SEI film smoothing stabilizer, electrolyte and lithium battery
By using SEI film smoothing stabilizer formed by carbon sulfide and main chain C3 compounds with amino groups at both ends in lithium-ion batteries, the problems of unevenness and excessive impedance of SEI film are solved, and uniform deposition of lithium ions and SEI are achieved. The flatness of the membrane improves the cycle stability and service life of lithium-ion batteries.
Patent Information
- Application Number
- CN202410933088.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The SEI film unevenness of existing lithium-ion batteries leads to region-dependent on the diffusion kinetics of lithium-ion, which is too high impedance, which affects cycling stability and safety, and the existing electrolyte additives cannot effectively form a conductive network or smooth SEI film.
Using a SEI film smoothing stabilizer, a ring-forming reaction between carbon sulfide and the main chain C3 compound with amino groups at both ends is formed to form an additive with amide bonds and heteroatom substituent groups. As a component of the electrolyte, it participates in the SEI film. Formulate, regulate its smoothness and density, and reduce dead lithium accumulation sites.
Achieve uniform deposition of lithium ions and flatness of SEI film, delay the growth of lithium dendrites, improve the cycle stability and service life of lithium ion batteries, reduce the precipitation of dead lithium, and enhance the versatility and application of batteries. prospect.
Smart Images

Figure CN118894811A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrolyte additives, and more specifically, to a SEI film smoothing stabilizer, an electrolyte and a lithium battery. Background Art
[0002] The solid electrolyte interface film (SEI) is a passivation layer covering the electrode surface after the electrolyte and the electrode undergo an electrochemical reaction at the solid / liquid interface. It is usually formed in the formation stage of the battery and has the characteristics of conducting ions and isolating electrons. A good SEI film is of great significance for improving the cycle life and safety of lithium-ion batteries (LIBs). The morphology and structure of the SEI film formed by different electrolyte systems are different, and have different degrees of influence on the performance of LIBs. Therefore, it is important to deeply analyze the structure-activity relationship between the morphology and structure of the SEI film and battery performance.
[0003] The inhomogeneity of the SEI film results in region-dependent kinetics for lithium ion diffusion. The slip lines and defects of thicker SEI have slower lithium ion conduction than smooth surfaces. The uneven stripping process will form cracks at the boundary between the slip lines and the smooth surface, which will further collapse and severely damage the SEI. Studies have shown that a multilayer SEI film can be formed by interface regulation methods. The regulated structure has the advantages of being dense and having good thermal stability, but it is easy to cause excessive interface impedance. When the electrode is exposed to the electrolyte, the reduction behavior of all components of the electrolyte shows low selectivity. Therefore, reducing the electrolyte components can make the target reduction reaction more selective. The introduction of film-forming additives such as fluoroethylene carbonate (FEC) will not increase the impedance of the battery while preferentially forming a dense SEI film, but an excessive amount of FEC will increase the charge transfer impedance of the SEI film.
[0004] The Chinese patent with publication number CN111477962A discloses a non-aqueous electrolyte for lithium-ion batteries and a lithium-ion battery containing the non-aqueous electrolyte. The electrolyte additive molecules used in the non-aqueous electrolyte have a high degree of unsaturation and do not have the ability to form a conductive network. They participate in film formation during the formation stage, which will lead to excessively high impedance of the SEI film and poor electron transmission capacity, affecting subsequent normal circulation. The Chinese patent with publication number CN116914257A discloses a non-aqueous electrolyte and a secondary battery thereof. The electrolyte additive molecules used in the non-aqueous electrolyte have no amide bonds, and the formed SEI film has poor conductivity and no amide bonds with Li +Due to the coordination bonding, there are fewer repulsive sites on the SEI film, and the ability to affect the smoothness of the SEI film during the formation stage is poor. The flatness of the formed SEI film is poor, and the problem of dead lithium accumulation in the subsequent cycle process has not been significantly improved. In addition, due to the poor conductivity of lithium iron phosphate (LFP) batteries, the formation of the SEI film is easily affected during the formation stage, the structure is unstable, and the capacity retention rate decays rapidly during normal temperature cycles. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a SEI film smoothing stabilizer, an electrolyte and a lithium battery. The SEI film smoothing stabilizer provided by the present invention is used as an electrolyte additive, can participate in the formation of the SEI film, regulate the smoothness of the SEI film, make it smoother, reduce dead lithium accumulation sites, and improve the later cycle stability.
[0006] The present invention provides a SEI film smoothing stabilizer having a structure shown in Formula A:
[0007]
[0008] Wherein, R1 and R3 are independently selected from H, F or a double bond connected to N, R2 is selected from H, a C1-C4 alkyl group, and R4 and R5 are independently selected from H, an amino group or a space.
[0009] Preferably, R1 is selected from H, F or a double bond connected to N; R2 is selected from H or methyl; R3 is selected from H or F; R4 is selected from H or amino; R5 is selected from H, amino or null.
[0010] Preferably, the formula A is any one of the following formulas A-1 to A-6:
[0011]
[0012] Preferably, the preparation method of the SEI film smoothing stabilizer comprises the following steps:
[0013] The carbon sulfide is subjected to a ring-forming reaction with a main chain C3 compound having amino groups at both ends, and a SEI film smoothing stabilizer is obtained after purification;
[0014] or,
[0015] The carbon sulfide is reacted with a main chain C3 compound with amino groups at both ends to form a ring, and a precursor is obtained after purification; and then a SEI film smoothing stabilizer is obtained after synthesis through N-N bonds or N=C and purification;
[0016] The mass ratio of the main chain C3 compound with amino groups at both ends to carbon sulfide is (0.5-1): (0.3-1);
[0017] The temperature of the cyclization reaction is 65° C. to 90° C., and the time is 1 h to 3 h.
[0018] The present invention also provides an electrolyte comprising a lithium salt, a non-aqueous organic solvent and an electrolyte additive, wherein the electrolyte additive comprises the SEI film smoothing stabilizer described in the above technical solution.
[0019] Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, and lithium difluorobis(oxalatophosphate);
[0020] The lithium salt accounts for 11% to 16% of the weight of the electrolyte.
[0021] Preferably, the non-aqueous organic solvent is an organic ester solvent and / or an ether solvent; the organic ester solvent is one or more of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl trifluoroethyl carbonate, di(2,2,2-trifluoroethyl) carbonate, ethyl formate, ethyl acetate, propyl acetate, and propyl propionate; the ether solvent is one or more of dimethyl ether, diethyl ether, methyl ethyl ether, ethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether;
[0022] The non-aqueous organic solvent accounts for 75% to 87% of the electrolyte by weight.
