Precipitation-preventing and crosslinking-assisting polyolefin grafting material as well as preparation method and application thereof

By using polyolefin elastomer for melt grafting in the photovoltaic adhesive film, a high grafting rate assisted crosslinking agent is prepared, which solves the problem of easy precipitation of crosslinking agents, and improves the crosslinking degree and peeling force of the adhesive film. Reduced costs and is suitable for the production of photovoltaic modules.

CN118894968AActive Publication Date: 2024-11-05NINGBO NENGZHIGUANG NEW MATERIALS TECH

Patent Information

Application Number
CN202411071504.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-05
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The crosslinking agent in the photovoltaic adhesive film is easy to precipitate, causing slippage between the adhesive film and the battery cell and the glass, insufficient cross-linking degree, low inter-layer peeling force, which affects the yield of component preparation. The existing solutions are costly or complex in process. , difficult to apply to large-scale production.

Method used

Using polyolefin elastomer as the matrix, the first monomer and the second monomer are added for melt grafting to prepare a photovoltaic crosslinking agent graft with high grafting rate and low crosslinking, and use initiators and antioxidants. Control the reaction to form a graft material with no crystal point impurities and good transparency, suitable for photovoltaic adhesive films.

Benefits of technology

It realizes the anti-precipitation of the adhesive film, improves the cross-linking degree and resistivity, enhances the transparency and peeling force of the adhesive film, reduces production costs, and is suitable for the long-term preservation and use of POE and EPE adhesive films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004981011610000111
    Figure BDA0004981011610000111
  • Figure BDA0004981011610000112
    Figure BDA0004981011610000112
Patent Text Reader

Abstract

The invention relates to the field of polymerization additives, and provides an anti-precipitation and crosslinking-assisting polyolefin grafting material as well as a preparation method and application thereof in order to solve the problem that a crosslinking-assisting agent of a photovoltaic adhesive film is easy to precipitate. The separation-preventing and crosslinking-assisting polyolefin grafting material comprises the following components: a polyolefin elastomer, a first monomer and a second monomer, the first monomer is selected from at least one of triallyl isocyanurate, triallyl cyanurate and an acrylate compound containing 2-4 carbon-carbon double bonds, and the second monomer is a dialkoxy silane or trialkoxy silane compound containing a carbon-carbon double bond. The polyolefin elastomer is used as a matrix, the first monomer and the second monomer are added for reaction to obtain the photovoltaic assistant crosslinker grafting material with high grafting rate and low crosslinking rate, and the assistant crosslinker grafting material is free of crystal point impurities, good in transparency, high in effective grafting rate and low in melt index drop, and has the characteristics of high volume resistivity, high transparency and the like which are suitable for photovoltaic adhesive films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymerization aids, in particular to a polyolefin graft material capable of preventing precipitation and assisting cross-linking, and a preparation method and application thereof. Background Art

[0002] In recent years, the market share of TOPCon batteries has continued to expand, and more and more industry leaders have turned to TOPCon batteries from PERC battery technology. Along with this, there are changes in battery structure and encapsulation film. The PID of N-type TOPCon batteries mainly occurs on the front side, so POE film or EPE film is required on the front side. However, POE itself is a non-polar material with poor absorption of additives. After being placed for a long time, liquid additives may migrate to the surface of the film (POE film) or the EVA layer (EPE film). This may cause slippage between the film and the battery cell and glass during use (POE film), or insufficient cross-linking of the film and low interlayer peeling force of the E layer and P layer (EPE film), thereby affecting the yield of component preparation.

[0003] Patent CN117925142A absorbs oily liquid additives (such as initiators, co-crosslinking agents, and tackifiers) through the hydrophobic cyclodextrin cavity, removes external moisture after vacuum drying the cyclodextrin hydrogel, retains the internal oily additives, and uses it as a raw material for preparing POE resin to make a POE film, which can prevent the precipitation of liquid additives. However, the preparation and vacuum drying process of cyclodextrin hydrogel is relatively complicated and time-consuming. In addition, the cost of cyclodextrin materials and the equipment and time cost of vacuum drying are high, which increases the overall production cost.

[0004] Patent CN116948560A uses polymer microcapsules to encapsulate organic additives and prevent them from leaching out. However, the microcapsules may break during processing, resulting in leakage of the additives, and the application cost of microcapsule technology is relatively high, which may not be suitable for large-scale production.

[0005] Patent CN117186781A uses a longer alkane structure to increase the compatibility of silane with polyolefin elastomer resin and reduce the risk of precipitation of silane additives, but this method only targets silane additives and fails to avoid the precipitation of other additives (such as co-crosslinking agents). Patent CN115895532A uses a solution grafting method to graft the anti-potential induced decay monomer onto the polyolefin elastomer molecular chain, avoiding the precipitation problem of direct blending, but the solution grafting process is quite complicated and continuous production is difficult.

