effectively improves the high-temperature oxidation resistance of graphite molds, extends its service life, is simple to operate and low cost, is suitable for large-scale industrial production, and significantly improves the overall performance.
Smart Images

Figure CN118894736A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of anti-oxidation impregnation process of graphite moulds, and more specifically to an anti-oxidation impregnation process of graphite moulds used for 3D glass mobile phone back panels. Background Art
[0002] With the advent of the 5G era, the materials of today's mobile phone back panels are becoming more and more diverse. In order to achieve better performance and better appearance, more and more advanced materials are used on mobile phone back panels. Glass, ceramics and some composite materials are developing very rapidly in the field of mobile phone back panels and occupy the market of various brands of mobile phones. Hot bending molds are an important factor affecting the quality of glass. Therefore, during hot bending, the quality of the mold must be guaranteed and the appropriate material must be selected to make the mold. Since the mold needs to work at high temperature for a long time, the mold material needs to have the characteristics of high temperature resistance, good thermal stability, and low thermal expansion coefficient. Graphite molds are widely used in the production of glass back panels because they can meet the above requirements and have low cost.
[0003] The graphite mold for the back panel of the mobile phone begins to oxidize at 450°C and the oxidation gradually intensifies as the temperature increases. When the temperature rises to 800°C, the oxidation rate increases sharply, causing the graphite mold material to fail and become unusable. The weight loss of graphite due to oxidation will significantly reduce the performance of the material. It will oxidize rapidly in an oxidizing environment above 500°C, and the weight loss of oxidation will seriously affect its mechanical properties. If the problem of high-temperature oxidation protection of graphite is not solved, its application as a high-temperature protection or anti-candle material in an oxidizing atmosphere will be greatly limited. Ensuring the stable and long-lasting oxidation resistance of graphite mold materials has become a prerequisite for fully utilizing their performance. The oxidation resistance problem is the key to using graphite materials as long-life high-temperature structural materials.
[0004] There are three methods for anti-oxidation treatment of graphite molds, namely matrix modification, surface coating and solution impregnation. The impregnation method has been widely used because of its simple and convenient operation and low cost. After impregnation, inorganic salts can be closely combined with graphite materials to form an anti-oxidation film, blocking the contact between graphite materials and oxygen, and achieving anti-oxidation function. At present, the impregnation system for the impregnation of ultrafine structure graphite materials is not comprehensive, and the impregnation process is not perfect, which requires further exploration and research.
[0005] Therefore, we proposed an anti-oxidation impregnation process for graphite molds for 3D glass mobile phone back panels to solve the above problems. Summary of the invention
[0006] In order to overcome the above-mentioned defects of the prior art, an embodiment of the present invention provides an anti-oxidation impregnation process for a graphite mold for a 3D glass mobile phone back panel to solve the problems raised in the above-mentioned background technology.
[0007] To achieve the above object, the present invention provides the following technical solution: an anti-oxidation impregnation process for a graphite mold for a 3D glass mobile phone back panel, comprising the following steps:
[0008] Step S1: Pretreatment of the graphite mold sample: polishing, cleaning and drying or burning the graphite mold sample cut into a fixed size by a diamond wire cutting machine;
[0009] Step S2: Vacuum impregnation treatment: put the graphite mold sample pretreated in step S1 into the impregnation reaction kettle, close the valve, tighten the kettle cover with a handle and then evacuate, open the air outlet and use a vacuum pump to evacuate the vacuum degree to above 0.09Mpa, then close the air outlet and open the feed port to automatically suck the impregnation liquid into the impregnation kettle, close the feed port after the impregnation liquid covers the graphite mold sample by more than 1cm, maintain the pressure for 15 minutes and then release the vacuum to complete the preliminary impregnation;
[0010] Step S3: Pressurized impregnation: pour out the impregnation liquid of the graphite mold sample preliminarily impregnated in step S2, introduce inert gas into the air inlet of the impregnation kettle for pressurization, the pressure range is 0.5Mpa-1Mpa, the pressure holding time is 1h, and then the pressure is released and taken out;
[0011] Step S4: high temperature curing: take out the graphite mold sample impregnated in step S3, drain the impregnation liquid remaining on the surface, and wipe it dry with dust-free paper if the viscosity is high;
[0012] The graphite mold sample is then placed in an oven and slowly heated to 70°C-90°C and dried for 4h-6h until the initial drying is completed when the weight loss change is not large. The graphite mold after the initial drying is then transferred to a muffle furnace and gradually heated to 400°C-450°C and kept warm for 30min to complete the final curing.