[0023] Preferably, the electrolyte additive is the SEI film smoothing stabilizer and an auxiliary additive; wherein the auxiliary additive is selected from vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, vinyl sulfate, divinyl sulfate, propylene sulfate, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, 2,4-butane sultone, phenyl methanesulfonate, methylene disulfonate, N-phenylbis(trifluoromethanesulfonyl)imide, triallyl phosphate, tris(trimethylsilane) ) phosphate, trimethyl phosphite, triphenyl phosphite, tris(2,2,2-trifluoroethyl)phosphite, tetramethylmethylene diphosphate, propargyl phosphate, (2-allylphenoxy)trimethylsilane, tris(trimethylsilyl)borate, 1,3,5-triallyl isocyanurate, isocyanoethyl methacrylate, hexamethylene diisocyanate, p-phenylene diisocyanate, 2,4-toluene diisocyanate, adiponitrile, succinonitrile, glutaronitrile, 1,3,6-hexanetrinitrile, 1,2-bis(cyanoethoxy)ethane;
[0024] The SEI film smoothing stabilizer accounts for 1% to 5% of the weight of the electrolyte; the auxiliary additive accounts for 1% to 4% of the weight of the electrolyte.
[0025] The present invention also provides a lithium battery, comprising: a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte is the electrolyte described in the above technical solution.
[0026] Preferably, the active material of the positive electrode is selected from lithium cobalt oxide, lithium manganese oxide, ternary nickel cobalt manganese lithium, lithium nickel manganese oxide, lithium iron phosphate or lithium manganese iron phosphate;
[0027] The active material of the negative electrode is selected from artificial graphite, natural graphite, lithium titanate, metallic lithium, silicon-carbon composite material or silicon oxide.
[0028] The present invention provides a SEI film smoothing stabilizer having a structure shown in Formula A:
[0029]
[0030] Wherein, R1 and R3 are independently selected from H, F or a double bond connected to N, R2 is selected from H, a C1-C4 alkyl group, and R4 and R5 are independently selected from H, an amino group or a space.
[0031] Compared with the prior art, the SEI film smoothing stabilizer provided by the present invention is a leveling additive based on an adsorption-protection mechanism, which can achieve uniform deposition of lithium and alleviate the problem of lithium dendrites; during the deposition process, the additive molecules are preferentially anchored on the surface of the negative electrode material to form a protective molecular layer, and at the same time, the SEI film constructed by the additive molecules can produce a steric hindrance effect on the solvated lithium ions, which effectively delays the random nucleation and uneven deposition of lithium ions participating in the SEI film formation stage.
[0032] At the same time, the additive molecule - Li + The complex can aggregate at the protrusions on the SEI film surface and repel Li + Pushing the lithium ions to the adjacent areas slows down the deposition of lithium ions at the tip of the protrusion and improves the flatness of the SEI film. By utilizing this attraction-repulsion effect, the growth of lithium dendrites can be successfully inhibited, and the disordered growth of the SEI film can also be slowed down in the subsequent cycle stage, thereby improving the cycle performance.
[0033] In addition, the SEI film smoothing stabilizer has organic compounds with heteroatoms and / or polar functional groups, which have greater versatility and broad application prospects due to their adsorption capacity and strong coordination. Therefore, the substituent groups in the molecular formula provided by the present invention include -S groups, halogen substituent groups, nitro groups and other groups with low film-forming resistance. DETAILED DESCRIPTION
[0034] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The present invention provides a SEI film smoothing stabilizer having a structure shown in Formula A:
[0036]
[0037] Wherein, R1 and R3 are independently selected from H, F or a double bond connected to N, R2 is selected from H, a C1-C4 alkyl group, and R4 and R5 are independently selected from H, an amino group or a space.
[0038] In the present invention, R1 is preferably selected from H, F or a double bond connected to N; R2 is preferably selected from H or methyl; R3 is preferably selected from H or F; R4 is preferably selected from H or amino; R5 is preferably selected from H, amino or empty; wherein, when R1 is a double bond connected to N, R5 is empty.
[0039] In the present invention, the formula A is preferably any one of the following formulas A-1 to A-6:
[0040]
[0041] First of all, the additive molecules can assist in the formation of the SEI film in the early stage of the formation due to the presence of the additive, the presence of fluorine-containing groups and unsaturated groups. The inorganic SEI layer containing LiF has a significant improvement in the cycle performance. Due to the characteristics of heteroatom substitution of the additive, the SEI film is compact on the electrode side and loose on the electrolyte side; this may be because the electrode is an excellent conductor of electrons, and the products formed after the electrolyte is effectively reduced on its surface are more densely stacked and present a denser structure; the conductivity of the SEI film containing N and S substitutions is better than that of the SEI film containing only carbon, and a more uniform and dense SEI film structure will be formed. Therefore, the additive can play a role in smoothing the SEI film in the formation stage.
[0042] The present invention provides an additive based on an absorption protection mechanism, which can achieve uniform lithium deposition and alleviate the problem of lithium dendrites. During the formation process, the amide group of the additive preferentially participates in the reaction to form a protective molecular layer on the surface of the negative electrode material, thereby preventing the active material from continuously reacting with the solvent. From a microscopic point of view, the additive molecules occupy the steric hindrance of the planar molecular layer in the formation of the SEI film, which effectively delays the random nucleation and uneven deposition of lithium atoms.
[0043] In addition, the polar groups on the pyrimidine derivatives react with Li + Binding, additive molecule - Li + The complex polarizes the solvent-state Li by repulsion. + Advancing to the adjacent area, this causes the Li anode to repel random lithium ion deposition, especially at the tip of the protrusion. The use of this additive can successfully inhibit the growth of lithium dendrites and effectively extend the service life of the LFP battery. In addition, during the cycle stage, due to the presence of the additive molecules, the occurrence of lithium plating can be weakened, the amount of dead lithium can be reduced, and the cycle performance can be improved.
[0044] In the present invention, the preparation method of the SEI film smoothing stabilizer preferably comprises the following steps:
[0045] The carbon sulfide is subjected to a ring-forming reaction with a main chain C3 compound having amino groups at both ends, and a SEI film smoothing stabilizer is obtained after purification;
[0046] or,
[0047] Carbon sulfide is reacted with a main chain C3 compound with amino groups at both ends to form a ring, and a precursor is obtained after purification; then a SEI film smoothing stabilizer is obtained after synthesis through NN bonds or N=C and purification.
[0048] The present invention has no particular limitation on the sources of the carbon sulfide and the main chain C3 compound with amino groups at both ends, and any commercially available product or laboratory-made product known to those skilled in the art can be used.
[0049] In the present invention, water and ethanol are preferably added during the cyclization reaction; on this basis, the mass ratio of the main chain C3 compound with amino groups at both ends, ethanol, water and carbon sulfide is preferably (0.5-1): (0.5-1): (1-2): (0.3-1).
[0050] In the present invention, the temperature of the cyclization reaction is preferably 65° C. to 90° C., and the time is preferably 1 h to 3 h.
