Preparation method of light-color-phase high-temperature-aging-resistant C9 petroleum resin

By using a low-temperature prepolymerization process and catalyst A to remove active olefins from C9 petroleum resin, and combining catalyst B and antioxidants, the problems of high bromine value and thermal aging of C9 petroleum resin were solved, enabling low-cost and high-efficiency production of light-colored, high-temperature aging resistant C9 petroleum resin.

CN118894965APending Publication Date: 2024-11-05GUANGDONG XINHUA YUE RESIN TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411122370.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing C9 petroleum resins have high bromine values, dark colors, and are prone to thermal aging during synthesis, which affects the quality of the resin and downstream products. In addition, the hydrogenation catalysts are expensive and easily deactivated, increasing production costs.

Method used

A light-colored, high-temperature aging resistant C9 petroleum resin was prepared by using a low-temperature prepolymerization process and catalyst A to remove carbon-carbon double bond active olefins such as dicyclopentadiene and phenylacetylene, combined with catalyst B and compounded antioxidants, and by controlling the polymerization reaction conditions.

Benefits of technology

This method enables the low-cost preparation of C9 petroleum resin with low bromine value, light color, and resistance to high-temperature aging, making it suitable for large-scale industrial application and improving product yield and thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004995450210000091
    Figure BDA0004995450210000091
  • Figure BDA0004995450210000101
    Figure BDA0004995450210000101
Patent Text Reader

Abstract

The invention relates to the technical field of petroleum resin, in particular to a preparation method of light-color-phase high-temperature-aging-resistant C9 petroleum resin. By designing a prepolymerization process, a C9 petroleum resin basic raw material is subjected to a prepolymerization reaction for 0.5-1 h under the action of a catalyst A and under the low-temperature condition of 5-10 DEG C, and the addition amount of the catalyst A is controlled, so that the light-color-phase high-temperature-aging-resistant C9 petroleum resin is obtained. According to the method, dicyclopentadiene, phenylacetylene and other carbon-carbon double-bond and triple-bond active olefins in a C9 petroleum resin basic raw material are removed, so that the C9 petroleum resin with light hue and low bromine value is obtained, and meanwhile, the yield of a C9 petroleum resin product is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of petroleum resins, in particular to a method for preparing a light-hued high-temperature aging-resistant C9 petroleum resin. Background Art

[0002] C9 petroleum resin is a thermoplastic resin produced by pre-treatment, polymerization, distillation and other processes from the C9 fraction produced by petroleum cracking. It is an oligomer with an average molecular weight between 300 and 3000. It has low acid value, good miscibility, water resistance, ethanol resistance and chemical resistance, chemical stability to acids and alkalis, and good viscosity adjustment and thermal stability. It is widely used in coatings, rubber, adhesives and other industries. Since the C9 raw material for producing petroleum resin contains active olefin components such as dicyclopentadiene and phenylacetylene with carbon-carbon double bonds and carbon-carbon triple bonds, it is easy to cause the synthesized C9 petroleum resin to have high bromine value and dark hue, and it is easy to produce thermal aging during use, which seriously affects the quality of the resin and downstream products. In order to solve this problem, people use the method of hydrorefining the resin to reduce the bromine value of the petroleum resin, such as a two-stage hydrorefining catalyst for C5 and / or C9 petroleum resin disclosed in a Chinese patent (authorization announcement number CN113101967B) and a preparation method and application thereof, and a method for hydrorefining a carbon nine petroleum resin disclosed in a Chinese patent (authorization announcement number CN102618326B), both of which are based on the preparation of C9 petroleum resin by hydrorefining, but the hydrogenation catalyst is expensive and easily deactivated, which increases equipment investment and production costs. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a method for preparing a light-hued high-temperature aging-resistant C9 petroleum resin. The preparation method is simple, requires little equipment investment, effectively reduces production costs, and ensures that the prepared C9 petroleum resin has a low bromine value, light hue and high-temperature aging resistance, and is easy to achieve large-scale industrial promotion.