[0013] In a preferred embodiment, in step S1, the size of the graphite mold sample cut by the diamond wire cutting machine is 20 mm×20 mm×6 mm. After cutting, the surface of the graphite mold sample needs to be cleaned immediately to remove contamination that may be caused during the cutting process.
[0014] In a preferred embodiment, the polishing process in step S1 requires grinding away the surface cutting marks on sandpaper of 400#, 1000#, and 2000# grits respectively and manually polishing to make the surface smoother.
[0015] In a preferred embodiment, the specific steps of the cleaning process described in step S1 are:
[0016] Put the polished graphite mold sample into a beaker filled with deionized water, ultrasonicate for about 5 minutes, take out the sample, wash it, change the water and ultrasonicate for another five minutes. Repeat this operation for about 3 times until the deionized water in the beaker remains transparent, then take it out, wipe it dry, and put it into a beaker filled with ethanol for ultrasonic cleaning for 10 minutes to complete the cleaning. Then transfer the sample to an oven and dry it at 110°C until it no longer loses weight.
[0017] In a preferred embodiment, the burning process described in step S1 is specifically as follows:
[0018] Put the graphite mold sample after preliminary drying into a muffle furnace and heat it up to 300°C at a rate of 3°C / min. During the mold impregnation process, the mold can be directly placed on a hot bending machine and taken out after being baked red, thus completing the burning process.
[0019] In a preferred embodiment, the impregnation liquid in step S2 comprises:
[0020] 10%-20% phosphoric acid, 25%-30% aluminum dihydrogen phosphate, 25%-30% silica sol, 5%-10% aluminum oxide, 10%-20% deionized water, and the sum of the mass percentages of each component is 100%.
[0021] In a preferred embodiment, the specific operation of pressure impregnation in step S3 is:
[0022] After the impregnation liquid in the impregnation kettle is discharged, the kettle cover, the gas outlet and the material inlet and outlet are closed, the gas inlet is opened, and then nitrogen or argon or other inert gases are introduced to gradually increase the pressure in the impregnation kettle to 0.5Mpa-1Mpa, and the gas inlet valve and the gas cylinder valve are closed to maintain the pressure for a while.
[0023] In a preferred embodiment, after the preliminary drying in step S4, the impregnation effect needs to be checked, and the specific process is as follows:
[0024] Weigh the dried impregnated samples separately and compare them with the weight of the unimpregnated samples. Calculate the weight gain rate and density. If the standard is met, proceed to the next step. If the standard is not met, repeat the impregnation until the standard is met before proceeding to the next step.
[0025] In a preferred embodiment, the specific process of the thermal treatment with gradient temperature increase in step S4 is:
[0026] The temperature was increased from room temperature to 200°C at a heating rate of 5°C / min, and kept at 200°C for 1 hour. After the insulation, it was heated to 300°C at a heating rate of 4°C / min and kept at this temperature for 1 hour. Subsequently, the temperature was increased to 400°C-450°C at a heating rate of 3°C / min, and kept at this temperature for 30 minutes. After the insulation, the sample was cooled to room temperature in the furnace to complete the heat treatment and curing.
[0027] Technical effects and advantages of the present invention:
[0028] 1. The impregnation liquid used in the present invention is composed of solution or nanoparticles, which are more suitable for the impregnation process of the graphite mold with ultra-fine structure of 3D glass on the back panel of the mobile phone; the curing temperature and thermal expansion coefficient are reduced by adding silica sol and nano-particle aluminum oxide or magnesium oxide as curing agents; during the impregnation and high-temperature curing process, the effective ingredients in the impregnation liquid will enter the interior of the graphite to form a network structure or a ceramic-like structure, which is more evenly distributed in the micropores of the graphite mold material, thereby preventing or slowing down the invasion speed of the oxidizing medium to achieve an antioxidant effect at high temperature.