[0051] The present invention also provides an electrolyte comprising a lithium salt, a non-aqueous organic solvent and an electrolyte additive, wherein the electrolyte additive comprises the SEI film smoothing stabilizer described in the above technical solution.
[0052] In the present invention, the lithium salt is preferably selected from one or more of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiODFB), and lithium difluorobis(oxalatophosphate) (LiDODFP), more preferably lithium hexafluorophosphate (LiPF6). The present invention has no particular restrictions on the source of the lithium salt, and commercially available products known to those skilled in the art may be used.
[0053] In the present invention, the lithium salt preferably accounts for 11% to 16% by weight of the electrolyte, and more preferably 13% to 14% by weight.
[0054] In the present invention, the non-aqueous organic solvent is preferably an organic ester solvent and / or an ether solvent; wherein the organic ester solvent is preferably one or more of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl trifluoroethyl carbonate, di(2,2,2-trifluoroethyl) carbonate, ethyl formate, ethyl acetate, propyl acetate, and propyl propionate; the ether solvent is preferably one or more of dimethyl ether, diethyl ether, methyl ethyl ether, ethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether. The present invention has no special restrictions on the source of the non-aqueous organic solvent, and commercially available products known to those skilled in the art can be used. In a preferred embodiment of the present invention, the non-aqueous organic solvent is ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) in a mass ratio of 20%:30%:(29% to 33%). The present invention has no special restrictions on the source of the non-aqueous organic solvent, and commercially available products known to those skilled in the art can be used.
[0055] In the present invention, the non-aqueous organic solvent preferably accounts for 75% to 87% by weight of the electrolyte, and more preferably 79% to 83% by weight.
[0056] In the present invention, the electrolyte additive is preferably the SEI film smoothing stabilizer and the auxiliary additive; wherein the auxiliary additive is preferably selected from vinylene carbonate (VC), vinyl ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, vinyl sulfate (DTD), disulfate, propylene sulfate, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, 2,4-butane sultone, phenyl methanesulfonate, methylene disulfonate, N-phenyl bis(trifluoromethanesulfonyl)imide, triallyl phosphate, tris(trimethylsilane) phosphate, trimethyl phosphite, triphenyl phosphite, tris(2,2,2-trifluoroethyl)imide Phosphate, tetramethylmethylene diphosphate, propargyl phosphate, (2-allylphenoxy) trimethylsilane, tris(trimethylsilane) borate, 1,3,5-triallyl isocyanurate, isocyanoethyl methacrylate, hexamethylene diisocyanate, p-phenylene diisocyanate, 2,4-toluene diisocyanate, adiponitrile, succinonitrile, glutaronitrile, 1,3,6-hexanetrinitrile, 1,2-bis(cyanoethoxy)ethane, one or more, more preferably vinylene carbonate (VC) and vinyl sulfate (DTD); in a preferred embodiment of the present invention, the auxiliary additive is vinylene carbonate (VC) and vinyl sulfate (DTD) in a mass ratio of (3 to 5): 1. The present invention has no special restrictions on the source of the auxiliary additive, and commercially available products known to those skilled in the art can be used.
[0057] In the present invention, the SEI film smoothing stabilizer preferably accounts for 1% to 5% by weight of the electrolyte, more preferably 3%; the auxiliary additive preferably accounts for 1% to 4% by weight of the electrolyte, more preferably 2% to 3%.
[0058] The present invention also provides a lithium battery, comprising: a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte is the electrolyte described in the above technical solution.
[0059] In the present invention, the lithium battery is a lithium battery containing the electrolyte described in the above technical solution, including but not limited to LFP battery, LNMO battery, lithium cobalt oxide (LCO) battery, Li metal negative electrode battery and other related secondary batteries.
[0060] In the present invention, the active material of the positive electrode is preferably selected from lithium cobalt oxide, lithium manganese oxide, ternary nickel cobalt manganese lithium, lithium nickel manganese oxide, lithium iron phosphate or lithium manganese iron phosphate, more preferably lithium iron phosphate (LFP); the present invention has no special restrictions on the source of the active material of the positive electrode, and commercially available products familiar to those skilled in the art can be used.
[0061] In the present invention, the active material of the negative electrode is preferably selected from artificial graphite, natural graphite, lithium titanate, metallic lithium, silicon-carbon composite material or silicon oxide, more preferably artificial graphite and natural graphite. The present invention has no particular restrictions on the source of the active material of the negative electrode, and commercially available products well known to those skilled in the art can be used.
[0062] The present invention obtains a positive electrode sheet by using the above-mentioned positive electrode active material using technical means well known to those skilled in the art. Similarly, a negative electrode sheet is obtained by using the above-mentioned negative electrode active material using technical means well known to those skilled in the art. Finally, the positive and negative electrode sheets are made into soft-pack batteries by technical means well known to those skilled in the art, such as winding, and then the electrolyte described in the above technical scheme is injected into the battery. After formation and capacity separation, a lithium battery is obtained, and its electrical performance is further tested.
[0063] The present invention provides a SEI film smoothing stabilizer having a structure shown in Formula A:
[0064]
[0065] Wherein, R1 and R3 are independently selected from H, F or a double bond connected to N, R2 is selected from H, a C1-C4 alkyl group, and R4 and R5 are independently selected from H, an amino group or a space.
[0066] Compared with the prior art, the SEI film smoothing stabilizer provided by the present invention is a leveling additive based on an adsorption-protection mechanism, which can achieve uniform deposition of lithium and alleviate the problem of lithium dendrites; during the deposition process, the additive molecules are preferentially anchored on the surface of the negative electrode material to form a protective molecular layer, and at the same time, the SEI film constructed by the additive molecules can produce a steric hindrance effect on the solvated lithium ions, which effectively delays the random nucleation and uneven deposition of lithium ions participating in the SEI film formation stage.
[0067] At the same time, the additive molecule - Li + The complex can aggregate at the protrusions on the SEI film surface and repel Li + Pushing the lithium ions to the adjacent areas slows down the deposition of lithium ions at the tip of the protrusion and improves the flatness of the SEI film. By utilizing this attraction-repulsion effect, the growth of lithium dendrites can be successfully inhibited, and the disordered growth of the SEI film can also be slowed down in the subsequent cycle stage, thereby improving the cycle performance.
[0068] In addition, the SEI film smoothing stabilizer has organic compounds with heteroatoms and / or polar functional groups, which have greater versatility and broad application prospects due to their adsorption capacity and strong coordination. Therefore, the substituent groups in the molecular formula provided by the present invention include -S groups, halogen substituent groups, nitro groups and other groups with low film-forming resistance.
[0069] In order to further illustrate the present invention, the following examples are provided for detailed description. In the following examples of the present invention, if no specific conditions are specified, the reaction is carried out according to conventional conditions or conditions recommended by the manufacturer, and if no manufacturer is specified for the reagents or instruments used, all of them are conventional products that can be purchased commercially.