[0006] Therefore, an economical and effective solution is needed to solve the precipitation problem of photovoltaic cross-linking agents such as ethoxylated trimethylolpropane triacrylate and triallyl cyanurate in POE and EPE films. Summary of the invention

[0007] In order to overcome the problem that the cross-linking agent of photovoltaic film is easy to precipitate, the present invention provides a polyolefin graft material that prevents precipitation and assists cross-linking, and a preparation method and application thereof. A polyolefin elastomer is used as a matrix, and a first monomer and a second monomer are added to react to obtain a photovoltaic cross-linking agent graft material with a high grafting rate and low cross-linking. The cross-linking agent graft material has no crystal point impurities, good transparency, high effective grafting rate, and little melt index reduction. At the same time, it also has the characteristics of high volume resistivity, high transparency, and other characteristics suitable for photovoltaic film.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions: The invention discloses a polyolefin graft material which can prevent precipitation and assist cross-linking, and comprises the following components: a polyolefin elastomer, a first monomer and a second monomer; the first monomer is selected from at least one of triallyl isocyanurate, triallyl cyanurate and acrylic ester compounds containing 2 to 4 carbon-carbon double bonds, and the second monomer is a dialkoxysilane or trialkoxysilane compound containing carbon-carbon double bonds; the sum of the mass of the first monomer and the second monomer is 1 to 10% of the polyolefin elastomer, and the mass ratio of the first monomer to the second monomer is (0.1 to 50):1.

[0009] Preferably, the polyolefin elastomer is one or more polymers produced by copolymerization of ethylene and any C3-C8 olefin (propylene, butene, pentene, hexene, octene), and the melt index of the polyolefin elastomer is 0.5-45g / 10min.

[0010] Preferably, the acrylate compound containing 2-4 carbon-carbon double bonds is selected from the following compounds: trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, ethoxylated glycerol triacrylate, propoxylated glycerol triacrylate, pentaerythritol tetraacrylate, ethoxylated pentaerythritol tetraacrylate, trimethylolpropane tetraacrylate, ditrimethylolpropane tetraacrylate, ditrimethylolpropane tetramethacrylate, propoxylated pentaerythritol tetraacrylate, tricyclopentane dimethanol diacrylate, propoxylated neopentyl glycol diacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, 2-butyl-2-ethyl-1,3-propanediol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, and polyethylene glycol dimethacrylate.

[0011] Preferably, the second monomer is selected from at least one of the following compounds: vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tripropoxysilane, vinyl triisopropoxysilane, vinyl tributoxysilane, vinyl tripentoxysilane, vinyl triphenoxysilane, vinyl tripenzyloxysilane, vinyl trimethylenedioxysilane, vinyl triethylenedioxysilane, vinyl propionyloxysilane, vinyl triacetoxysilane, vinyl tricarboxysilane and other vinyl silanes or (meth) acryloxysilanes such as γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl methyldimethoxysilane, γ-acryloxypropyl trimethoxysilane, and γ-methacryloxypropyl methyldimethoxysilane.

[0012] Preferably, one of the first monomer and the second monomer attracts electrons while the other pushes electrons; the conjugation effect Q value of the second monomer is ≥0.2, more preferably 0.2-1; the Q values ​​of the first monomer and the second monomer differ by more than 0.2, more preferably by more than 0.8.

[0013] As a further preference, the first monomer is triallyl isocyanurate, and the second monomer is γ-methacryloxypropylmethyldimethoxysilane.

[0014] Melt grafting is a suitable method due to its advantages such as simple process and continuous production. The cross-linking aid is grafted into the base resin by melt grafting to prepare an anti-precipitation grafted material. However, the cross-linking aid (the first monomer of the present invention) contains multiple double bonds that can participate in the reaction, which easily induces cross-linking during the grafting process, weakening the fluidity and cross-linking effect in the subsequent processing. Therefore, a method for inhibiting cross-linking during the grafting process is needed. The present invention selects a second monomer with opposite electron-withdrawing (pushing) properties according to the Q and e values ​​of the first monomer. Under the action of the initiator, the second monomer and the first monomer form a more stable free radical, thereby inhibiting the cross-linking reaction of the first monomer.

[0015] Preferably, the mass ratio of the first monomer to the second monomer is (0.25-10):1.

[0016] Preferably, the anti-precipitation and cross-linking polyolefin graft material is composed of the following components: polyolefin elastomer 91.0-97.5wt%, first monomer 1.0-5.0wt%, second monomer 0.5-4.0wt%, initiator 0.08-0.2wt%, antioxidant 0-0.2wt%; the sum of the amounts of each component is equal to 100%.

[0017] Preferably, the initiator is a peroxide initiator, and more preferably at least one of the following compounds: tert-butyl peroxy isopropyl carbonate, 2,5-dimethyl-2,5-(bis-tert-butylperoxy)hexane, tert-butyl peroxy carbonate-2-ethylhexyl ester, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(tert-butylperoxy)butane, tert-butyl peroxy 2-ethylhexyl carbonate, tert-amyl peroxy 2-ethylhexyl carbonate, and tert-butyl peroxy 3,3,5-trimethylhexanoate.

