White ink, preparation method thereof and backlight module
By doping mica microsheets into the white ink of Mini-LED display equipment and adjusting its layout method, combined with the titanium dioxide particle coating, the problems of low reflectivity and poor high temperature stability of white ink are solved, and high reflectivity and The improvement of heat resistance enhances the optical performance and reliability of the equipment.
Patent Information
- Application Number
- CN202410949976.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
The reflectivity of white ink in Mini-LED display equipment is low, resulting in low light utilization efficiency, unstable in high temperature environments, prone to peeling, affecting the reliability and life of the equipment.
Mica microsheets with sheet-like structures are doped in resin substrates. By adjusting the angle and arrangement of the surface plane of the mica microsheet and the plane of the resin substrate, a high reflectivity white ink is formed and the surface of the mica microsheet is placed on the surface of the mica microsheet. Titanium dioxide particles are coated to improve optical performance and heat resistance.
It significantly improves the reflectivity and high temperature stability of white ink, enhances the utilization rate of light, reduces light loss, and improves the reliability and durability of the equipment.
Smart Images

Figure CN118895064A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of display technology and relates to white ink and a preparation method thereof and a backlight module. Background Art
[0002] Compared with the current mainstream display technologies such as LCD and OLED, Mini-LED screens have advantages such as high brightness, long life, high contrast, wide color gamut, and excellent light control;
[0003] Although mini-LED display technology has many advantages and broad prospects, there are still some problems that need to be solved in a timely manner, such as high prices due to high costs, unsatisfactory response speeds, and high heat generated during operation.
[0004] The reflective layer used on the substrate of Mini-LED display devices is mostly white ink. However, its reflectivity is low (≤85%), the light utilization efficiency is not high, and the process steps require exposure and development, which increases the cost and process time. During reliability verification, especially during the hot and cold shock process, the bonding parts will peel off. In addition, mini-LED will release a lot of heat during operation, which also poses a challenge to the heat resistance of the material.
[0005] The performance of inks from different manufacturers may vary. The influence of different ink thicknesses and post-processing (such as high-temperature baking) on reflectivity leads to lower reflectivity. At the same time, the composition formula of white ink raw materials, such as base resin materials, pigments, fillers, additives and solvents, will also have a great impact on reliability.
[0006] Therefore, improving the reflectivity and high-temperature stability of white ink to meet the usage requirements of Mini-LED screens is a research focus in this field. Summary of the invention
[0007] In order to improve the reflectivity and reliability of white ink, the present invention aims to provide a white ink and a preparation method thereof and a backlight module. By doping mica microflakes with a flaky structure in a resin substrate, the high temperature stability and reflectivity of the white ink are improved.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a white ink, comprising a resin substrate and mica microflakes doped in the resin substrate.
[0010] In the present invention, the mica microflakes have a layered structure inside and are lamellar crystals, which have the advantages of high temperature resistance, insulation, acid and alkali corrosion resistance and good gloss. When they are doped into the resin matrix of white ink, the optical properties (reflectivity) of the white ink are higher and the high temperature stability is also improved.
[0011] In a second aspect, the present invention provides a method for preparing the white ink as described in the first aspect, the preparation method comprising the following steps:
[0012] The resin base material raw material and the mica micro-flakes are mixed and cured to obtain the white ink.
[0013] In a third aspect, the present invention further provides a backlight module, comprising a backlight substrate and a reflective layer formed by curing the white ink as described in the first aspect.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] In the present invention, the mica microflakes have a layered structure inside and are lamellar crystals, which have the advantages of high temperature resistance, insulation, acid and alkali corrosion resistance and good gloss. When they are doped into the resin matrix of white ink, the optical properties (reflectivity) of the white ink are higher and the high temperature stability is also improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a structural schematic diagram of a cross-sectional view of white ink provided in Example 1 of the present invention.
[0017] Figure 2 This is a schematic structural diagram of a cross-sectional view of white ink provided in Example 8 of the present invention.
[0018] Figure 3 This is a structural schematic diagram of a cross-sectional view of white ink provided in Example 10 of the present invention.
[0019] Among them, 1-resin substrate, 2-mica microflakes. DETAILED DESCRIPTION
[0020] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.
[0022] In the description of the embodiments of the present application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features.
[0023] One of the objectives of the present invention is to provide a white ink, which includes a resin matrix and mica microflakes doped in the resin matrix.