[0070] The raw materials used are as follows:
[0071]
[0072] Preparation Example 1 (Molecular Formula A-1)
[0073] Ethanol and deionized water were added to a 2L three-necked round-bottom flask in a mass ratio of 1:1, and the flask was equipped with a mechanical stirrer, a Claessen adapter, an addition funnel, a reflux condenser and a thermocouple. The raw material of structural formula I-1 was added to the reaction flask in a ratio of 0.5 parts by weight of deionized water and stirred to dissolve, and carbon disulfide was added dropwise at 25°C to 33°C for 35 minutes according to 0.5 parts by weight of deionized water through an addition funnel to obtain a milky white mixture. The temperature was maintained with an ice bath. The reaction mixture was refluxed at 73.4°C for 2 hours to obtain a yellow solution. The reaction mixture was cooled to 25°C in an ice bath, and concentrated HCl (30% mass fraction of concentrated hydrochloric acid, 84 mL) was added dropwise at a temperature of 25°C to 26°C. The reaction mixture was refluxed at 88.4°C for 21 hours, and the reaction solution was cooled to 2°C, and the product was collected by vacuum filtration. The white solid was washed three times with 50 mL of ethanol and water in a volume ratio of 1:1, and dried in vacuo at 40°C to obtain molecular formula A-1 (after testing, purity 89.6%, yield 74.7%) as a white solid.
[0074] The above product is subjected to secondary recrystallization to obtain purified molecular formula A-1, the purity of which reaches battery grade (purity ≥ 99%).
[0075] The reaction formula is as follows:
[0076]
[0077] The mass spectrum data of product A-1 are TOF-MS (ESI) m / z calcd for C4H6F2N2S: 152.16; [M+H]+ found: 152.02.
[0078] Preparation Example 2 (Ratio of Synthetic Reactants)
[0079] Ethanol and deionized water were added to a 2L three-necked round-bottom flask in a mass ratio of 0.5:2, and the flask was equipped with a mechanical stirrer, a Claessen adapter, an addition funnel, a reflux condenser and a thermocouple. The raw material of structural formula I-1 was added to the reaction flask in a ratio of 0.6 parts by weight of deionized water and stirred to dissolve, and carbon disulfide was added dropwise at 25°C to 33°C for 35 minutes according to 0.3 parts by weight of deionized water through an addition funnel to obtain a milky white mixture. The temperature was maintained with an ice bath. The reaction mixture was refluxed at 65°C for 2 hours to obtain a yellow solution. The reaction mixture was cooled to 25°C in an ice bath, and concentrated HCl (30% mass fraction of concentrated hydrochloric acid, 84 mL) was added dropwise at a temperature of 25°C to 26°C. The reaction mixture was refluxed at 78.4°C for 21 hours, and the reaction solution was cooled to 2°C, and the product was collected by vacuum filtration. The white solid was washed three times with 50 mL of ethanol and water in a volume ratio of 1:1, and dried in vacuo at 40°C to obtain molecular formula A-1 (after testing, purity 75.6%, yield 63.2%) as a white solid.
[0080] The above product is subjected to secondary recrystallization to obtain purified molecular formula A-1, the purity of which reaches battery grade (purity ≥ 99%).
[0081] The reaction formula is as follows:
[0082]
[0083] Preparation Example 3 (Ratio of Synthetic Reactants)
[0084] Ethanol and deionized water were added to a 2L three-necked round-bottom flask in a mass ratio of 0.5:2, and the flask was equipped with a mechanical stirrer, a Claessen adapter, an addition funnel, a reflux condenser and a thermocouple. The raw material of structural formula I-1 was added to the reaction flask in a ratio of 0.1 parts by weight of deionized water and stirred to dissolve, and carbon disulfide was added dropwise at 25°C to 33°C for 35 minutes according to 1 part by weight of deionized water through an addition funnel to obtain a milky white mixture. The temperature was maintained with an ice bath. The reaction mixture was refluxed at 90°C for 2 hours to obtain a yellow solution. The reaction mixture was cooled to 25°C in an ice bath, and concentrated HCl (30% mass fraction of concentrated hydrochloric acid, 84 mL) was added dropwise at a temperature of 25°C to 26°C. The reaction mixture was refluxed at 78.4°C for 21 hours, and the reaction solution was cooled to 2°C, and the product was collected by vacuum filtration. The white solid was washed three times with 50 mL of ethanol and water in a volume ratio of 1:1, and dried in vacuo at 40°C to obtain molecular formula A-1 (after testing, purity 80.6%, yield 56.7%) as a white solid.
[0085] The above product is subjected to secondary recrystallization to obtain purified molecular formula A-1, the purity of which reaches battery grade (purity ≥ 99%).
[0086] The reaction formula is as follows:
[0087]
[0088] Preparation Example 4 (Molecular Formula A-2)
[0089] Ethanol and deionized water were added to a 2L three-necked round-bottom flask in a mass ratio of 1:1, and the flask was equipped with a mechanical stirrer, a Claessen adapter, an addition funnel, a reflux condenser and a thermocouple. The raw material of structural formula I-2 was added to the reaction flask in a ratio of 0.5 parts by weight of deionized water and stirred to dissolve, and carbon disulfide was added dropwise at 25°C to 33°C for 35 minutes according to 0.5 parts by weight of deionized water through an addition funnel to obtain a milky white mixture. The temperature was maintained with an ice bath. The reaction mixture was refluxed at 73.4°C for 2 hours to obtain a yellow solution. The reaction mixture was cooled to 25°C in an ice bath, and concentrated HCl (30% mass fraction of concentrated hydrochloric acid, 84 mL) was added dropwise at a temperature of 25°C to 26°C. The reaction mixture was refluxed at 78.4°C for 21 hours, and the reaction solution was cooled to 2°C, and the product was collected by vacuum filtration. The white solid was washed three times with 50 mL of ethanol and water in a volume ratio of 1:1, and dried in vacuo at 40°C to obtain molecular formula A-2 (after testing, purity 85.3%, yield 75.2%) as a white solid.
[0090] The above product is subjected to secondary recrystallization to obtain purified molecular formula A-2, the purity of which reaches battery grade (purity ≥ 99%).
[0091] The reaction formula is as follows:
[0092]
[0093] The mass spectrum data of product A-2 is TOF-MS (ESI) m / z calcd for C4H8N2S: 116.18; [M+H]+ found: 116.04.