[0029] 2. Compared with the substrate modification method and the surface coating method, the impregnation method has the advantages of simple operation, low equipment requirements, easy large-scale industrial production, and significant economic and social benefits.
[0030] 3. For the graphite mold used for the 3D glass on the back panel of the mobile phone, it is difficult to allow the impregnation liquid to enter the micropores inside the graphite mold using the traditional wet impregnation process. Therefore, through vacuum impregnation, pressure impregnation, curing and other processes, the effective components of the impregnation liquid are allowed to penetrate as deeply as possible into the graphite mold, thereby obtaining better overall performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the overall flow chart of the anti-oxidation impregnation process of the 3D glass mobile phone back panel graphite mold sample;
[0032] Figure 2 This is a surface scanning electron micrograph of the impregnated graphite mold sample after high temperature oxidation for 2.5 hours;
[0033] Figure 3 It is the oxidation weight loss rate of the graphite mold sample after impregnation with different impregnation liquids in a mixed gas with an oxygen content of 5% and a nitrogen content of 95% at a temperature of 800℃ at different times. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Reference Figure 1-3 , an anti-oxidation impregnation process for graphite molds for 3D glass mobile phone back panels,
[0036] Example 1
[0037] Prepare the impregnation solution: measure 20 ml of deionized water and transfer it to a beaker, then measure 5 ml of phosphoric acid (purity 85%) and transfer it to the beaker containing deionized water, put the beaker on a stirrer and stir evenly, then weigh 1.6 g of boric acid, 15 g of aluminum dihydrogen phosphate and 3.8 g of sodium tetraborate, and add them to the liquid in the beaker in small amounts and in multiple times. After the addition is completed, move the beaker into a magnetic stirrer and stir at a speed of 250 rpm and a temperature of 70°C. Stir for 2-3 hours until the liquid becomes transparent and set aside;
[0038] The graphite mold was cut and separated by a diamond wire cutting machine, and finally cut into blocks of 20mm×20mm×6mm in size. After cutting, the surface was cleaned of oil stains contaminated during the cutting process, and polished on sandpaper of 400#, 1000#, and 2000# grit. The polished sample was ultrasonically cleaned in deionized water for three times, each for five minutes, and then ultrasonically cleaned with anhydrous ethanol for five minutes and then placed in an oven to dry at 110°C;
[0039] The sample was further pre-treated by placing the sample in a calcination boat in a muffle furnace and gradually heating it to 300°C. After keeping it warm for half an hour, it was cooled with the furnace to remove impurities on the surface and micropores of the graphite mold sample for later use.
[0040] Put the graphite mold sample after pretreatment into the impregnation reactor, tighten the lid, open the air outlet, and evacuate for half an hour. After the vacuum reaches -0.085Mpa or above, close the air outlet. Open the feed port, and the other end of the feed port is connected to the impregnation liquid. Due to the vacuum negative pressure, the impregnation liquid is sucked into the impregnation reactor. After the sample is submerged to a certain height, close the feed port, maintain the pressure for 15 minutes, and vacuum impregnate for a period of time. After the impregnation is completed, open the air inlet to release the pressure. After the pressure release is completed, pour out the impregnation liquid, take out the sample, drain or wipe the residual impregnation liquid on the surface of the sample with a dust-free cloth, and put it in an oven at 70°C for preliminary drying for a period of time to remove moisture;
[0041] The sample impregnation weight gain rate is calculated according to the mass of the graphite mold sample before and after impregnation. The calculation formula is as follows:
[0042]
[0043] In the above formula: ω 增重 is the immersion weight gain rate, in %;
[0044] m0 is the mass of the sample before immersion, in g, and m1 is the mass of the sample after immersion, in g.
[0045] If the weight gain rate is low, repeated dipping and drying operations are required until the weight gain reaches the required level before subsequent curing.