[0024] It should be noted that the mica micro-flakes in the present invention can be directly purchased through commercial channels.
[0025] In the present invention, the mica microsheets have a layered structure inside and are lamellar crystals, which have the advantages of high temperature resistance, insulation, acid and alkali corrosion resistance and good gloss. When they are doped into the resin matrix of white ink, the optical properties (reflectivity) of the white ink will be significantly improved, and the high temperature stability will also be improved.
[0026] If the resin matrix is doped with mica powder, that is, a non-flaky structure, the above optimization effect cannot be achieved, because the reflectivity of nano-scale mica powder is slightly lower than that of titanium dioxide, and the micro-mirror structure cannot be realized in the matrix.
[0027] In one embodiment,
[0028] The angle between the plane where the surface of the mica micro-sheet is located and the first direction is α; wherein,
[0029] α≥45°, and the first direction is perpendicular to the plane where the surface of the resin substrate is located.
[0030] In the present invention, the angle α between the plane where the surface of the mica microflakes is located and the first direction is adjusted to be ≥45°, so that the mica microflakes in the resin substrate are regularly oriented and arranged, forming a "micromirror" structure in the resin substrate, so that the reflectivity of the white ink is higher, which can reach more than 95%.
[0031] Furthermore, α=90°, the angle between the mica micro-sheets and the first direction is 90°, and the reflectivity of the white ink is higher.
[0032] In one embodiment,
[0033] N mica micro-sheets are arranged adjacent to each other in the second direction, and the angle between the plane where the surface of each mica micro-sheet is located and the first direction is the same; wherein,
[0034] N≥2, the first direction is perpendicular to the plane where the surface of the resin substrate is located, the first direction is parallel to the second direction, or the first direction intersects with the second direction.
[0035] In the present invention, the mica micro-sheets are all arranged and doped in the same direction in the second direction, forming a same-orientation distribution, forming a "micro-mirror" structure in the resin matrix, and the optical performance (reflectivity) is significantly improved.
[0036] Furthermore, the angle between the plane where the surface of each mica micro-sheet is located and the first direction is greater than or equal to 45°.
[0037] In one embodiment,
[0038] The surface of the mica microsheet also includes a coating layer, and the coating layer includes titanium dioxide particles.
[0039] In the present invention, titanium dioxide particles are coated on the surface of mica micro-sheets, which not only achieves a whitening effect but also improves the reflectivity of white ink.
[0040] In an optional embodiment, the average diameter of the titanium dioxide particles in the coating layer is 200-300 nm, for example, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, 260 nm, 270 nm, 280 nm, 290 nm or 300 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] In an optional embodiment, the titanium dioxide particles in the coating layer include anatase titanium dioxide particles and / or rutile titanium dioxide particles, preferably rutile titanium dioxide particles; the rutile type is selected for its better weather resistance and stability, and can maintain high whiteness for a long time in harsh environments, and has a more obvious whitening effect in white ink.
[0042] In one embodiment, the thickness of the coating layer is 300 to 1000 nm, for example, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm or 1000 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] In the present invention, the thickness of the coating layer is within the numerical range of 300 to 1000 nm, which can better achieve a more excellent whitening effect on the mica microsheets; if the thickness of the coating layer is too thick, the orientation process will become difficult to achieve the expected optical effect, and the viscosity of the substrate will increase, affecting the final coating process; if the thickness of the coating layer is too thin, it will affect the final optical effect (reflectivity).
[0044] In one embodiment,
[0045] The mica micro-sheet includes a first mica micro-sheet and a second mica micro-sheet, the coating layer includes a first coating layer and a second coating layer, the first coating layer corresponds to the first mica micro-sheet, and the second coating layer corresponds to the second mica micro-sheet; wherein,
[0046] The maximum long diameter of the first mica micro-sheet is different from the maximum long diameter of the second mica micro-sheet, and / or the thickness of the first coating layer is different from the thickness of the second coating layer.
[0047] The “corresponding” mentioned in the present invention means that the first coating layer is located on the surface of the first mica micro-sheet, and the second coating layer is located on the surface of the second mica micro-sheet.