[0018] Preferably, the antioxidant includes at least one of a hindered phenol antioxidant, a phosphite antioxidant and a thioester antioxidant. More preferably, the antioxidant is selected from at least one of the following: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (antioxidant 101), tris[2.4-di-tert-butylphenyl]phosphite (antioxidant 168), tris(nonylphenyl)phosphite, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate octadecyl alcohol; more preferably, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0019] The present invention also provides a method for preparing the anti-precipitation and cross-linking polyolefin graft material, comprising the following steps: mixing the raw material components, extruding and granulating at 85-220°C to obtain pellets; homogenizing and drying the pellets to obtain the polyolefin graft material.

[0020] The anti-precipitation and cross-linking polyolefin grafted material is used for photovoltaic film, and the photovoltaic film is a POE film or an EPE film. The POE layer of the photovoltaic film contains the following components: 1-25wt% of the polyolefin grafted material, 70-98wt% of a polyolefin elastomer and 1-5wt% of an auxiliary agent; the auxiliary agent includes at least one of a cross-linking agent, an auxiliary cross-linking agent, a silane coupling agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a tackifier, and a pigment.

[0021] Preferably, the photovoltaic film is an EPE film, which is composited by an EVA layer, the POE layer and an EVA layer, and the EVA layer contains the following components: 95-99.0wt% EVA resin and 1.0-5.0wt% additives; the additives include at least one of a cross-linking agent, a co-cross-linking agent, a silane coupling agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a tackifier or a pigment.

[0022] Therefore, the beneficial effects of the present invention are as follows: (1) The present invention uses polyolefin elastomer as a matrix, adds a first monomer and a second monomer, selects a suitable initiator, and controls the ratio of each raw material to obtain a photovoltaic co-crosslinking agent grafted material with a high grafting rate and low crosslinking. The co-crosslinking agent grafted material has no crystal point impurities, good transparency, high effective grafting rate, and little melt index reduction. At the same time, it has the characteristics of high volume resistivity and high transparency that are suitable for photovoltaic adhesive films.

[0023] (2) The anti-precipitation and cross-linking film prepared by the present invention has fast vulcanization, high cross-linking degree, high volume resistivity, high light transmittance, and small yellowing value after PCT aging. The additive does not precipitate and the peeling force does not decay after the film is placed for a long time. It has obvious benefits for the long-term storage of the film, the anti-slip of the POE film, and the interlayer peeling of the EPE film. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described below through specific embodiments.

[0025] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the embodiments, unless otherwise specified, are all conventional methods in the art. Unless otherwise specified, parts are all weight parts, temperatures are expressed in ° C or at ambient temperature, and pressures are atmospheric pressure or near atmospheric pressure. There are many variations and combinations of reaction conditions (such as component concentrations, desired solvents, solvent mixtures, temperatures, pressures, and other reaction ranges) and conditions that can be used to optimize the purity and yield of the product obtained by the method, and only reasonable routine experiments will be required to optimize such method conditions.

[0026] Example 1. The anti-precipitation and cross-linking polyolefin graft material is composed of the following components: polyolefin elastomer 91.0-97.5wt%, first monomer 1.0-5.0wt%, second monomer 0.5-4.0wt%, initiator 0.08-0.2wt%, antioxidant 0-0.2wt%; the sum of the amounts of each component is equal to 100%.

[0027] (1) The polyolefin elastomer is one or more polymers produced by copolymerization of ethylene and any C3-C8 olefin (more preferably propylene, butene, pentene, hexene, octene), and the melt index of the polyolefin elastomer is 0.5-45 g / 10 min.

[0028] (2) The first monomer is at least one selected from triallyl isocyanurate, triallyl cyanurate, and an acrylic ester compound containing 2 to 4 carbon-carbon double bonds, and more preferably triallyl isocyanurate. Specifically, the acrylate compound containing 2-4 carbon-carbon double bonds is selected from the following compounds: trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, ethoxylated glycerol triacrylate, propoxylated glycerol triacrylate, pentaerythritol tetraacrylate, ethoxylated pentaerythritol tetraacrylate, trimethylolpropane tetraacrylate, ditrimethylolpropane tetraacrylate, ditrimethylolpropane tetramethacrylate, propoxylated pentaerythritol tetraacrylate, tricyclohexane dimethanol diacrylate, propoxylated neopentyl glycol diacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, 2-butyl-2-ethyl-1,3-propanediol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, and polyethylene glycol dimethacrylate.

[0029] (3) The second monomer is a trialkoxysilane compound containing a carbon-carbon double bond. Specifically, it is at least one selected from the following compounds: vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tripropoxysilane, vinyl triisopropoxysilane, vinyl tributoxysilane, vinyl tripentoxysilane, vinyl triphenoxysilane, vinyl tripenzyloxysilane, vinyl trimethylenedioxysilane, vinyl triethylenedioxysilane, vinyl propionyloxysilane, vinyl triacetoxysilane, vinyl tricarboxysilane and other vinyl silanes or (meth)acryloxysilanes such as γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl methyldimethoxysilane, γ-acryloxypropyl trimethoxysilane, γ-methacryloxypropyl methyldimethoxysilane.