[0094] Preparation Example 5 (Molecular Formula A-3)
[0095] Step 1: Add ethanol and deionized water in a mass ratio of 1:1 into a 2L three-necked round-bottom flask equipped with a mechanical stirrer, a Claessen adapter, an addition funnel, a reflux condenser and a thermocouple. The raw material of structural formula I-1 is added to the reaction bottle in a ratio of 0.5 parts by weight of deionized water and stirred to dissolve. Carbon disulfide is added dropwise at 25°C to 33°C for 35 minutes through an addition funnel according to 0.5 parts by weight of deionized water to obtain a milky white mixture. Maintain the temperature with an ice bath. Reflux the reaction mixture at 73.4°C for 2 hours to obtain a yellow solution. Cool the reaction mixture to 25°C in an ice bath, add concentrated HCl (30% mass fraction of concentrated hydrochloric acid, 84mL) dropwise at a temperature of 25°C to 26°C, reflux the reaction mixture at 78.4°C for 21 hours, cool the reaction solution to 2°C, and collect the product by vacuum filtration. The white solid was washed three times with 50 mL of ethanol and water in a volume ratio of 1:1, and dried in vacuo at 40°C to obtain molecular formula A-1 (after testing, purity 89.6%, yield 74.7%) as a white solid.
[0096] The above product is subjected to secondary recrystallization to obtain a purified precursor of molecular formula A-3, which is used as a reactant for the next reaction, and has a purity higher than analytical grade.
[0097] Step 2: Take the product of step 1, the precursor of molecular formula A-3. The synthesis of molecular formula A-3 adopts halogenated trans elimination and follows Saytzeff's rule. The specific reaction is as follows: After the precursor of molecular formula A-3 is mixed with ethanol and potassium hydroxide in a mass ratio of 0.5:1:1, stir it with a stirrer at a speed of 700rpm to 800rpm for 30 minutes. Transfer the mixed reaction solution to a three-necked flask, use ruthenium dioxide as a catalyst (according to the above mass ratio of 0.2, that is, the mass ratio of potassium hydroxide to ruthenium dioxide is 1:0.2), heat in a water bath, the reaction temperature is 50°C, control the heating rate, react for 2 hours, and the temperature fluctuation does not exceed ±2°C. After the reaction, perform vacuum distillation to obtain a product mixed with compound A-3, purify it on a silica gel column, and elute it with ether to obtain the purified molecular formula A-3, and continue to recrystallize until the purity of the additive molecular formula A-3 reaches battery grade (purity ≥99%).
[0098] The reaction formula is as follows:
[0099]
[0100] The mass spectrum data of product A-3 are TOF-MS (ESI) m / z calcd for C4H5FN2S: 132.16; [M+H]+ found: 132.02.
[0101] Preparation Example 6 (Molecular Formula A-4)
[0102] Ethanol and deionized water were added to a 2L three-necked round-bottom flask in a mass ratio of 1:1, and the flask was equipped with a mechanical stirrer, a Claessen adapter, an addition funnel, a reflux condenser and a thermocouple. The raw material of structural formula I-3 was added to the reaction flask in a ratio of 0.5 parts by weight of deionized water and stirred to dissolve, and carbon disulfide was added dropwise at 25°C to 33°C for 35 minutes according to 0.5 parts by weight of deionized water through an addition funnel to obtain a milky white mixture. The temperature was maintained with an ice bath. The reaction mixture was refluxed at 73.4°C for 2 hours to obtain a yellow solution. The reaction mixture was cooled to 25°C in an ice bath, and concentrated HCl (30% mass fraction of concentrated hydrochloric acid, 84 mL) was added dropwise at a temperature of 25°C to 26°C. The reaction mixture was refluxed at 78.4°C for 21 hours, and the reaction solution was cooled to 2°C, and the product was collected by vacuum filtration. The white solid was washed three times with 50 mL of ethanol and water in a volume ratio of 1:1, and dried under vacuum at 40°C to obtain molecular formula A-4 (after testing, purity 83.6%, yield 72.1%) as a white solid.
[0103] The above product is subjected to secondary recrystallization to obtain purified molecular formula A-4, the purity of which reaches battery grade (purity ≥ 99%).
[0104] The reaction formula is as follows:
[0105]
[0106] The mass spectrum data of product A-4 is TOF-MS (ESI) m / z calcd for C5H8F2N2S: 166.04; [M+H]+found: 166.19.
[0107] Preparation Example 7 (Molecular Formula A-5)
[0108] Ethanol and deionized water were added to a 2L three-necked round-bottom flask in a mass ratio of 1:1, and the flask was equipped with a mechanical stirrer, a Claessen adapter, an addition funnel, a reflux condenser and a thermocouple. The raw material of structural formula I-4 was added to the reaction flask in a ratio of 0.5 parts by weight of deionized water and stirred to dissolve, and carbon disulfide was added dropwise at 25°C to 33°C for 35 minutes through an addition funnel in a ratio of 0.5 parts by weight of deionized water to obtain a milky white mixture. The temperature was maintained with an ice bath. The reaction mixture was refluxed at 73.4°C for 2 hours to obtain a yellow solution. The reaction mixture was cooled to 25°C in an ice bath, and concentrated HCl (30% mass fraction of concentrated hydrochloric acid, 84 mL) was added dropwise at a temperature of 25°C to 26°C. The reaction mixture was refluxed at 78.4°C for 21 hours, and the reaction solution was cooled to 2°C, and the product was collected by vacuum filtration. The white solid was washed three times with 50 mL of ethanol and water in a volume ratio of 1:1, and dried under vacuum at 40°C to obtain molecular formula A-5 (after testing, purity 87.4%, yield 71.9%) as a white solid.
[0109] The above product is subjected to secondary recrystallization to obtain purified molecular formula A-5, the purity of which reaches battery grade (purity ≥ 99%).
[0110] The reaction formula is as follows:
[0111]
[0112] The mass spectrum data of product A-5 are TOF-MS (ESI) m / z calcd for C4H7FN2S: 134.03; [M+H]+ found: 134.17.
[0113] Preparation Example 8 (Molecular Formula A-6)
[0114] Step 1: Add ethanol and deionized water in a mass ratio of 1:1 into a 2L three-necked round-bottom flask equipped with a mechanical stirrer, a Claessen adapter, an addition funnel, a reflux condenser and a thermocouple. The raw material of structural formula I-1 is added to the reaction bottle in a ratio of 0.5 parts by weight of deionized water and stirred to dissolve. Carbon disulfide is added dropwise at 25°C to 33°C for 35 minutes through an addition funnel according to 0.5 parts by weight of deionized water to obtain a milky white mixture. Maintain the temperature with an ice bath. Reflux the reaction mixture at 73.4°C for 2 hours to obtain a yellow solution. Cool the reaction mixture to 25°C in an ice bath, add concentrated HCl (30% mass fraction of concentrated hydrochloric acid, 84mL) dropwise at a temperature of 25°C to 26°C, reflux the reaction mixture at 78.4°C for 21 hours, cool the reaction solution to 2°C, and collect the product by vacuum filtration. The white solid was washed three times with 50 mL of ethanol and water in a volume ratio of 1:1, and dried in vacuo at 40°C to obtain molecular formula A-1 (after testing, purity 89.6%, yield 74.7%) as a white solid.