[0048] In the present invention, by matching the first mica micro-sheet and the second mica micro-sheet with different maximum long diameters, the mica micro-sheets with larger sizes (i.e., the mica micro-sheets with relatively longer maximum long diameters) play a leading role to form a reflective layer, and the mica micro-sheets with smaller sizes (i.e., the mica micro-sheets with relatively shorter maximum long diameters) are filled in the gaps to enhance the light utilization rate, reduce light leakage, and thus improve the reflectivity; if all the mica micro-sheets are larger in size, larger gaps will inevitably be generated to cause light leakage, resulting in a loss of light utilization rate, and vice versa. If it is small in size, it is easy to form agglomerations, which also causes poor lighting efficiency; further, the mass ratio of the first mica microflakes to the second mica microflakes is 5:1 to 20:1, for example 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1 or 20:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] In an optional embodiment, the maximum long axis of the first mica microsheet and the maximum long axis of the second mica microsheet are each independently 1 to 10 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0050] Specifically,
[0051] The maximum long diameter of the first mica micro-sheet is greater than the maximum long diameter of the second mica micro-sheet, and the thickness of the first coating layer is greater than the thickness of the second coating layer;
[0052] or,
[0053] The maximum long diameter of the first mica micro-sheet is smaller than the maximum long diameter of the second mica micro-sheet, and the thickness of the first coating layer is greater than the thickness of the second coating layer.
[0054] In the present invention, while selecting first mica microsheets and second mica microsheets of different major diameters, the thickness of the first cladding layer and the thickness of the second cladding layer corresponding to the corresponding mica microsheets are adjusted, thereby improving the comprehensive effect of the orientation arrangement and the utilization rate of light.
[0055] In one embodiment,
[0056] The coating layer also includes zirconium dioxide particles, and / or
[0057] The surface of the coating layer also includes a protective layer;
[0058] The protective layer includes zirconium dioxide particles.
[0059] In an optional embodiment, the average diameter of the zirconium dioxide particles in the coating layer or the protective layer is 10 to 80 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm or 80 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0060] In the present invention, the coating layer also includes zirconium dioxide particles, which cooperate with the titanium dioxide particles in the coating layer to further improve the refractive index of the white ink and reduce light loss; if the coating layer only contains titanium dioxide particles, particle agglomeration may occur, the dispersion effect is poor, and large gaps are formed in the space to cause scattering and light leakage, resulting in reduced reflectivity; and when the zirconium dioxide particles are further coated on the surface of the coating layer as a separate protective layer, the reliability and stability of the material are greatly improved without losing light efficiency.
[0061] In one embodiment,
[0062] The coating layer also includes zirconium dioxide particles;
[0063] The zirconium dioxide particles are filled between the titanium dioxide particles; or,
[0064] The zirconium dioxide particles are filled in the mesopores of the titanium dioxide particles.
[0065] In the present invention, zirconium dioxide particles are present between titanium dioxide particles in the coating layer or in the mesopores of titanium dioxide particles in a filling manner, thereby filling the gaps in the coating layer, reducing light loss, and improving the refractive index.
[0066] Further,
[0067] The filling amount of the zirconium dioxide particles in the coating layer is 10-20%, for example 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0068] In the present invention, if the amount of zirconium dioxide particles filled in the coating layer is too much, exceeding 20%, the problem of too high surface hardness of the product will occur. If the amount of zirconium dioxide particles filled in the coating layer is too little, less than 10%, too many gaps will remain in the coating layer, affecting the utilization rate of light.
[0069] In one embodiment,
[0070] The thickness of the protective layer is 50-100 nm, for example, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0071] In the present invention, if the thickness of the protective layer is too thin, less than 50 nm, the coating effect is poor, which may cause the scratch resistance of the material surface to decrease; if the thickness is too thick, exceeding 100 nm, although it plays a role in improving stability and reliability, it will cause loss of light efficiency.
[0072] In one embodiment,
[0073] The mica micro-sheet includes a first mica micro-sheet and a second mica micro-sheet, the coating layer includes a first coating layer and a second coating layer, the protective layer includes a first protective layer and a second protective layer, the first coating layer and the first protective layer correspond to the first mica micro-sheet, and the second coating layer and the second protective layer correspond to the second mica micro-sheet; wherein,
[0074] The difference between the thickness of the first coating layer and the first protective layer of the first mica microsheet is different from the difference between the thickness of the second coating layer and the second protective layer of the second mica microsheet.
[0075] In the present invention, the "corresponding" means that the first coating layer is located on the surface of the first mica microsheet, the first protective layer is coated on the surface of the first coating layer, the second coating layer is located on the surface of the second mica microsheet, and the second protective layer is coated on the surface of the second coating layer.