[0030] (4) The initiator is a peroxide initiator. Specifically, it is at least one selected from the following compounds: tert-butyl isopropyl peroxycarbonate, 2,5-dimethyl-2,5-(bis-tert-butylperoxy)hexane, tert-butyl peroxy-2-ethylhexyl carbonate, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(tert-butylperoxy)butane, tert-butyl peroxy-2-ethylhexyl carbonate, tert-amyl peroxy-2-ethylhexyl carbonate, and tert-butyl peroxy-3,3,5-trimethylhexanoate.

[0031] (5) The antioxidant is at least one of a hindered phenol antioxidant, a phosphite antioxidant and a thioester antioxidant. Specifically, at least one of the following compounds is selected: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (Antioxidant 101), tris[2,4-di-tert-butylphenyl]phosphite (Antioxidant 168), tris(nonylphenyl)phosphite, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate; more preferably, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0032] Preferably, one of the first monomer and the second monomer attracts electrons while the other pushes electrons, i.e., the e values ​​are opposite; the conjugation effect Q value of the second monomer is ≥0.2, more preferably 0.2-1; the Q values ​​of the first monomer and the second monomer differ by more than 0.2, more preferably by more than 0.8.

[0033] 2. Preparation method of the anti-precipitation and cross-linking-aiding polyolefin grafted material The following steps are involved: (1) Preparation of polyolefin modified resin pellets: polyolefin elastomer, initiator, first monomer, second monomer, antioxidant components are put into high mixing equipment according to proportion and mixed, and then granulated in a twin-screw extruder at 85-220° C. to obtain pellets; (2) The extruded pellets are homogenized in a homogenizing barrel, dehumidified and dried to obtain a polyolefin grafted material.

[0034] 3. Application of the anti-precipitation and cross-linking-aiding polyolefin grafted material in photovoltaic modules (1) For POE photovoltaic adhesive film. The POE photovoltaic adhesive film comprises the following components: 1-25wt% of the polyolefin grafted material, 70-98wt% of the polyolefin elastomer and 1-5wt% of the auxiliary agent; the sum of the amounts of the components is equal to 100%. The auxiliary agent comprises at least one of a crosslinking agent, a co-crosslinking agent, a silane coupling agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a tackifier and a pigment.

[0035] (2) For EPE photovoltaic film, the EPE film is composed of EVA layer, POE layer and EVA layer from top to bottom. The POE layer is the same as the POE photovoltaic film in (1). The EVA layer contains the following components: 95-99.0wt% EVA resin, 1.0-5.0wt% auxiliary agent; the sum of the amounts of each component is equal to 100%. The auxiliary agent includes at least one of a cross-linking agent, a co-cross-linking agent, a silane coupling agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a tackifier or a pigment. The POE layer and the EVA layer are added to the co-extrusion equipment for melt co-extrusion, and after cooling and shaping by the casting equipment, the edges are cut and rolled to obtain the EPE photovoltaic film.

[0036] Example 1 A polyolefin graft material that prevents precipitation and assists cross-linking, comprising the following components in parts by weight: 94.8 parts of a polyolefin elastomer, an ethylene-1-butene copolymer (brand number LF675) having a melt index of 14 g / 10 min; 3 parts of the first monomer, triallyl isocyanurate; 2 parts of the second monomer, γ-methacryloxypropylmethyldimethoxysilane; 0.1 part initiator, 2,5-dimethyl-2,5-(di-tert-butylperoxy)hexane; 0.1 parts of antioxidant, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0037] The preparation method of a polyolefin grafted material that prevents precipitation and aids cross-linking comprises the following steps: adding the above raw material components into a high-mixing device in proportion and mixing them evenly, setting the processing temperature to 210°C, and using a twin-screw extruder to granulate to obtain pellets; the extruded pellets are homogenized in a homogenizing barrel, dehumidified and dried to obtain a polyolefin grafted material.

[0038] A preparation method of a POE photovoltaic adhesive film comprises the following steps: mixing 13 wt% of the above-mentioned polyolefin grafted material, 84 wt% of a polyolefin elastomer (brand LF675) and 3 wt% of other additives, wherein the other additives are 0.8 wt% of tert-amyl peroxy-2-ethylhexyl carbonate, 0.5 wt% of triallyl isocyanurate, 0.5 wt% of trimethylolpropane trimethacrylate, 0.7 wt% of vinyl trimethoxysilane, 0.1 wt% of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester, 0.1 wt% of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (ultraviolet absorber 770) and 0.3 wt% of 2-hydroxy-4-n-octyloxybenzophenone, uniformly, melt-extruding, cooling, shaping and rolling to obtain the POE photovoltaic adhesive film.

[0039] A method for preparing an EPE photovoltaic film, comprising the following steps: (1) Preparation of POE resin layer: 13 wt% of the above-mentioned polyolefin graft material, 84 wt% of polyolefin elastomer (brand LF675) and 3 wt% of other additives, the other additives are 0.8 wt% of tert-amyl peroxide-2-ethylhexyl carbonate, 0.5 wt% of triallyl isocyanurate, 0.5 wt% of trimethylolpropane trimethacrylate, 0.7 wt% of vinyl trimethoxysilane, 0.1 wt% of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl ester, 0.1 wt% of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (ultraviolet absorber 770) and 0.3 wt% of 2-hydroxy-4-n-octyloxybenzophenone, mixed uniformly, melt-extruded, cooled, shaped and rolled up to obtain a POE resin layer.