[0046] High temperature curing: put the graphite mold sample into a firing boat and heat it to 200℃ at a heating rate of 5℃ / min from room temperature, keep it at 200℃ for 1h, heat it to 300℃ at 4℃ / min and keep it for 1h, then heat it to 400℃-450℃ at a heating rate of 3℃ / min, keep it for 30min, cool it to room temperature with the furnace and take it out for use;
[0047] The test of the anti-oxidation performance of graphite molds should be as consistent with its use conditions as possible and the operation process should be as simple and safe as possible. Therefore, the anti-oxidation performance of the impregnated graphite sample is characterized by its weight change in a certain period of time in limited static air and at a temperature of 800°C. The specific steps are as follows:
[0048] Take the marked impregnated graphite sample, dry it at 110°C to constant weight, and then cool the sample to room temperature;
[0049] Weigh the sample and mark the initial weight as m1;
[0050] The weighed sample is placed in a firing boat, covered with a lid, and placed in a muffle furnace, and the firing program is set to heat;
[0051] After the muffle furnace cools down, take out the burning boat and the sample, weigh it and mark it as m2. The high-temperature weight loss rate ω of the graphite sample is obtained by formula 1-3:
[0052]
[0053] Wherein, ω is the oxidation weight loss rate of the material, unit %; m1 is the initial mass of the sample of impregnated graphite, unit g; m2 is the mass of the material after high temperature oxidation, unit g;
[0054] The larger the ω value, the greater the oxidation weight loss rate, that is, the material's antioxidant effect is not good. In this experiment, in order to improve the oxidation resistance of graphite, the ω value needs to be as small as possible.
[0055] Example 2
[0056] (1) Preparation of impregnation solution: 10 ml of silica sol (content 30%), 5 ml of phosphoric acid (purity 85%) and 10 ml of aluminum dihydrogen phosphate solution are measured and transferred into a beaker containing deionized water. The beaker is placed on a magnetic stirrer and stirred evenly. Subsequently, 3 g of alumina nanopowder is weighed and added to the liquid in the beaker. The mixture is then heated and stirred at a speed of 250 rpm and a temperature of 70° C. After stirring for 2-3 h, the liquid becomes transparent and is then set aside.
[0057] (2) Vacuum impregnation: Place the graphite mold sample after calcination pretreatment into the impregnation kettle, then evacuate for 30 minutes, introduce the impregnation liquid and maintain the pressure for a period of time for vacuum impregnation. After the impregnation is completed, pour out the impregnation liquid, drain the residual impregnation liquid on the surface of the sample, blow dry with compressed air or wipe off the residual impregnation liquid on the surface with dust-free paper, and place the impregnated sample in an oven for preliminary drying at a drying temperature of 90°C.
[0058] (3) High temperature curing: Place the vacuum impregnated graphite mold sample in a calcining boat and heat it to 200°C at a heating rate of 5°C / min from room temperature, keep it at 200°C for 1 hour, heat it to 300°C at a heating rate of 4°C / min and keep it at that temperature for 1 hour, then heat it to 400-450°C at a heating rate of 3°C / min, keep it at that temperature for 30 minutes, cool it to room temperature in the furnace, and then take it out for use;
[0059] (4) Test of antioxidant properties: The impregnated and cured graphite mold sample was weighed and placed in a calcination boat and then moved into a tubular furnace. A mixed gas with an oxygen content of 5% and a nitrogen content of 95% was introduced. The temperature was raised to 800°C at a rate of 5°C and kept at that temperature for one hour. The mixed gas was then stopped after the furnace was cooled to room temperature. The sample was taken out and weighed for weight loss after oxidation.