[0076] Specifically,
[0077] The maximum long diameter of the first mica microsheet is greater than the maximum long diameter of the second mica microsheet, and the difference between the thickness of the first coating layer and the first protective layer of the first mica microsheet is greater than the difference between the thickness of the second coating layer and the second protective layer of the second mica microsheet;
[0078] or,
[0079] The maximum long diameter of the first mica microsheet is smaller than the maximum long diameter of the second mica microsheet, and the difference between the thickness of the first coating layer and the first protective layer of the first mica microsheet is smaller than the difference between the thickness of the second coating layer and the second protective layer of the second mica microsheet.
[0080] In the present invention, the thickness difference between the coating layer and the protective layer of the mica micro-sheet with a relatively large maximum long diameter is relatively larger, thereby achieving the purpose of reducing the difficulty in process preparation without affecting the overall light effect.
[0081] In one embodiment,
[0082] The resin matrix is further doped with titanium dioxide particles and / or zirconium dioxide particles.
[0083] In the present invention, titanium dioxide particles are doped into the resin matrix (i.e., titanium dioxide particles are also doped in addition to mica microflakes), so that the reflectivity of the white ink is greatly improved; and zirconium dioxide particles are doped into the resin matrix (i.e., zirconium dioxide particles are also doped in addition to mica microflakes), which plays a role of filling the gaps, realizes the full utilization of light, and reduces the loss of reflectivity.
[0084] In the present invention, when titanium dioxide particles and zirconium dioxide particles are doped in the resin substrate at the same time, the amount of titanium dioxide particles added is 50-70%, such as 50%, 55%, 60%, 65% or 70%, etc., and the amount of zirconium dioxide particles added is 30-50%, such as 30%, 35%, 40%, 45% or 50%, etc., based on the sum of the mass of titanium dioxide particles and zirconium dioxide particles as 100%. However, the above values are not limited to the above values, and other values not listed within the above value range are also applicable.
[0085] In one embodiment,
[0086] The resin substrate includes a silicone resin substrate.
[0087] The white ink of the present invention uses silicone resin as a base material. The silicone resin has a high silicon-oxygen bond energy (443 Kj / mol), high heat resistance and mechanical properties, and excellent compatibility with other materials (such as mica microsheets, etc.), so that the white ink can work stably for a long time at a higher temperature without any malfunction, and has excellent reliability and stability.
[0088] It is understandable that the resin substrate provided by the present invention, in addition to the silicone resin, may also include other types of conventional resin substrates, such as polyester resin and the like.
[0089] A second object of the present invention is to provide a method for preparing the white ink as described in the first object.
[0090] The preparation method comprises the following steps:
[0091] The resin base material raw material and the mica micro-flakes are mixed and cured to obtain the white ink.
[0092] The preparation method provided by the invention is simple and easy to operate, does not require a complicated preparation process, and is suitable for industrial application.
[0093] In one embodiment,
[0094] Before the mixing, the mica micro-sheets are coated with a coating layer;
[0095] The coating layer includes titanium dioxide particles.
[0096] In the present invention, any conventional method that can achieve coating of titanium dioxide particles on mica microsheets is applicable to the present invention, such as in-situ growth coating method or physical coating method, and in-situ growth coating method is preferred.
[0097] Exemplarily, the present invention provides a method for coating mica microflakes with titanium dioxide particles:
[0098] The titanium salt and the mica microsheets to be coated are precipitated and coated in a solution, such as titanium tetrachloride plus alkali method, organic acid titanium method, thermal hydrolysis method or buffer method, etc. Commonly used soluble titanium salts include titanium tetrachloride or titanyl sulfate, etc. The specific preparation parameters, etc., can be adaptively selected and adjusted by technical personnel in this field according to actual needs.
[0099] For example, the present invention takes the titanium tetrachloride alkali method as an example, dissolving an appropriate amount of sodium hydroxide in deionized water to prepare a 1 mol / L alkali solution, and then slowly adding the prepared mixture of titanium tetrachloride and mica microflakes to the alkali solution, and the reaction rate and temperature of this process should not be too high. After the reaction is complete, the generated precipitate is fully washed with deionized water and placed in a vacuum oven for drying, and finally the product can be obtained.
[0100] Further, in one embodiment,
[0101] The coating layer also includes zirconium dioxide particles;
[0102] The zirconium dioxide particles are filled between the titanium dioxide particles; or,
[0103] The zirconium dioxide particles are filled in the mesopores of the titanium dioxide particles.