[0004] The present invention provides a method for preparing a light-hued high-temperature aging-resistant C9 petroleum resin, which comprises at least the following steps:

[0005] S1, stirring and mixing C9 petroleum resin base raw materials to obtain a material, controlling the material temperature and adding catalyst A to carry out a prepolymerization reaction;

[0006] S2. After the prepolymerization reaction is completed, an alkaline aqueous solution is added to terminate the reaction and the liquid is separated to obtain the upper layer of the reaction liquid and washed with water until it is neutral;

[0007] S3, then under the protection of inert gas, the temperature and pressure are controlled to perform reduced pressure distillation to evaporate the unpolymerized carbon nine raw material, and the oligomers formed during the prepolymerization process are removed from the bottom of the kettle;

[0008] S4, stirring and mixing the unpolymerized carbon nine raw material distilled out of S3 and the organic solvent to obtain a material, controlling the material temperature and adding catalyst B to carry out a polymerization reaction;

[0009] S5. After the polymerization reaction is completed, an alkaline aqueous solution is added to terminate the reaction, and the upper layer of the reaction liquid is obtained by separation and washed with water until it is neutral;

[0010] S6. Add an antioxidant to the reaction solution after washing with water, and distill under the protection of an inert gas to obtain a light-colored C9 petroleum resin resistant to high temperature aging.

[0011] As a preferred technical solution, the C9 petroleum resin base material includes at least the following components by mass percentage: 10-35% methyl styrene, 2-5% dicyclopentadiene, 0.5-3.5% phenylacetylene, 15-30% indene, 20-45% methyl indene, and the inevitable C9 petroleum resin components are supplemented to 100%.

[0012] As a preferred technical solution, the prepolymerization reaction temperature is 5-20°C and the time is 0.5-2h.

[0013] Preferably, the prepolymerization reaction temperature is 5-10°C and the time is 0.5-1h.

[0014] As a preferred technical solution, the added amount of the catalyst A is 0.3%-1% by mass of the C9 petroleum resin base material, preferably 0.5%-0.8%.

[0015] As a preferred technical solution, the catalyst A and the catalyst B are both boron trifluoride complexes.

[0016] Preferably, the boron trifluoride complex is selected from one or a combination of boron trifluoride ethyl ether, boron trifluoride monoethylamine, boron trifluoride methanol, boron trifluoride dimethyl carbonate, preferably boron trifluoride ethyl ether.

[0017] As a preferred technical solution, the addition amount of the catalyst B is 0.5%-3% of the mass of the carbon nine raw material, preferably 0.8%-2.5%.

[0018] As a preferred technical solution, the polymerization reaction temperature is 20-40°C and the time is 3-8h.

[0019] Preferably, the polymerization reaction temperature is 20-30°C and the time is 3-5h.

[0020] As a preferred technical solution, the alkaline substance aqueous solution is a sodium hydroxide aqueous solution;

[0021] Preferably, the concentration of the alkaline substance aqueous solution in step S2 is 5-30wt%, preferably 6-20wt%.

[0022] Preferably, the concentration of the alkaline substance aqueous solution in step S5 is 5-30wt%, preferably 6-20wt%.

[0023] As a preferred technical solution, the amount of the alkaline substance aqueous solution added in step S2 is 3-6 times the mass of catalyst A.

[0024] As a preferred technical solution, the amount of the alkaline substance aqueous solution added in step S5 is 3-6 times the mass of catalyst B.

[0025] As a preferred technical solution, the organic solvent is selected from one or a combination of toluene, xylene, trimethylbenzene, n-hexane, and cyclohexane, preferably toluene.

[0026] As a preferred technical solution, the amount of the organic solvent added is 50-200% of the mass of the carbon nine raw material, preferably 50-100%.

[0027] As a preferred technical solution, the antioxidant is a compound antioxidant of antioxidant 1010 and antioxidant 168. Preferably, the mass ratio of antioxidant 1010 to antioxidant 168 in the compound antioxidant is (1-2):1, preferably 1:1;

[0028] As a preferred technical solution, the added amount of the antioxidant is 0.3%-1% of the mass of the carbon nine raw material.

[0029] As a preferred technical solution, the temperature of the reduced pressure distillation is 100-160°C and the pressure is -0.8 to -0.1 MPa.

[0030] As a preferred technical solution, the distillation in step S6 is vacuum distillation, the temperature of the vacuum distillation is 220-260° C., and the pressure is -0.8 to -0.1 MPa.

[0031] As a preferred technical solution, the inert gas is nitrogen.