[0040] (2) Preparation of EVA resin layer: 97 wt% of EVA resin and 3 wt% of other additives, including at least one or more of a cross-linking agent, a co-cross-linking agent, a silane coupling agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a tackifier or a pigment, are mixed and evenly melted and extruded, and then cooled, shaped and rolled up to obtain an EVA resin layer.

[0041] (3) Compounding: The POE resin layer prepared in step (1) and the EVA resin layer prepared in step (2) are added to a co-extrusion device for melt co-extrusion. After cooling and shaping in a casting device, the three-layer EPE photovoltaic film is trimmed and rolled up, which comprises, from top to bottom, a 100 μm thick EVA resin layer, a 250 μm thick POE resin layer, and a 100 μm thick EVA resin layer.

[0042] Example 2 A polyolefin graft material that prevents precipitation and assists cross-linking, comprising the following components in parts by weight: 91 parts of polyolefin elastomer, ethylene-1-butene copolymer (brand LF675) with a melt index of 14 g / 10 min; 4.72 parts of the first monomer, triallyl isocyanurate; 4 parts of the second monomer, γ-methacryloxypropylmethyldimethoxysilane; 0.08 parts of initiator, 2,5-dimethyl-2,5-(di-tert-butylperoxy)hexane; 0.2 parts of antioxidant, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0043] The preparation method of a polyolefin grafted material that prevents precipitation and aids cross-linking comprises the following steps: adding the above raw material components into a high-mixing device in proportion and mixing them evenly, setting the processing temperature to 210°C, and using a twin-screw extruder to granulate to obtain pellets; the extruded pellets are homogenized in a homogenizing barrel, dehumidified and dried to obtain a polyolefin grafted material.

[0044] A preparation method of a POE photovoltaic adhesive film comprises the following steps: mixing 13 wt% of the above-mentioned polyolefin grafted material, 84 wt% of a polyolefin elastomer (brand LF675) and 3 wt% of other additives, wherein the other additives are 0.8 wt% of tert-amyl peroxy-2-ethylhexyl carbonate, 0.5 wt% of triallyl isocyanurate, 0.5 wt% of trimethylolpropane trimethacrylate, 0.7 wt% of vinyl trimethoxysilane, 0.1 wt% of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester, 0.1 wt% of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (ultraviolet absorber 770) and 0.3 wt% of 2-hydroxy-4-n-octyloxybenzophenone, uniformly, melt-extruding, cooling, shaping and rolling to obtain the POE photovoltaic adhesive film.

[0045] A method for preparing an EPE photovoltaic film, comprising the following steps: (1) Preparation of POE resin layer: 13 wt% of the above-mentioned polyolefin graft material, 84 wt% of polyolefin elastomer (brand LF675) and 3 wt% of other additives, the other additives are 0.8 wt% of tert-amyl peroxide-2-ethylhexyl carbonate, 0.5 wt% of triallyl isocyanurate, 0.5 wt% of trimethylolpropane trimethacrylate, 0.7 wt% of vinyl trimethoxysilane, 0.1 wt% of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl ester, 0.1 wt% of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (ultraviolet absorber 770) and 0.3 wt% of 2-hydroxy-4-n-octyloxybenzophenone, mixed uniformly, melt-extruded, cooled, shaped and rolled up to obtain a POE resin layer.

[0046] (2) Preparation of EVA resin layer: 97 wt% of EVA resin and 3 wt% of other additives, including at least one or more of a cross-linking agent, a co-cross-linking agent, a silane coupling agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a tackifier or a pigment, are mixed and evenly melted and extruded, and then cooled, shaped and rolled up to obtain an EVA resin layer.

[0047] (3) Compounding: The POE resin layer prepared in step (1) and the EVA resin layer prepared in step (2) are added to a co-extrusion device for melt co-extrusion. After cooling and shaping in a casting device, the three-layer EPE photovoltaic film is trimmed and rolled up, which comprises, from top to bottom, a 100 μm thick EVA resin layer, a 250 μm thick POE resin layer, and a 100 μm thick EVA resin layer.

[0048] Example 3 A polyolefin graft material that prevents precipitation and assists cross-linking, comprising the following components in parts by weight: 97.5 parts of a polyolefin elastomer, an ethylene-1-butene copolymer (brand LF675) having a melt index of 14 g / 10 min; 1.5 parts of the first monomer, triallyl isocyanurate; 0.8 parts of the second monomer, γ-methacryloxypropylmethyldimethoxysilane; 0.2 parts of initiator, 2,5-dimethyl-2,5-(di-tert-butylperoxy)hexane.

[0049] The preparation method of a polyolefin grafted material that prevents precipitation and aids cross-linking comprises the following steps: adding the above raw material components into a high-mixing device in proportion and mixing them evenly, setting the processing temperature to 210°C, and using a twin-screw extruder to granulate to obtain pellets; the extruded pellets are homogenized in a homogenizing barrel, dehumidified and dried to obtain a polyolefin grafted material.