[0104] and / or, in one embodiment,
[0105] Covering the coating layer with a protective layer;
[0106] The protective layer includes zirconium dioxide particles.
[0107] The present invention does not specifically limit the method for preparing zirconium dioxide particles, and the present invention is applicable to any method that is reasonably known to those skilled in the art and is applicable to the present invention.
[0108] Exemplarily, the present invention provides a method for filling zirconium dioxide particles in a coating layer:
[0109] A surfactant template method is provided to fill zirconium dioxide between titanium dioxide particles or in the mesopores of titanium dioxide particles; first, a suitable surfactant is selected and dissolved, and then inorganic raw material titanium dioxide is added to form a sol or gel state under certain conditions; an appropriate amount of zirconium dioxide particles is added to the formed sol or gel and a hydrothermal reaction is carried out, and finally a preliminary mesoporous material is obtained after cooling / filtration and drying, and then the surfactant template is removed by roasting or solvent extraction.
[0110] The present invention also provides a method for coating the surface of a coating layer with zirconium dioxide particles as a protective layer:
[0111] A sol-gel method is provided, in which titanium dioxide and zirconium dioxide are dissolved as precursor substances in a suitable solvent, and then the precursor solution is hydrolyzed and condensed by controlling temperature, pH and other conditions to gradually form a sol. As the reaction proceeds, the particles in the sol gradually aggregate to form a gel with a three-dimensional network structure, and then the gel is heat-treated to remove excess solvent and water to obtain the corresponding material.
[0112] In one embodiment,
[0113] Before the curing, the mixed colloidal substance is subjected to distribution and orientation adjustment of mica microsheets, and the method for adjusting the distribution and orientation includes applying an electric field or a natural leveling method.
[0114] Specifically,
[0115] The electric field parameters of the applied electric field method include: the electric field range is 0.01 to 1000 V / m, and the frequency range is 20 to 2000 Hz;
[0116] The preparation parameters of the natural leveling method include: a leveling temperature of 60 to 70° C. and a leveling time of 30 to 60 minutes.
[0117] In the present invention, the specific preparation process of the electric field application method includes: applying an electric field in a first direction, and achieving the orientation arrangement of mica microsheets in the resin substrate by adjusting the parameters of the electric field;
[0118] The specific preparation process of the natural leveling method includes: regulating the temperature and time of the mixed colloidal substance, that is, placing it in an oven and heating it at 60°C for 1 hour to promote natural leveling, and the natural leveling state realizes the orientation arrangement of mica microsheets in the resin matrix.
[0119] In one embodiment, the resin substrate raw material includes a resin, a coupling agent, a catalyst, an inhibitor and a curing agent;
[0120] The resin substrate raw material further includes first particles and / or second particles; the first particles include titanium dioxide particles, and the second particles include zirconium dioxide particles.
[0121] In the present invention, in addition to the resin, the types of coupling agents, catalysts, inhibitors and curing agents are also selected according to conventional techniques; those skilled in the art can select and adjust them according to actual needs;
[0122] In an alternative embodiment, the coupling agent includes but is not limited to dimethylbis(chloroethyl)silane, triethylchlorosilane, methyltri(vinyldioxy)silane, etc.;
[0123] In an optional embodiment, the catalyst includes but is not limited to a platinum group metal catalyst, a vinyl silane catalyst, an epoxy resin catalyst, a nitro compound catalyst, etc.;
[0124] In an optional embodiment, the curing agent includes but is not limited to acid / base catalyzed silicone curing agent, alkyl silicone curing agent, alcoholamine silicone curing agent, ethyl silicate, etc.
[0125] In one embodiment,
[0126] In parts by weight, the mixed raw materials include:
[0127]
[0128] For example, the weight proportion of the resin can be 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, 45 parts, 46 parts, 47 parts, 48 parts, 49 parts, 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts or 60 parts, etc.; the weight proportion of the coupling agent can be 0.05 parts, 0.1 parts, 0.5 parts, 1 parts, 1.5 parts or 2 parts, etc.; the weight proportion of the catalyst can be 0.05 parts, 0.1 parts, 0.5 parts, 1 parts, 1.5 parts or 2 parts, etc. ; The inhibitor can be 0.01 parts, 0.05 parts, 0.1 parts, 0.5 parts, 1 parts, 1.5 parts or 2 parts, etc.; the curing agent can be 1 part, 1.5 parts, 2 parts, 2.5 parts or 3 parts, etc.; the weight proportions of the first particles and / or the second particles can be 0 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts, etc., but are not limited to the listed values, and other values not listed within the numerical range are equally applicable.