[0032] As a preferred technical solution, the preparation method of the light-hued high-temperature aging-resistant C9 petroleum resin specifically comprises the following steps:

[0033] S1. Add C9 petroleum resin base material into the reactor, start magnetic stirring, introduce inert gas to replace the air in the container, control the material temperature at 5-10°C with a constant temperature water bath, add catalyst A for prepolymerization, and react for 0.5-1h;

[0034] S2. After the prepolymerization reaction is completed, an alkaline aqueous solution is added to terminate the reaction and the liquid is separated to obtain the upper layer of the reaction liquid and washed with water until it is neutral;

[0035] S3, then under the protection of inert gas, the temperature and pressure are controlled to perform reduced pressure distillation to evaporate the unpolymerized carbon nine raw material, and the oligomers formed during the prepolymerization process are removed from the bottom of the kettle;

[0036] S4, adding the unpolymerized carbon nine raw material and organic solvent distilled out of S3 into the reaction kettle, turning on the magnetic stirring, introducing inert gas to replace the air in the container, controlling the material temperature at 20-40°C with a constant temperature water bath, adding catalyst B for polymerization reaction, and reacting for 3-8h;

[0037] S5. After the polymerization reaction is completed, an alkaline aqueous solution is added to terminate the reaction, and the upper layer of the reaction liquid is obtained by separation and washed with water until it is neutral;

[0038] S6. Add an antioxidant to the reaction solution after washing with water, and distill under the protection of an inert gas to obtain a light-colored C9 petroleum resin resistant to high temperature aging.

[0039] The present invention designs a prepolymerization process, specifically, carries out a prepolymerization reaction of a C9 petroleum resin base raw material under the action of a catalyst A at a low temperature of 5-10° C. for 0.5-1 h, and controls the addition amount of the catalyst A, so as to remove carbon-carbon double bonds and triple bonds active olefins such as dicyclopentadiene and phenylacetylene in the C9 petroleum resin base raw material, thereby obtaining a C9 petroleum resin with a light hue and a low bromine value, while ensuring the yield of the C9 petroleum resin product.

[0040] Furthermore, the present invention ensures the yield of C9 petroleum resin products while avoiding loss of device capacity by comprehensively controlling the selection and addition amount of polymerization catalyst B, as well as the temperature and time of the polymerization reaction, thereby achieving high-quality C9 petroleum resin products at higher production efficiency.

[0041] Furthermore, by introducing a compound antioxidant, especially a compound antioxidant consisting of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, and cooperating with subsequent reduced pressure distillation, the thermal stability of the prepared C9 petroleum resin product is ensured, and the hue and bromine value of the C9 petroleum resin product are further reduced.

[0042] Beneficial Effects

[0043] 1. The present invention provides a method for preparing a light-hued, high-temperature-resistant C9 petroleum resin. The preparation method is simple, requires little equipment investment, and effectively reduces production costs while ensuring that the prepared C9 petroleum resin has a low bromine value, light hue, and high-temperature-resistant aging, making it easy to achieve large-scale industrial promotion.

[0044] 2. The present invention designs a prepolymerization process, specifically, the C9 petroleum resin base raw material is subjected to a prepolymerization reaction for 0.5-1h under the action of catalyst A at a low temperature of 5-10°C, and the amount of catalyst A added is controlled to remove carbon-carbon double bonds and triple bonds active olefins such as dicyclopentadiene and phenylacetylene in the C9 petroleum resin base raw material, thereby obtaining C9 petroleum resin with a light hue and a low bromine value, while ensuring the yield of the C9 petroleum resin product.

[0045] 3. The present invention ensures the yield of C9 petroleum resin products while avoiding the loss of device capacity by comprehensively controlling the selection and addition amount of polymerization reaction catalyst B, as well as the temperature and time of the polymerization reaction, thereby achieving high-quality C9 petroleum resin products at a higher production efficiency.

[0046] 4. The present invention introduces a compound antioxidant, especially a compound antioxidant composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, and cooperates with subsequent reduced pressure distillation to ensure the thermal stability of the prepared C9 petroleum resin product, while further reducing the hue and bromine value of the C9 petroleum resin product.