[0050] A preparation method of a POE photovoltaic adhesive film comprises the following steps: mixing 13 wt% of the above-mentioned polyolefin grafted material, 84 wt% of a polyolefin elastomer (brand LF675) and 3 wt% of other additives, wherein the other additives are 0.8 wt% of tert-amyl peroxy-2-ethylhexyl carbonate, 0.5 wt% of triallyl isocyanurate, 0.5 wt% of trimethylolpropane trimethacrylate, 0.7 wt% of vinyl trimethoxysilane, 0.1 wt% of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester, 0.1 wt% of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (ultraviolet absorber 770) and 0.3 wt% of 2-hydroxy-4-n-octyloxybenzophenone, uniformly, melt-extruding, cooling, shaping and rolling to obtain the POE photovoltaic adhesive film.

[0051] A method for preparing an EPE photovoltaic film, comprising the following steps: (1) Preparation of POE resin layer: 13 wt% of the above-mentioned polyolefin graft material, 84 wt% of polyolefin elastomer (brand LF675) and 3 wt% of other additives, the other additives are 0.8 wt% of tert-amyl peroxide-2-ethylhexyl carbonate, 0.5 wt% of triallyl isocyanurate, 0.5 wt% of trimethylolpropane trimethacrylate, 0.7 wt% of vinyl trimethoxysilane, 0.1 wt% of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl ester, 0.1 wt% of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (ultraviolet absorber 770) and 0.3 wt% of 2-hydroxy-4-n-octyloxybenzophenone, mixed uniformly, melt-extruded, cooled, shaped and rolled up to obtain a POE resin layer.

[0052] (2) Preparation of EVA resin layer: 97 wt% of EVA resin and 3 wt% of other additives, including at least one or more of a cross-linking agent, a co-cross-linking agent, a silane coupling agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a tackifier or a pigment, are mixed and evenly melted and extruded, and then cooled, shaped and rolled up to obtain an EVA resin layer.

[0053] (3) Compounding: The POE resin layer prepared in step (1) and the EVA resin layer prepared in step (2) are added to a co-extrusion device for melt co-extrusion. After cooling and shaping in a casting device, the three-layer EPE photovoltaic film is trimmed and rolled up, which comprises, from top to bottom, a 100 μm thick EVA resin layer, a 250 μm thick POE resin layer, and a 100 μm thick EVA resin layer.

[0054] Example 4 The difference from Example 1 is that the first monomer is propoxylated pentaerythritol tetraacrylate.

[0055] Example 5 The difference from Example 1 is that the second monomer is vinyltrimethylenedioxysilane.

[0056] Example 6 The difference from Example 1 is that the first monomer is propoxylated trimethylolpropane triacrylate.

[0057] Example 7 The difference from Example 1 is that the second monomer is vinyltributoxysilane.

[0058] Example 8 The difference from Example 1 is that the first monomer is trimethylolpropane tetraacrylate.

[0059] Example 9 The difference from Example 1 is that the second monomer is vinyltriethylenedioxysilane.

[0060] Comparative Example 1 The difference from Example 1 is that the second monomer is not added, and the missing amount is made up with polyolefin elastomer. The details are as follows: A polyolefin graft material that prevents precipitation and assists cross-linking, comprising the following components in parts by weight: 96.8 parts of a polyolefin elastomer, an ethylene-1-butene copolymer (brand number LF675) having a melt index of 14 g / 10 min; 3 parts of the first monomer, triallyl isocyanurate; 0.1 part initiator, 2,5-dimethyl-2,5-(di-tert-butylperoxy)hexane; 0.1 parts of antioxidant, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0061] The preparation method of a polyolefin grafted material that prevents precipitation and aids cross-linking comprises the following steps: adding the above raw material components into a high-mixing device in proportion and mixing them evenly, setting the processing temperature to 210°C, and using a twin-screw extruder to granulate to obtain pellets; the extruded pellets are homogenized in a homogenizing barrel, dehumidified and dried to obtain a polyolefin grafted material.

[0062] A preparation method of a POE photovoltaic adhesive film comprises the following steps: mixing 13 wt% of the above-mentioned polyolefin grafted material, 84 wt% of a polyolefin elastomer (brand LF675) and 3 wt% of other additives, wherein the other additives are 0.8 wt% of tert-amyl peroxy-2-ethylhexyl carbonate, 0.5 wt% of triallyl isocyanurate, 0.5 wt% of trimethylolpropane trimethacrylate, 0.7 wt% of vinyl trimethoxysilane, 0.1 wt% of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester, 0.1 wt% of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (ultraviolet absorber 770) and 0.3 wt% of 2-hydroxy-4-n-octyloxybenzophenone, uniformly, melt-extruding, cooling, shaping and rolling to obtain the POE photovoltaic adhesive film.