[0129] It should be noted that in the preparation process of the specific embodiments of the present invention, the weight percentage added in the preparation raw materials can be a single value or a range value, which does not affect the formation of the final product structure.
[0130] It can be understood that in the preparation raw materials provided by the present invention, the purpose of enhancing the reflectivity of the material system is achieved by regulating the weight fraction of mica microflakes added; however, if the weight fraction of mica microflakes is too small, that is, the amount added is too little, it is not conducive to improving the reflectivity; and if the weight fraction is too large, that is, the amount added is too much, it will affect the orientation process of the mica microflakes, and may make the surface of the material become sticky and uneven.
[0131] A third object of the present invention is to provide a backlight module, which includes a backlight substrate and a reflective layer formed by curing the white ink as described in the first object.
[0132] In the present invention, except for the reflective layer, the structures in the backlight module are all conventional technical solutions.
[0133] Example 1
[0134] This embodiment provides a white ink such as Figure 1 As shown, the white ink includes a resin substrate 1 (organic silicone resin substrate) and mica micro-sheets 2 (with a maximum long diameter of 5 μm) doped in the organic silicone resin substrate.
[0135] The preparation method of the white ink is as follows:
[0136] In parts by weight, the raw materials for preparation are:
[0137]
[0138] The above-mentioned raw materials in parts by weight are mixed and solidified to obtain the white ink.
[0139] Example 2
[0140] This embodiment provides a white ink, which includes an organic silicone resin substrate and mica microsheets (with a maximum long diameter of 1 μm) doped in the organic silicone resin substrate.
[0141] The preparation method of the white ink is as follows:
[0142] In parts by weight, the raw materials for preparation are:
[0143]
[0144] The above-mentioned raw materials in parts by weight are mixed and solidified to obtain the white ink.
[0145] Example 3
[0146] This embodiment provides a white ink, which includes an organic silicone resin substrate and mica microsheets (with a maximum long diameter of 10 μm) doped in the organic silicone resin substrate.
[0147] The preparation method of the white ink is as follows:
[0148] In parts by weight, the raw materials for preparation are:
[0149]
[0150] The above-mentioned raw materials in parts by weight are mixed and solidified to obtain the white ink.
[0151] Example 4
[0152] The difference between this embodiment and embodiment 1 is that in the preparation method of this embodiment, the weight proportion of mica microsheets is 40 parts.
[0153] The rest of the preparation methods and parameters were the same as those in Example 1.
[0154] Example 5
[0155] The difference between this embodiment and embodiment 1 is that in the preparation method of this embodiment, the weight proportion of mica microsheets is 5 parts.
[0156] The rest of the preparation methods and parameters were the same as those in Example 1.
[0157] Example 6
[0158] The difference between this embodiment and embodiment 1 is that in this embodiment, the angle α between the plane where the surface of each mica microplate is located and the first direction is ≥45°, and the first direction is perpendicular to the plane where the surface of the resin substrate is located.
[0159] In the preparation method:
[0160] Apply an electric field along a first direction to the mixed colloidal substance, wherein the electric field parameters are as follows: the electric field range is 0.01 to 1000 V / m, and the frequency range is 20 to 2000 Hz, so as to achieve the oriented distribution of the mica microsheets in the silicone resin substrate; and then cure the mixed colloidal substance to obtain the white ink.
[0161] The rest of the preparation methods and parameters were the same as those in Example 1.
[0162] Example 7
[0163] The difference between this embodiment and embodiment 1 is that in this embodiment, the angle α between the plane where the surface of each mica microplate is located and the first direction is ≥45°, and the first direction is perpendicular to the plane where the surface of the resin substrate is located.
[0164] In the preparation method:
[0165] The mixed colloidal substance is naturally leveled at 60° C. for 1 hour to achieve the orientation distribution of the mica microsheets in the silicone resin matrix; and then cured to obtain the white ink.
[0166] Example 8
[0167] The difference between this embodiment and embodiment 1 is that Figure 2 As shown, in this embodiment, the angle α between the plane where the surface of each mica microflake is located and the first direction is 90° (i.e., the mica microflakes are arranged in a super-horizontal manner in the silicone resin substrate), and the first direction is perpendicular to the plane where the surface of the resin substrate is located.