[0047] 5. The present invention achieves efficient production of C9 petroleum resin products with light hue, low bromine value and good high temperature aging resistance at a lower production cost than the existing hydrorefining process by comprehensively controlling the coordination of various process conditions. DETAILED DESCRIPTION

[0048] Example 1

[0049] Embodiment 1 of the present invention provides a method for preparing a light-hued high-temperature aging-resistant C9 petroleum resin, which specifically comprises the following steps:

[0050] S1. Add 200g of C9 petroleum resin base material into a reactor, start magnetic stirring, introduce inert gas to replace the air in the container, control the material temperature at 5°C with a constant temperature water bath, add 1g of catalyst A for prepolymerization, and react for 1h;

[0051] S2. After the prepolymerization reaction is completed, 100 g of alkaline aqueous solution is added to terminate the reaction and the liquid is separated to obtain the upper layer of the reaction liquid and washed with water until it is neutral;

[0052] S3, then under the protection of inert gas, the temperature and pressure are controlled to perform reduced pressure distillation to evaporate the unpolymerized carbon nine raw material, and the oligomers formed during the prepolymerization process are removed from the bottom of the kettle;

[0053] S4, add 180g of the unpolymerized carbon nine raw material and 90g of the organic solvent distilled out of S3 into the reactor, start magnetic stirring, introduce inert gas to replace the air in the container, control the material temperature at 30°C with a constant temperature water bath, add 3.6g of catalyst B for polymerization reaction, and react for 4h;

[0054] S5. After the polymerization reaction is completed, 90 g of alkaline aqueous solution is added to terminate the reaction and the upper layer of the reaction liquid is obtained by separation and washed with water until it is neutral;

[0055] S6. Add 1 g of antioxidant to the reaction solution after washing with water, and distill under the protection of inert gas to obtain light-colored high-temperature aging-resistant C9 petroleum resin.

[0056] The C9 petroleum resin base material comprises the following components by mass percentage: 20% methyl styrene, 2.5% dicyclopentadiene, 2% phenylacetylene, 25% indene, 30% methyl indene, and the inevitable C9 petroleum resin components are supplemented to 100%.

[0057] The catalyst A and the catalyst B are both boron trifluoride etherate.

[0058] The alkaline substance aqueous solution is a sodium hydroxide aqueous solution.

[0059] The concentration of the alkaline substance aqueous solution in step S2 is 6 wt %.

[0060] The concentration of the alkaline substance aqueous solution in step S5 is 20 wt %.

[0061] The organic solvent is toluene.

[0062] The antioxidant is a compound antioxidant of antioxidant 1010 and antioxidant 168, and the mass ratio of antioxidant 1010 to antioxidant 168 in the compound antioxidant is 1:1.

[0063] The temperature of the reduced pressure distillation in step S3 is 120° C. and the pressure is -0.85 MPa.

[0064] The distillation in step S6 is vacuum distillation, and the temperature of the vacuum distillation is 220° C. and the pressure is -0.85 MPa.

[0065] The inert gas is nitrogen.

[0066] Example 2

[0067] Embodiment 2 of the present invention provides a method for preparing a light-hued high-temperature aging-resistant C9 petroleum resin, which specifically comprises the following steps:

[0068] S1. Add 200 g of C9 petroleum resin base material into a reactor, start magnetic stirring, introduce inert gas to replace the air in the container, control the material temperature at 10° C. with a constant temperature water bath, add 1.6 g of catalyst A for prepolymerization, and react for 0.5 h;

[0069] S2. After the prepolymerization reaction is completed, 100 g of alkaline aqueous solution is added to terminate the reaction and the liquid is separated to obtain the upper layer of the reaction liquid and washed with water until it is neutral;

[0070] S3, then under the protection of inert gas, the temperature and pressure are controlled to perform reduced pressure distillation to evaporate the unpolymerized carbon nine raw material, and the oligomers formed during the prepolymerization process are removed from the bottom of the kettle;

[0071] S4, add 180g of the unpolymerized carbon nine raw material and 180g of the organic solvent distilled out of S3 into the reactor, start magnetic stirring, introduce inert gas to replace the air in the container, control the material temperature at 20°C with a constant temperature water bath, add 1.8g of catalyst B for polymerization reaction, and react for 5h;

[0072] S5. After the polymerization reaction is completed, 90 g of alkaline aqueous solution is added to terminate the reaction and the upper layer of the reaction liquid is obtained by separation and washed with water until it is neutral;

[0073] S6. Add 0.9 g of antioxidant to the reaction solution after washing with water, and distill under the protection of inert gas to obtain light-colored high-temperature aging-resistant C9 petroleum resin.