[0115] The above product is subjected to secondary recrystallization to obtain a purified precursor of molecular formula A-6, which is used as a reactant for the next reaction, and the purity reaches analytical grade or above.
[0116] Step 2: Take 0.1 mol of the product molecular formula A-6 precursor of step 1, equipped with a constant pressure drop funnel, a thermometer, and a 250 mL three-necked flask with an exhaust gas absorption device, add dissolved n-methylaminopiperidine (0.1 mol), maintain a low temperature reaction condition of 10°C, and pass 0.2 mol of chlorine for 2 hours. Then add 90 mL of a 15% sodium hydroxide solution drop by drop, stir continuously during the addition process, and maintain the addition process for 0.5 hours. The reaction is completed and the lower layer of oil is collected. After the above reaction product is extracted with toluene and vacuum distilled, concentrated hydrochloric acid is added to the remaining solution under stirring to adjust the pH to 2, and then a rotary evaporation operation is performed to collect the rotary evaporation product at 70°C to 75°C, and recrystallized with ethanol and ethyl acetate in a volume ratio of 1:3 to obtain the product molecular formula A-6 (after testing, the yield is 69.4% and the purity is 88.3%). After continuous purification and recrystallization, it reaches battery grade purity (purity ≥ 99%).
[0117] The reaction formula is as follows:
[0118]
[0119] The mass spectrum data of product A-6 are TOF-MS (ESI) m / z calcd for C4H8F2N4S: 182.04; [M+H]+ found: 182.19.
[0120] Electrolyte preparation:
[0121] Example 1
[0122] In a glove box filled with argon (water content <1ppm, oxygen content <1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 20%:30%:33%, 2wt% VC, 0.5wt% DTD, 1wt% molecular formula A-1 were added, and then 13.5wt% LiPF6 was added. After stirring evenly, the lithium ion battery electrolyte of Example 1 was obtained.
[0123] Example 2
[0124] In a glove box filled with argon (water content <1ppm, oxygen content <1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 20%:30%:32%, 2wt% VC, 0.5wt% DTD, 2wt% of molecular formula A-1 were added, and then 13.5wt% LiPF6 was added. After stirring evenly, the lithium ion battery electrolyte of Example 2 was obtained.
[0125] Example 3
[0126] In a glove box filled with argon (water content <1ppm, oxygen content <1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 20%:30%:31%, 2wt% VC, 0.5wt% DTD, 3wt% molecular formula A-1 were added, and then 13.5wt% LiPF6 was added. After stirring evenly, the lithium ion battery electrolyte of Example 3 was obtained.
[0127] Example 4
[0128] In a glove box filled with argon (water content <1ppm, oxygen content <1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 20%:30%:29%, 2wt% VC, 0.5wt% DTD, 5wt% molecular formula A-1 were added, and then 13.5wt% LiPF6 was added. After stirring evenly, the lithium ion battery electrolyte of Example 4 was obtained.
[0129] Example 5
[0130] In a glove box filled with argon (water <1ppm, oxygen <1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of 20%:30%:31%, 2wt% VC, 0.5wt% DTD, 3wt% molecular formula A-2 are added, and then 13.5wt% LiPF6 is added. After stirring evenly, the lithium ion battery electrolyte of Example 5 is obtained.
[0131] Example 6
[0132] In a glove box filled with argon (water content <1ppm, oxygen content <1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of 20%:30%:31%, 2wt% VC, 0.5wt% DTD, 3wt% molecular formula A-3 are added, and then 13.5wt% LiPF6 is added. After stirring evenly, the lithium ion battery electrolyte of Example 6 is obtained.
[0133] Example 7
[0134] In a glove box filled with argon (water content <1ppm, oxygen content <1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 20%:30%:31%, 2wt% VC, 0.5wt% DTD, 3wt% molecular formula A-4 were added, and then 13.5wt% LiPF6 was added. After stirring evenly, the lithium ion battery electrolyte of Example 7 was obtained.
[0135] Example 8
[0136] In a glove box filled with argon (water content <1ppm, oxygen content <1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of 20%:30%:31%, 2wt% VC, 0.5wt% DTD, 3wt% molecular formula A-5 are added, and then 13.5wt% LiPF6 is added. After stirring evenly, the lithium ion battery electrolyte of Example 8 is obtained.
[0137] Example 9
[0138] In a glove box filled with argon (water content <1ppm, oxygen content <1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of 20%:30%:31%, 2wt% VC, 0.5wt% DTD, 3wt% molecular formula A-6 are added, and then 13.5wt% LiPF6 is added. After stirring evenly, the lithium ion battery electrolyte of Example 9 is obtained.
[0139] Comparative Example 1
[0140] The lithium ion battery electrolyte was obtained by the preparation method provided in Example 1; the difference was: 0wt% of molecular formula A-1.
[0141] Comparative Example 2
[0142] The lithium ion battery electrolyte was obtained by the preparation method provided in Example 3; the difference was that the molecular formula B-1 was used instead of the molecular formula A-1.
[0143] The molecular formula B-1 has the following structure:
[0144]
[0145] Comparative Example 3
[0146] The lithium ion battery electrolyte is obtained by the preparation method provided in Example 3; the difference is that the molecular formula B-2 is used instead of the molecular formula A-1.
[0147] The molecular formula B-2 has the following structure:
[0148]
[0149] Comparative Example 4
[0150] The lithium ion battery electrolyte is obtained by the preparation method provided in Example 3; the difference is that the molecular formula B-3 is used instead of the molecular formula A-1.
[0151] The molecular formula B-3 has the following structure:
[0152]
[0153] Preparation and electrochemical performance testing of lithium batteries:
[0154] The preparation method of lithium battery is as follows:
[0155] (1) Highly compacted lithium iron phosphate material (LFP) was selected as the positive electrode material. LFP, CNTs, and binder were mixed evenly in a ratio of 96:2:2, coated on an aluminum foil current collector, dried in an oven, and rolled on a roller press. The compaction density was 2.5 g / cm 3 , obtain the required positive electrode sheet, and conduct electrolyte wettability test on it;
[0156] (2) Similarly, highly compacted artificial natural composite graphite was selected as the negative electrode material, and graphite, CMC, conductive agent, and binder were mixed evenly in a ratio of 94:1:3:2 to prepare a negative electrode sheet with a compaction density of 1.7 g / cm 3 , and conduct electrolyte wettability test on it;
[0157] (3) The positive and negative electrode sheets were wound into soft-pack batteries, and the electrolytes prepared in Examples 1 to 9 and Comparative Examples 1 to 4 were injected into the batteries. After formation and capacity separation, the electrical performance of the batteries was tested at room temperature of 25° C. Three soft-packs were taken for each test, and the test results were averaged.