[0060] Example 3
[0061] Prepare the impregnation liquid: measure 10 ml of silica sol (content 30%), 5 ml of phosphoric acid (purity 85%) and 10 ml of deionized water and transfer them into a beaker, place the beaker on a magnetic stirrer and stir evenly, then weigh 1.5 g of alumina nanopowder and 1.5 g of sodium tetraborate and add them to the liquid in the beaker, then heat and stir at a speed of 250 rpm and a temperature of 70°C. Stir for 2-3 hours until the liquid becomes transparent and set aside;
[0062] Pretreatment: The cut samples were ultrasonically cleaned to remove oil stains and dried, then polished with sandpaper of different grits until the surface was smooth, and ultrasonically cleaned with deionized water and anhydrous ethanol for multiple times to remove impurities and residual graphite powder, and finally heated in a muffle furnace for 30 minutes and cooled for later use;
[0063] Vacuum impregnation: put the graphite mold sample after calcination pretreatment into the impregnation kettle, then evacuate for 30 minutes, introduce the prepared impregnation liquid, and then maintain the pressure for a period of time for vacuum impregnation. After the impregnation is completed, the impregnation liquid is drawn out, and then the impregnation kettle is closed and the air inlet is opened. Inert gas is filled and pressurized to 2Mpa, and the air inlet is closed. Then the impregnation kettle is heated to 70°C, and after maintaining the pressure for a period of time, the temperature is lowered, opened and the pressure is released, and the impregnated sample is taken out. The residual impregnation liquid on the surface of the sample is removed with dust-free paper, and it is preliminarily dried in an oven. Then the graphite mold sample after vacuum and pressure impregnation is placed in a calcination boat, and the room temperature is heated to 200°C at a heating rate of 5°C / min, and it is kept at 200°C for 1h. After the insulation is completed, it is heated to 300°C at 4°C / min and kept for 1h, and then it is heated to 400-450°C at a heating rate of 3°C / min. After keeping the temperature for 30min, it is cooled to room temperature with the furnace and taken out for use;
[0064] Test of antioxidant performance: weigh the impregnated and cured graphite mold sample, put it into a burning boat and then move it into a tubular furnace. Pass a mixed gas with an oxygen content of 5% and a nitrogen content of 95%. Heat it to 800℃ at a rate of 5℃ and keep it warm for one hour. Then cool it to room temperature with the furnace and stop passing the mixed gas. Take out the sample, weigh the mass after oxidation, and calculate the weight loss rate.
[0065] like Figure 3 As shown, antioxidant A is composed of phosphate as the main component, antioxidant B is composed of silicate as the main component, and antioxidant C is composed of phosphoric acid and borate as the main components. Under the above-mentioned oxidation conditions, the antioxidant properties of the samples after immersion are greatly improved, among which antioxidant B has the best antioxidant effect.
[0066] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An anti-oxidation impregnation process for a graphite mold for a 3D glass mobile phone back panel, characterized in that; The following steps are involved: Step S1: Pretreatment of the graphite mold sample: polishing, cleaning and drying or burning the graphite mold sample cut into a fixed size by a diamond wire cutting machine; Step S2: Vacuum impregnation treatment: put the graphite mold sample pretreated in step S1 into the impregnation reaction kettle, close the valve, tighten the kettle cover with a handle and then evacuate, open the air outlet and use a vacuum pump to evacuate the vacuum degree to above 0.09Mpa, then close the air outlet and open the feed port to automatically suck the impregnation liquid into the impregnation kettle, close the feed port after the impregnation liquid covers the graphite mold sample by more than 1cm, maintain the pressure for 15 minutes and then release the vacuum to complete the preliminary impregnation; Step S3: Pressurized impregnation: pour out the impregnation liquid of the graphite mold sample preliminarily impregnated in step S2, introduce inert gas into the air inlet of the impregnation kettle for pressurization, the pressure range is 0.5Mpa-1Mpa, the pressure holding time is 1h, and then the pressure is released and taken out; Step S4: high temperature curing: take out the graphite mold sample impregnated in step S3, drain the impregnation liquid remaining on the surface, and wipe it dry with dust-free paper if the viscosity is high; The graphite mold sample is then placed in an oven and slowly heated to 70°C-90°C and dried for 4h-6h until the initial drying is completed when the weight loss change is not large. The graphite mold after the initial drying is then transferred to a muffle furnace and gradually heated to 400°C-450°C and kept warm for 30min to complete the final curing.