[0074] The C9 petroleum resin base material comprises the following components by mass percentage: 25% methyl styrene, 3% dicyclopentadiene, 1% phenylacetylene, 20% indene, 35% methyl indene, and the inevitable C9 petroleum resin components are supplemented to 100%.

[0075] The catalyst A and the catalyst B are both boron trifluoride etherate.

[0076] The alkaline substance aqueous solution is a sodium hydroxide aqueous solution.

[0077] The concentration of the alkaline substance aqueous solution in step S2 is 6 wt %.

[0078] The concentration of the alkaline substance aqueous solution in step S5 is 6 wt %.

[0079] The organic solvent is toluene.

[0080] The antioxidant is a compound antioxidant of antioxidant 1010 and antioxidant 168, and the mass ratio of antioxidant 1010 to antioxidant 168 in the compound antioxidant is 1:1.

[0081] The temperature of the reduced pressure distillation in step S3 is 160° C. and the pressure is -0.9 MPa.

[0082] The distillation in step S6 is vacuum distillation, and the temperature of the vacuum distillation is 240° C. and the pressure is -0.9 MPa.

[0083] The inert gas is nitrogen.

[0084] Example 3

[0085] Embodiment 3 of the present invention provides a method for preparing a light-hued high-temperature aging-resistant C9 petroleum resin, which specifically comprises the following steps:

[0086] S1. Add 200 g of C9 petroleum resin base material into a reactor, start magnetic stirring, introduce inert gas to replace the air in the container, control the material temperature at 10° C. with a constant temperature water bath, add 1.2 g of catalyst A for prepolymerization, and react for 1 hour;

[0087] S2. After the prepolymerization reaction is completed, 100 g of alkaline aqueous solution is added to terminate the reaction and the liquid is separated to obtain the upper layer of the reaction liquid and washed with water until it is neutral;

[0088] S3, then under the protection of inert gas, the temperature and pressure are controlled to perform reduced pressure distillation to evaporate the unpolymerized carbon nine raw material, and the oligomers formed during the prepolymerization process are removed from the bottom of the kettle;

[0089] S4, add 180g of the unpolymerized carbon nine raw material and 180g of the organic solvent distilled out of S3 into the reactor, start magnetic stirring, introduce inert gas to replace the air in the container, control the material temperature at 25°C with a constant temperature water bath, add 1.8g of catalyst B for polymerization reaction, and react for 5h;

[0090] S5. After the polymerization reaction is completed, 90 g of alkaline aqueous solution is added to terminate the reaction and the upper layer of the reaction liquid is obtained by separation and washed with water until it is neutral;

[0091] S6. Add 0.5 g of antioxidant to the reaction solution after washing with water, and distill under the protection of inert gas to obtain light-colored high-temperature aging-resistant C9 petroleum resin.

[0092] The C9 petroleum resin base material comprises the following components by mass percentage: 20% methyl styrene, 3.5% dicyclopentadiene, 1.5% phenylacetylene, 20% indene, 35% methyl indene, and the inevitable C9 petroleum resin components are supplemented to 100%.

[0093] The catalyst A and the catalyst B are both boron trifluoride etherate.

[0094] The alkaline substance aqueous solution is a sodium hydroxide aqueous solution.

[0095] The concentration of the alkaline substance aqueous solution in step S2 is 6 wt %.

[0096] The concentration of the alkaline substance aqueous solution in step S5 is 6 wt %.

[0097] The organic solvent is toluene.

[0098] The antioxidant is a compound antioxidant of antioxidant 1010 and antioxidant 168, and the mass ratio of antioxidant 1010 to antioxidant 168 in the compound antioxidant is 1:1.

[0099] The temperature of the reduced pressure distillation in step S3 is 140° C. and the pressure is -0.1 MPa.

[0100] The distillation in step S6 is vacuum distillation, and the temperature of the vacuum distillation is 260° C. and the pressure is -0.9 MPa.