[0158] The specific test method is as follows:
[0159] After the soft pack is filled with liquid, the rated capacity is 2.5Ah and the filling coefficient is 6g / Ah. After the filling, it is formed, aged, and divided into volumes. After standing, a three-gram soft pack with a similar capacity is selected to calculate the first effect, test the internal resistance and open-circuit voltage, and then transferred to a constant temperature test room with a fixture, a voltage range of 2.5~3.65V, and a 1C cycle test for 500 weeks.
[0160] The battery is formed according to the following steps: 0.1C constant current charging to 3.0V, 0.2C constant current charging to 3.3V, the formed battery is first aged, then vacuum sealed, and then capacity divided according to the following steps: 0.5C constant current discharge to 2.5V, 0.5C constant current constant voltage charging to 3.65V, constant current discharge to 2.5V, cross-current charging to 3.3V, first effect = (constant current discharge total capacity / (constant current constant voltage charging capacity+formation charging capacity))×100%.
[0161] The test results are shown in Table 1 below.
[0162] Table 1 Test effect data
[0163] Group Special additives First effect / % Capacity / Ah Internal resistance / mΩ 1C cycle 500 cycles capacity retention rate (25℃) Example 1 1wt%A-1 90.88 2.36 2.82 97.53% Example 2 2wt%A-1 91.38 2.39 2.83 97.08% Example 3 3wt%A-1 91.28 2.35 2.84 97.79% Example 4 5wt%A-1 88.66 2.35 3.03 97.40% Example 5 3wt%A-2 86.63 2.36 3.04 96.27% Example 6 3wt%A-3 87.23 2.37 3.02 95.38% Example 7 3wt%A-4 86.22 2.37 3.09 95.37% Example 8 3wt%A-5 86.12 2.33 3.00 96.52% Example 9 3wt%A-6 87.64 2.37 3.03 96.51% Comparative Example 1 0wt%A-1 83.50 2.36 3.07 96.04% Comparative Example 2 3wt%B-1 84.71 2.35 2.91 92.69% Comparative Example 3 3wt%B-2 86.12 2.35 3.16 93.35% Comparative Example 4 3wt%B-3 85.21 2.34 3.06 94.60%
[0164] The experimental results show that:
[0165] By comparing Examples 1 to 4 and Comparative Example 1, we can find that the additive formula A-1 has the best performance at a ratio of 3wt%. By comparing Example 3 with Comparative Example 1, we find that the molecular formula A-1 can improve the cycle retention rate in the normal temperature cycle stage, and the performance is best when the addition amount is 3wt%. According to the capacity and ACR resistance data, we speculate that the reason why the addition amount of 3wt% has the best performance is that the distribution number of C=S double bonds after the molecular formula A-1 is opened and filmed affects the solvation of Li in the subsequent cycle stage. + When the number of C=S double bonds is small, the SEI layer surface is unevenly distributed. + The repulsion effect is weak, which will eventually affect the subsequent room temperature cycle performance. Similarly, when the addition amount is greater than 3wt%, the distribution of C=S double bonds on the SEI film surface will also be uneven, affecting the subsequent Li + Transmission, in summary, the addition ratio of molecular formula A-1 is 3wt% as the optimal addition amount.
[0166] By comparing Example 5 with Example 3, we can find that compared with Molecular Formula A-1 and Molecular Formula A-2, the two mono-fluorinated structures have a greater advantage in capacity retention rate during room temperature cycling. It is speculated that this is because the fluorinated structure participates in film formation during the formation stage to form an SEI film containing a LiF structure. This inorganic structured SEI film has a good Li ion transport function during the cycle. The presence of fluorinated groups and unsaturated groups can assist in the formation of the SEI film. The inorganic SEI layer containing LiF has a significant improvement in the cycle performance. As an excellent conductor of electrons, the product formed by the effective reduction of the electrolyte on its surface is more densely stacked and presents a denser structure.
[0167] By comparing Example 6 with Example 3, we can find that compared with Molecular Formula A-1, Molecular Formula A-3 undergoes a dehalogenation reaction, reduces a fluorine substitution group, increases a double bond structure, and increases the unsaturation of the additive, which results in a certain increase in the membrane impedance ACR performance. It is speculated that the increase in the unsaturation of the additive leads to an increase in film formation impedance. This inference is further supported by the differential discharge capacity. The increase in unsaturated bonds participates in the formation of the SEI film during the formation stage. The increase in the thickness of the SEI film leads to an increase in impedance, which affects the subsequent normal temperature cycle performance. Additives with high unsaturation, such as Molecular Formula A-3, should be avoided as much as possible in the normal temperature cycle of the LFP system.
[0168] By comparing Example 7 with Example 3, we can find that compared with Molecular Formula A-1, Molecular Formula A-4 has an additional F substitution. After the addition of F substitution, it has certain advantages in the initial performance, but performs worse than Molecular Formula A-3 in Example 3 in the impedance and capacity performance stages. It is speculated that the ratio of organic layer SEI to inorganic layer SEI in the components of the SEI film is affected due to polyfluorine substitution. It is speculated that too much F participates in the formation of the SEI film in the formation stage. After the ring opening of Molecular Formula A-4 in the SEI film components, the number of organic components participating in the formation of the SEI film is reduced, which affects the subsequent distribution of C=S double bonds, and the surface of the SEI film is less sensitive to Li + The transmission function is adversely affected, which ultimately leads to the degradation of cycle performance.
[0169] By comparing Example 8 with Example 3, we can find that compared with Formula A-1, Formula A-5 has one less F substitution. The monofluorinated Formula A-5 has a larger polarity due to the asymmetric structure, which is more soluble in the solvated Li + The competitive attraction mechanism for solvent molecules affects the Li + The desolvation process may affect the distribution of the SEI film, causing spike-like protrusions on the surface, affecting the flatness of the SEI film, increasing the overall polarization of the battery, and reducing the room temperature cycle retention rate. The above data show that the molecular formula A-1 with less polarity has a greater improvement in the room temperature cycle performance of LFP.
[0170] By comparing Example 9 with Example 3, we can find that compared with Molecular Formula A-1, Molecular Formula A-6 has two new amino groups added. The introduction of these two amino groups is used to prove that the distribution of nitrogen-containing components in the SEI film mainly plays a role in increasing conductivity, which is mainly manifested in that the capacity of Example 9 has an advantage, but the ACR resistance is low, indicating that Molecular Formula A-6 participates in the capacity contribution of the SEI film, and the construction of the N-containing network increases the conductivity of the SEI layer. The final actual effect is not as good as that of Example 1. It is speculated that this is because the C=S double bond and the -NH2 network structure have a certain conflict, resulting in a decrease in the first efficiency, and affecting the subsequent C=S double bond, The formation of the SEI film smooth layer, ultimately resulting in a low overall room temperature cycle capacity retention rate.