2. The anti-oxidation impregnation process of a graphite mold for a 3D glass mobile phone back panel according to claim 1, characterized in that: In step S1, the size of the graphite mold sample cut by the diamond wire cutting machine is 20 mm×20 mm×6 mm. After cutting, the surface of the graphite mold sample needs to be cleaned immediately to remove contamination that may be caused during the cutting process.
3. The anti-oxidation impregnation process of a graphite mold for a 3D glass mobile phone back panel according to claim 1, characterized in that: The polishing process in step S1 requires grinding away the surface cutting marks on sandpaper of 400#, 1000#, and 2000# grits respectively and manually polishing to make the surface smoother.
4. The anti-oxidation impregnation process of a graphite mold for a 3D glass mobile phone back panel according to claim 1, characterized in that: The specific steps of the cleaning process described in step S1 are: Put the polished graphite mold sample into a beaker filled with deionized water, ultrasonicate for about 5 minutes, take out the sample, wash it, change the water and ultrasonicate for another five minutes. Repeat this operation for about 3 times until the deionized water in the beaker remains transparent, then take it out, wipe it dry, and put it into a beaker filled with ethanol for ultrasonic cleaning for 10 minutes to complete the cleaning. Then transfer the sample to an oven and dry it at 110°C until it no longer loses weight.
5. The anti-oxidation impregnation process of a graphite mold for a 3D glass mobile phone back panel according to claim 1, characterized in that: The burning process described in step S1 is specifically as follows: Put the graphite mold sample after preliminary drying into a muffle furnace and heat it up to 300°C at a rate of 3°C / min. During the mold impregnation process, the mold can be directly placed on a hot bending machine and taken out after being baked red, thus completing the burning process.
6. The anti-oxidation impregnation process of a graphite mold for a 3D glass mobile phone back panel according to claim 1, characterized in that: The composition of the impregnation liquid in step S2 is: 10%-20% phosphoric acid, 25%-30% aluminum dihydrogen phosphate, 25%-30% silica sol, 5%-10% aluminum oxide, 10%-20% deionized water, and the sum of the mass percentages of each component is 100%.
7. The anti-oxidation impregnation process of a graphite mold for a 3D glass mobile phone back panel according to claim 1, characterized in that: The specific operation of pressure impregnation in step S3 is: After the impregnation liquid in the impregnation kettle is discharged, the kettle cover, the gas outlet and the material inlet and outlet are closed, the gas inlet is opened, and then nitrogen or argon or other inert gases are introduced to gradually increase the pressure in the impregnation kettle to 0.5Mpa-1Mpa, and the gas inlet valve and the gas cylinder valve are closed to maintain the pressure for a while.
8. The anti-oxidation impregnation process of a graphite mold for a 3D glass mobile phone back panel according to claim 1, characterized in that: After the preliminary drying in step S4, the impregnation effect needs to be checked, and the specific process is as follows: Weigh the dried impregnated samples separately and compare them with the weight of the unimpregnated samples. Calculate the weight gain rate and density. If the standard is met, proceed to the next step. If the standard is not met, repeat the impregnation until the standard is met before proceeding to the next step.
9. The anti-oxidation impregnation process of a graphite mold for a 3D glass mobile phone back panel according to claim 1, characterized in that: The specific process of the thermal treatment with gradient temperature increase in step S4 is as follows: The temperature was increased from room temperature to 200°C at a heating rate of 5°C / min, and kept at 200°C for 1 hour. After the insulation, it was heated to 300°C at a heating rate of 4°C / min and kept at this temperature for 1 hour. Subsequently, the temperature was increased to 400°C-450°C at a heating rate of 3°C / min, and kept at this temperature for 30 minutes. After the insulation, the sample was cooled to room temperature in the furnace to complete the heat treatment and curing.
Citation Information
Patent Citations
Anti-oxidation impregnation liquid for graphite mold, and preparation method and application of anti-oxidation impregnation liquid
CN110452019A
Graphite high-temperature antioxidant capable of being quickly dried at normal temperature and application thereof
CN111825476A
Graphite die and maintenance method and application thereof
CN112645738A
High-temperature anti-oxidation graphite product and preparation method thereof
CN114478068A
Oxidation inhibitor for graphite material, graphite product and treatment process of the same graphite product