[0168] In the preparation method, the electric field parameters are adjusted to an electric field range of 800 to 1500 V / m and a frequency range of 1500 to 2000 Hz.
[0169] The rest of the preparation methods and parameters were the same as those in Example 1.
[0170] Example 9
[0171] The difference between this embodiment and Embodiment 1 is that, in this embodiment, the angle α between the plane where the surface of each mica micro-sheet is located and the first direction is less than 45°.
[0172] In the preparation method, the electric field parameters are adjusted to an electric field range of 0.01 to 100 V / m and a frequency range of 10 to 100 Hz.
[0173] The rest of the preparation methods and parameters were the same as those in Example 1.
[0174] Example 10
[0175] The difference between this embodiment and embodiment 1 is that Figure 3 As shown, the surface of the mica micro-sheet of this embodiment includes a coating layer, the coating particles in the coating layer are titanium dioxide particles (with an average particle size of 300 nm), and the thickness of the coating layer is 600 nm.
[0176] In the preparation method, the mica micro-sheets are firstly subjected to coating and modification treatment, as follows:
[0177] Dissolve 40g of sodium hydroxide in 1L of deionized water to prepare a 1mol / L alkali solution, then slowly add the prepared mixture of 20g of titanium tetrachloride and 40g of mica microflakes into the alkali solution. The reaction rate and temperature of this process should not be too high. The temperature is room temperature and the duration is 4h. After the reaction is complete, wash the generated precipitate with deionized water and place it in a vacuum oven for drying. Finally, titanium dioxide-coated modified mica microflakes are obtained.
[0178] The titanium dioxide-coated modified mica micro-sheets are then used as the preparation raw material.
[0179] The rest of the preparation methods and parameters were the same as those in Example 1.
[0180] Figure 3 In the figure, the mica micro-sheets in the white ink are magnified, and it can be seen that the surface is covered with titanium dioxide particles, forming a Figure 3 The core-shell structure shown on the far right.
[0181] Embodiment 11
[0182] The difference between this embodiment and embodiment 1 is that this embodiment includes a first mica micro-sheet (with a maximum long diameter of 8 μm) and a second mica micro-sheet (with a maximum long diameter of 3 μm), and the mass ratio of the first mica micro-sheet to the second mica micro-sheet is 5:1;
[0183] The surface of the first mica microsheet is coated with a first coating layer, the coated particles of the first coating layer are titanium dioxide particles (with an average particle size of 300 nm), and the thickness of the first coating layer is 600 nm;
[0184] The surface of the second mica microsheet is coated with a second coating layer, the coated particles of the second coating layer are titanium dioxide particles (with an average particle size of 300 nm), and the thickness of the second coating layer is 300 nm;
[0185] In the preparation method, the first mica micro-sheet and the second mica micro-sheet are first coated and modified, as follows: the same titanium tetrachloride alkali method as in Example 10 is adopted; 20g of sodium hydroxide is added to 200mL of deionized water and stirred at a uniform speed until dissolved, and the two alkaline waters are named A and B, respectively, and then the prepared 4g of titanium tetrachloride and 4g of mica micro-sheets (respectively the first mica micro-sheet and the second mica micro-sheet) are slowly added to the alkaline water A, and 4g of titanium tetrachloride and 8g of mica micro-sheets are added to B. The reaction rate and temperature of this process are room temperature and the duration is 5h. After the reaction is complete, the generated precipitate is fully washed and dried in a vacuum oven at 120°C for 6h to finally obtain the product.
[0186] The first mica micro-sheet and the second mica micro-sheet that have been coated and modified are used as preparation raw materials.
[0187] The rest of the preparation methods and parameters were the same as those in Example 1.
[0188] Example 12
[0189] The difference between this embodiment and embodiment 11 is that this embodiment only contains the first mica micro-sheet.
[0190] The rest of the preparation methods and parameters were the same as those in Example 11.
[0191] Embodiment 13
[0192] The difference between this embodiment and embodiment 11 is that this embodiment only contains the second mica micro-sheet.
[0193] The rest of the preparation methods and parameters were the same as those in Example 11.