[0101] The inert gas is nitrogen.

[0102] Comparative Example 1

[0103] Comparative Example 1 of the present invention provides a method for preparing C9 petroleum resin, which specifically comprises the following steps:

[0104] S1. Add 200g of C9 petroleum resin base material into a reactor, start magnetic stirring, introduce inert gas to replace the air in the container, control the material temperature at 25°C with a constant temperature water bath, add 2g of catalyst A for polymerization reaction, and react for 5h;

[0105] S2. After the polymerization reaction is completed, 100 g of alkaline aqueous solution is added to terminate the reaction and the liquid is separated to obtain the upper layer of the reaction liquid and washed with water until it is neutral;

[0106] S3. Add 1 g of antioxidant to the reaction solution after washing with water, and distill under the protection of inert gas to obtain C9 petroleum resin.

[0107] The C9 petroleum resin base material comprises the following components by mass percentage: 20% methyl styrene, 2.5% dicyclopentadiene, 2% phenylacetylene, 20% indene, 30% methyl indene, and the inevitable C9 petroleum resin components are supplemented to 100%.

[0108] The catalyst A is boron trifluoride etherate.

[0109] The alkaline substance aqueous solution is a sodium hydroxide aqueous solution.

[0110] The concentration of the alkaline substance aqueous solution in step S2 is 10 wt %.

[0111] The antioxidant is a compound antioxidant of antioxidant 1010 and antioxidant 168, and the mass ratio of antioxidant 1010 to antioxidant 168 in the compound antioxidant is 1:1.

[0112] The distillation in step S3 is vacuum distillation, and the temperature of the vacuum distillation is 220° C. and the pressure is -0.85 MPa.

[0113] The inert gas is nitrogen.

[0114] Comparative Example 2

[0115] Comparative Example 2 of the present invention provides a method for preparing a C9 petroleum resin, which specifically comprises the following steps:

[0116] S1. Add 200g of C9 petroleum resin base material into a reactor, start magnetic stirring, introduce inert gas to replace the air in the container, control the material temperature at 25°C with a constant temperature water bath, add 6g of catalyst A for polymerization reaction, and react for 4h;

[0117] S2. After the polymerization reaction is completed, 100 g of alkaline aqueous solution is added to terminate the reaction and the liquid is separated to obtain the upper layer of the reaction liquid and washed with water until it is neutral;

[0118] S3. Add 0.9 g of antioxidant to the reaction solution after washing with water, and distill under the protection of inert gas to obtain C9 petroleum resin.

[0119] The C9 petroleum resin base material comprises the following components by mass percentage: 20% methyl styrene, 3.5% dicyclopentadiene, 1.5% phenylacetylene, 20% indene, 35% methyl indene, and the inevitable C9 petroleum resin components are supplemented to 100%.

[0120] The catalyst A is boron trifluoride etherate.

[0121] The alkaline substance aqueous solution is a sodium hydroxide aqueous solution.

[0122] The concentration of the alkaline substance aqueous solution in step S2 is 18 wt %.

[0123] The antioxidant is a compound antioxidant of antioxidant 1010 and antioxidant 168, and the mass ratio of antioxidant 1010 to antioxidant 168 in the compound antioxidant is 1:1.

[0124] The distillation in step S3 is vacuum distillation, and the temperature of the vacuum distillation is 260° C. and the pressure is -0.9 MPa.

[0125] The inert gas is nitrogen.

[0126] Performance Testing

[0127] (1) Hue: The C9 petroleum resin products provided in the examples and comparative examples were analyzed using the Gardner colorimetric method of GB / T22295-2008. The instrument used was a PFXI195 colorimeter produced by LOVIBOND in the United Kingdom. The results are shown in Table 1.

[0128] (2) Bromine value: The bromine value of the C9 petroleum resin products provided in the examples and comparative examples was measured using the ASTM D1159 method. The results are shown in Table 1.

[0129] (3) Thermal stability: The thermal stability of a resin represents the ability of the resin to resist high temperature aging. The C9 petroleum resin products provided in the examples and comparative examples were analyzed using the thermal stability test method described in Appendix B of GB / T24138-2022. The hue measurement instrument was a PFXI195 colorimeter produced by LOVIBOND in the United Kingdom. The larger the test result, the worse the resin's ability to resist high temperature aging. The results are shown in Table 1.