[0063] A method for preparing an EPE photovoltaic film, comprising the following steps: (1) Preparation of POE resin layer: 13 wt% of the above-mentioned polyolefin graft material, 84 wt% of polyolefin elastomer (brand LF675) and 3 wt% of other additives, the other additives are 0.8 wt% of tert-amyl peroxide-2-ethylhexyl carbonate, 0.5 wt% of triallyl isocyanurate, 0.5 wt% of trimethylolpropane trimethacrylate, 0.7 wt% of vinyl trimethoxysilane, 0.1 wt% of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl ester, 0.1 wt% of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (ultraviolet absorber 770) and 0.3 wt% of 2-hydroxy-4-n-octyloxybenzophenone, mixed uniformly, melt-extruded, cooled, shaped and rolled up to obtain a POE resin layer.

[0064] (2) Preparation of EVA resin layer: 97 wt% of EVA resin and 3 wt% of other additives, including at least one or more of a cross-linking agent, a co-cross-linking agent, a silane coupling agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a tackifier or a pigment, are mixed and evenly melted and extruded, and then cooled, shaped and rolled up to obtain an EVA resin layer.

[0065] (3) Compounding: The POE resin layer prepared in step (1) and the EVA resin layer prepared in step (2) are added to a co-extrusion device for melt co-extrusion. After cooling and shaping in a casting device, the three-layer EPE photovoltaic film is trimmed and rolled up, which comprises, from top to bottom, a 100 μm thick EVA resin layer, a 250 μm thick POE resin layer, and a 100 μm thick EVA resin layer.

[0066] Comparative Example 2 The difference from Example 1 is that no polyolefin grafting material is added.

[0067] Comparative Example 3 The difference from Example 1 is that the usage amounts of the first monomer and the second monomer are 0.5 wt % and 5.0 wt % respectively.

[0068] Performance Testing The maximum static friction coefficient of the POE photovoltaic adhesive films prepared in each embodiment and comparative example was tested according to GB / T 10006-2021 standard, and the results are shown in Table 1.

[0069] Table 1. The performance tests of the EPE photovoltaic films prepared in each embodiment and comparative example are shown in Table 2. The test methods are as follows: ① light transmittance: tested with reference to the method described in GB / T 29848-2018 "Ethylene-vinyl acetate copolymer (EVA) adhesive film for photovoltaic module encapsulation"; ② crosslinking degree: tested with reference to the method described in GB / T 29848-2018 "Ethylene-vinyl acetate copolymer (EVA) adhesive film for photovoltaic module encapsulation"; ③ peeling force test: tested with reference to the method described in GB / T 29848-2018 "Ethylene-vinyl acetate copolymer (EVA) adhesive film for photovoltaic module encapsulation".

[0070] Table 2. It can be seen from Table 1 and Table 2 that, compared with Comparative Example 2, the photovoltaic films prepared in each embodiment by adding the polyolefin grafted material of the present invention when preparing the films have excellent light transmittance and anti-precipitation performance.

[0071] The components of the polyolefin grafted material are critical. Compared with Example 1: (1) Comparative Example 1 did not add the second monomer, because the first monomer contains multiple double bonds that can participate in the reaction, which is easy to cause cross-linking during the grafting process, and will weaken the fluidity and cross-linking effect in the subsequent processing. Therefore, Example 1 adds the second monomer so that the second monomer and the first monomer form a more stable free radical, inhibiting the cross-linking reaction of the first monomer.

[0072] (2) In comparative example 3, the amounts of the first monomer and the second monomer are not within the preferred range, resulting in the crosslinking degree and grafting rate of the obtained polyolefin grafted material being outside the ideal range, and ultimately resulting in poor anti-precipitation effect of the film.

[0073] (3) The first monomer and the second monomer selected in Examples 4-9 have inferior anti-precipitation effects on the film as Example 1, because among these examples, the difference in Q and e values ​​between the first monomer and the second monomer in Example 1 is the largest, with a Q value difference of more than 0.8. The triallyl structure of the first monomer triallyl isocyanurate in Example 1 has high reactivity and can effectively react with the active sites in the polymer at a lower temperature, thereby increasing the crosslinking rate and degree of crosslinking; the second monomer γ-methacryloxypropylmethyldimethoxysilane has a stronger conjugated effect and is more likely to form stable free radicals, and its electron-withdrawing effect is easy to copolymerize with the electron-pushing first monomer. The Q and e values ​​of the monomers can be inferred based on the chemical structure. The -CH 2 -N, has a more obvious electron-pushing property and a smaller e value; while the ester group directly connected to the carbon-carbon double bond of γ-methacryloxypropylmethyldimethoxysilane has a conjugated property and exhibits electron-withdrawing properties, so its Q and e values ​​are both larger. In Example 8, the first monomer uses an acrylate monomer, and the Q and e values ​​of the second monomer γ-methacryloxypropylmethyldimethoxysilane are close to those of the acrylate monomer, with a Q value difference of 0.2-0.8, and the anti-precipitation effect is not as good as that of Example 1.