[0171] By comparing Example 3 with Comparative Example 2, it can be found from the comparative data of Molecular Formula A-1 and Molecular Formula B-1 that the presence of the C=S double bond improves the room temperature cycle capacity retention rate of the LFP soft pack, and the unsaturation of Molecular Formula B-1 is also low, which is also affected by the formation of the SEI film. Combined with the ACR data, it can be found that the ACR data of Comparative Example 1 is low, and it is inferred that the SEI film of Molecular Formula B-1 has a lower thickness than that of the SEI film of Molecular Formula A-1. After 500 cycles, the soft pack of Comparative Example 1 with low impedance was disassembled and lithium precipitation was found on its surface, proving that the C=S double bond has a relatively excellent effect in inhibiting the accumulation of dead lithium.
[0172] By comparing Example 3 with Comparative Example 3, and comparing the data of Molecular Formula A-1 with Molecular Formula B-2, it can be found that the position of the C=S double bond also has a relatively large impact on the subsequent cycles. According to the inferred mechanism, in the molecular formula A-1 after ring opening, the C=S double bond should be distributed on the outside of the SEI layer, and the C=S double bond acts as a thorn on the surface of the SEI film to adsorb and repel solvated lithium ions. The structure of the molecular formula B-2 causes the C=S double bond to fail to be arranged as expected during the SEI film formation stage, and cannot play a role in smoothing the SEI film, which ultimately manifests as a decrease in the room temperature cycle retention rate.
[0173] By comparing Example 3 with Comparative Example 4, it can be found from the data of Molecular Formula A-1 and Molecular Formula B-3 that in the presence of C=S double bonds, the removal of N elements eventually leads to the disappearance of the N-containing conductive network in the SEI component, affecting the uniform conductivity of the SEI film. By comparing the room temperature cycle capacity retention rates of the two groups of experiments, it can be found that the construction of the nitrogen-containing conductive network of Molecular Formula A-1 is also a necessary condition for the substance to act as a SEI film smoothener. By ensuring the uniform distribution of electrons, it is ensured that the substance after the ring opening of Molecular Formula A-1 can be evenly distributed on the surface of the graphite layer, and the C=S double bonds are evenly distributed on the outside of the SEI layer, which plays a role in adsorbing and repelling the solvated Li + The ultimate goal is to smooth the SEI film, reduce dead lithium deposition, and improve the capacity retention rate of room temperature cycles.
[0174] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A SEI film smoothing stabilizer, characterized in that: It has the structure shown in formula A: Wherein, R1 and R3 are independently selected from HF or a double bond connected to N, R2 is selected from H, a C1-C4 alkyl group, and R4 and R5 are independently selected from H, or an amino group.
2. The SEI film smoothing stabilizer according to claim 1, characterized in that: The R1 is selected from H or F or a double bond connected to N; the R2 is selected from H or methyl; the R3 is selected from H or F; the R4 is selected from H or amino; and the R5 is selected from H or amino.
3. The SEI film smoothing stabilizer according to claim 1, characterized in that: The formula A is specifically any one of the following formulas A-1 to A-6:
4. The SEI film smoothing stabilizer according to claim 1, characterized in that: The preparation method of the SEI film smoothing stabilizer comprises the following steps: The carbon sulfide is subjected to a ring-forming reaction with a main chain C3 compound having amino groups at both ends, and a SEI film smoothing stabilizer is obtained after purification; or, The carbon sulfide is reacted with a main chain C3 compound with amino groups at both ends to form a ring, and a precursor is obtained after purification; and then a SEI film smoothing stabilizer is obtained after synthesis through N-N bonds or N=C and purification; The mass ratio of the main chain C3 compound with amino groups at both ends to carbon sulfide is (0.5-1): (0.3-1); The temperature of the cyclization reaction is 65° C. to 90° C., and the time is 1 h to 3 h.
5. An electrolyte comprising a lithium salt, a non-aqueous organic solvent and an electrolyte additive, characterized in that: The electrolyte additive comprises the SEI film smoothing stabilizer according to any one of claims 1 to 4.
6. The electrolyte according to claim 5, characterized in that The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, and lithium difluorobis(oxalatophosphate); The lithium salt accounts for 11% to 16% of the weight of the electrolyte.
7. The electrolyte according to claim 5, characterized in that The non-aqueous organic solvent is an organic ester solvent and / or an ether solvent; the organic ester solvent is one or more of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl trifluoroethyl carbonate, di(2,2,2-trifluoroethyl) carbonate, ethyl formate, ethyl acetate, propyl acetate, and propyl propionate; the ether solvent is one or more of dimethyl ether, diethyl ether, methyl ethyl ether, ethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether; The non-aqueous organic solvent accounts for 75% to 87% of the electrolyte by weight.
8. The electrolyte according to claim 5, characterized in that The electrolyte additive is the SEI film smoothing stabilizer and auxiliary additive; wherein the auxiliary additive is selected from vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, vinyl sulfate, divinyl sulfate, propylene sulfate, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, 2,4-butane sultone, phenyl methanesulfonate, methylene disulfonate, N-phenyl bis(trifluoromethanesulfonyl)imide, triallyl phosphate, tris(trimethylsilane)phosphide one or more of esters, trimethyl phosphite, triphenyl phosphite, tris(2,2,2-trifluoroethyl)phosphite, tetramethylmethylene diphosphate, propargyl phosphate, (2-allylphenoxy)trimethylsilane, tris(trimethylsilyl)borate, 1,3,5-triallyl isocyanurate, isocyanoethyl methacrylate, hexamethylene diisocyanate, p-phenylene diisocyanate, 2,4-toluene diisocyanate, adiponitrile, succinonitrile, glutaronitrile, 1,3,6-hexanetrinitrile, and 1,2-bis(cyanoethoxy)ethane; The SEI film smoothing stabilizer accounts for 1% to 5% of the weight of the electrolyte; the auxiliary additive accounts for 1% to 4% of the weight of the electrolyte.
9. A lithium battery comprising: A positive electrode, a negative electrode and an electrolyte, wherein the electrolyte is the electrolyte according to any one of claims 5 to 8.
10. The lithium battery according to claim 9, characterized in that: The active material of the positive electrode is selected from lithium cobalt oxide, lithium manganese oxide, ternary nickel cobalt manganese lithium, lithium nickel manganese oxide, lithium iron phosphate or lithium manganese iron phosphate; The active material of the negative electrode is selected from artificial graphite, natural graphite, lithium titanate, metallic lithium, silicon-carbon composite material or silicon oxide.
Citation Information
Patent Citations
Lithium ion battery non-aqueous electrolyte and lithium ion battery containing non-aqueous electrolyte
CN111477962A
Non-aqueous electrolyte and secondary battery thereof
CN116914257A
Image forming method by silver salt diffusion transfer