[0130] Table 1

[0131]

[0132]

[0133] From the comparison of the results of the embodiments and the comparative examples, it can be seen that the resin synthesized from the carbon nine raw material by the method of the present invention through low-temperature prepolymerization to remove carbon-carbon double bonds and triple bonds of active olefins such as dicyclopentadiene and phenylacetylene in the carbon nine resin raw material has the beneficial effects of light hue, low bromine value and good high temperature aging resistance.

Claims

1. A method for preparing a light-hued high-temperature aging-resistant C9 petroleum resin, characterized in that: At least the following steps are included: S1, stirring and mixing C9 petroleum resin base raw materials to obtain a material, controlling the material temperature and adding catalyst A to carry out a prepolymerization reaction; S2. After the prepolymerization reaction is completed, an alkaline aqueous solution is added to terminate the reaction and the liquid is separated to obtain the upper layer of the reaction liquid and washed with water until it is neutral; S3, then under the protection of inert gas, the temperature and pressure are controlled to perform reduced pressure distillation to evaporate the unpolymerized carbon nine raw material, and the oligomers formed during the prepolymerization process are removed from the bottom of the kettle; S4, stirring and mixing the unpolymerized carbon nine raw material distilled out of S3 and the organic solvent to obtain a material, controlling the material temperature and adding catalyst B to carry out a polymerization reaction; S5. After the polymerization reaction is completed, an alkaline aqueous solution is added to terminate the reaction, and the upper layer of the reaction liquid is obtained by separation and washed with water until it is neutral; S6. Add an antioxidant to the reaction solution after washing with water, and distill under the protection of an inert gas to obtain a light-colored C9 petroleum resin resistant to high temperature aging.

2. The method for preparing the light-hued high-temperature aging-resistant C9 petroleum resin according to claim 1, characterized in that: The C9 petroleum resin base material comprises at least the following components by mass percentage: 10-35% methyl styrene, 2-5% dicyclopentadiene, 0.5-3.5% phenylacetylene, 15-30% indene, 20-45% methyl indene, and the inevitable C9 petroleum resin components are supplemented to 100%.

3. The method for preparing the light-hued high-temperature aging-resistant C9 petroleum resin according to claim 1, characterized in that: The prepolymerization reaction temperature is 5-20°C and the time is 0.5-2h.

4. The method for preparing the light-hued high-temperature aging-resistant C9 petroleum resin according to claim 1, characterized in that: The added amount of the catalyst A is 0.3%-1% of the mass of the C9 petroleum resin base material.

5. The method for preparing the light-hued high-temperature aging-resistant C9 petroleum resin according to claim 1, characterized in that: The polymerization reaction temperature is 20-40° C. and the reaction time is 3-8 hours.

6. The method for preparing the light-hued high-temperature aging-resistant C9 petroleum resin according to claim 1, characterized in that: The added amount of the catalyst B is 0.5%-3% of the mass of the carbon nine raw material.

7. The method for preparing the light-hued high-temperature aging-resistant C9 petroleum resin according to claim 1, characterized in that: The catalyst A and the catalyst B are both boron trifluoride complexes.

8. The method for preparing the light-hued high-temperature aging-resistant C9 petroleum resin according to claim 1, characterized in that: The organic solvent is selected from toluene, xylene, trimethylbenzene, n-hexane, cyclohexane or a combination thereof.

9. The method for preparing the light-hued high-temperature aging-resistant C9 petroleum resin according to claim 1, characterized in that: The temperature of the reduced pressure distillation is 100-160° C., and the pressure is -0.8 to -0.1 MPa.

10. The method for preparing the light-hued high-temperature aging-resistant C9 petroleum resin according to claim 1, characterized in that: The distillation in step S6 is vacuum distillation, the temperature of the vacuum distillation is 220-260° C., and the pressure is -0.8 to -0.1 MPa.

Citation Information

Patent Citations

  • Preparation method of cold polymerized styrene-indene resin

    CN102746459A

  • Light-color C9 cold polymerized petroleum resin product and preparation technology thereof

    CN110183577A

  • New pale hydrocarbon resins of aromatic nature and process for their preparation

    FR2659972A1