[0074] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A polyolefin graft material that prevents precipitation and assists cross-linking, characterized in that: The invention comprises the following components: a polyolefin elastomer, a first monomer and a second monomer; the first monomer is selected from at least one of triallyl isocyanurate, triallyl cyanurate and an acrylate compound containing 2 to 4 carbon-carbon double bonds; the second monomer is a dialkoxysilane or trialkoxysilane compound containing a carbon-carbon double bond; the sum of the mass of the first monomer and the second monomer is 1 to 10% of the polyolefin elastomer, and the mass ratio of the first monomer to the second monomer is (0.1 to 50):

1.

2. The anti-sedimentation and cross-linking-aiding polyolefin graft material according to claim 1, characterized in that: The polyolefin elastomer is one or more polymers generated by copolymerization of ethylene and any C3-C8 olefin, and the melt index of the polyolefin elastomer is 0.5-45 g / 10min.

3. The anti-sedimentation and cross-linking-aiding polyolefin graft material according to claim 1, characterized in that: The acrylate compound containing 2-4 carbon-carbon double bonds is selected from the following compounds: trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, tri(2-hydroxyethyl)isocyanuric acid triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, ethoxylated glycerol triacrylate, propoxylated glycerol triacrylate, pentaerythritol tetraacrylate, ethoxylated pentaerythritol tetraacrylate, trimethylolpropane tetraacrylate, ditrimethylolpropane tetraacrylate, ditrimethylolpropane tetramethacrylate, propoxylated pentaerythritol tetraacrylate, tricyclohexane dimethanol diacrylate, propoxylated neopentyl glycol diacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, 2-butyl-2-ethyl-1,3-propanediol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, and polyethylene glycol dimethacrylate.

4. The anti-sedimentation and cross-linking-aiding polyolefin graft material according to claim 1, 2 or 3, characterized in that: The second monomer is selected from at least one of the following compounds: vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tripropoxysilane, vinyl triisopropoxysilane, vinyl tributoxysilane, vinyl tripentoxysilane, vinyl triphenoxysilane, vinyl tripenzyloxysilane, vinyl trimethylenedioxysilane, vinyl triethylenedioxysilane, vinyl propionyloxysilane, vinyl triacetoxysilane, vinyl tricarboxysilane and other vinyl silanes or (meth) acryloxysilanes such as γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl methyldimethoxysilane, γ-acryloxypropyl trimethoxysilane, and γ-methacryloxypropyl methyldimethoxysilane.

5. The anti-sedimentation and cross-linking-aiding polyolefin graft material according to claim 1, characterized in that: The mass ratio of the first monomer to the second monomer is (0.25-10):

1.

6. The anti-sedimentation and cross-linking-aiding polyolefin graft material according to claim 1 or 5, characterized in that: The anti-sedimentation and cross-linking polyolefin graft material is composed of the following components: 91.0-97.5 wt% of polyolefin elastomer, 1.0-5.0 wt% of the first monomer, 0.5-4.0 wt% of the second monomer, 0.08-0.2 wt% of the initiator, and 0-0.2 wt% of the antioxidant; the sum of the amounts of the components is equal to 100%.

7. The anti-sedimentation and cross-linking-aiding polyolefin graft material according to claim 1, characterized in that: The initiator is a peroxide initiator; the antioxidant comprises at least one of a hindered phenol antioxidant, a phosphite antioxidant and a thioester antioxidant.

8. The method for preparing the anti-precipitation and cross-linking-aiding polyolefin graft material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: mixing various components of the raw materials, extruding and granulating at 85-220°C to obtain pellets; and homogenizing and drying the pellets to obtain polyolefin grafted materials.

9. Use of the anti-precipitation and cross-linking-aiding polyolefin grafted material according to any one of claims 1 to 7 in photovoltaic adhesive films, characterized in that: The POE layer of the photovoltaic film comprises the following components: 1-25 wt% of the polyolefin grafted material, 70-98 wt% of the polyolefin elastomer and 1-5 wt% of the auxiliary agent; the auxiliary agent includes at least one of a crosslinking agent, a co-crosslinking agent, a silane coupling agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a tackifier and a pigment.

10. The use according to claim 9, characterized in that: The photovoltaic film is an EPE film, which is composited by an EVA layer, the POE layer, and an EVA layer. The EVA layer contains the following components: 95-99.0 wt% EVA resin and 1.0-5.0 wt% additives; the additives include at least one of a cross-linking agent, a co-cross-linking agent, a silane coupling agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a tackifier, or a pigment.

Citation Information

Patent Citations

  • Polyolefin elastomer rubber film with low water vapor permeability and preparation method thereof,

    CN110016170A

  • Hot melt adhesive film

    CN111334202A

  • High-viscosity packaging adhesive film for solar photovoltaic cell and preparation method of high-viscosity packaging adhesive film

    CN116144276A

  • Polyolefin photovoltaic adhesive film as well as preparation method and application thereof

    CN116285717A

  • Fast-crosslinking, low-cost and high-peel-strength POE adhesive film and preparation method thereof

    CN117447924A

Cited By

  • Polyolefin elastomer particle as well as preparation method and application thereof

    CN120944021A

  • Polyolefin elastomer particles, and methods of making and using the same

    CN120944021B

  • Grafted polyolefin material capable of preventing precipitation and assisting in crosslinking, preparation method therefor and use thereof

    WO2026031653A1