[0194] Embodiment 14
[0195] The difference between this embodiment and embodiment 1 is that the surface of the mica microflakes in this embodiment is coated with a coating layer, and the coating particles in the coating layer are titanium dioxide particles (average particle size is 300nm) and zirconium dioxide particles filled in the mesopores of the titanium dioxide particles (average particle size is 30nm, filling amount is 15%), and the thickness of the coating layer is 600nm.
[0196] In the preparation method, the mica microsheets are first coated and modified, specifically as follows: the aforementioned template method or sol-gel method is used to prepare a mesoporous material, the material comprising titanium dioxide and zirconium dioxide filled in the titanium dioxide mesopores; then the coating layer is prepared by the same method as in Example 10; the specific steps are as follows: first, 10g of a long-chain alkyl quaternary ammonium salt is selected as a surfactant and dissolved in 200mL of deionized water, then 15g of an inorganic raw material titanium dioxide is added, and the mixture is heated to 60°C and kept warm for 8h to form a sol or gel state; 7g of zirconium dioxide particles are added to the formed sol or gel and a hydrothermal reaction is carried out, and finally, a preliminary mesoporous material is obtained after cooling / filtration and drying, and then the surfactant template is removed by roasting or solvent extraction;
[0197] Then, 40g of sodium hydroxide is dissolved in 1L of deionized water to prepare a 1mol / L alkali solution, and then the prepared mesoporous material and 40g of mica microsheets are gradually added to the alkali solution. The reaction rate and temperature of this process should not be too high, the temperature is room temperature, and the duration is 5h. After the reaction is complete, the generated precipitate is fully washed with deionized water and placed in a vacuum oven for drying to obtain the product.
[0198] The coated and modified mica micro-sheets are then used as the preparation raw materials.
[0199] The rest of the preparation methods and parameters were the same as those in Example 1.
[0200] Embodiment 15
[0201] The difference between this embodiment and embodiment 1 is that in this embodiment, the surface of the mica microflakes is coated with a coating layer, and the surface of the coating layer is coated with a protective layer; the coating particles in the coating layer are titanium dioxide particles (average particle size is 300nm), and the thickness of the coating layer is 600nm; the coating particles in the protective layer are zirconium dioxide particles (average particle size is 80nm), and the thickness of the protective layer is 80nm.
[0202] In the preparation method, the mica micro-sheets are first coated with a coating layer and a protective layer, as follows: first, 20g of mica slurry is heated to 70-80°C, and an appropriate amount of alkali solution is added under uniform stirring to control the pH to 12-12.5, and then 20g of titanium salt (titanium tetrachloride) is gradually added. After sufficient reaction (6h), hydrated titanium dioxide can be deposited on the surface of the mica sheet, and the target product can be obtained after filtering, drying and high-temperature calcination at 900°C for 2h. After that, zirconium dioxide can be coated on the surface of the mica micro-sheet by thermal hydrolysis, and the specific steps are as follows: take 50g of mica slurry and control the temperature at 70-80°C, then add 10g of zirconium nitrate or zirconium sulfate, boil and reflux for about 1h, then filter, water system, dry, heat to 950°C and calcine for half an hour to obtain the target product.
[0203] The processed mica micro-flakes are then used as raw materials for preparation.
[0204] The rest of the preparation methods and parameters were the same as those in Example 1.
[0205] Example 16
[0206] The difference between this embodiment and embodiment 1 is that this embodiment includes a first mica micro-sheet (with a maximum long diameter of 8 μm) and a second mica micro-sheet (with a maximum long diameter of 3 μm), and the mass ratio of the first mica micro-sheet to the second mica micro-sheet is 10:1 to 3:1;
[0207] The surface of the first mica microsheet is coated with a first coating layer and a first protective layer in sequence from the inside to the outside, the coated particles of the first coating layer are titanium dioxide particles (with an average particle size of 200 nm), the thickness of the first coating layer is 600 nm, the coated particles of the first protective layer are zirconium dioxide particles (with an average particle size of 80 nm), and the thickness of the first protective layer is 100 nm;
[0208] The surface of the second mica microsheet is coated with a second coating layer and a second protective layer in sequence from the inside to the outside, the coated particles of the second coating layer are titanium dioxide particles (with an average particle size of 200 nm), the thickness of the second coating layer is 300 nm, the coated particles of the second protective layer are zirconium dioxide particles (with an average particle size of 30 nm), and the thickness of the second protective layer is 40 nm;
[0209] In the preparation method, the first mica microsheet and the second mica microsheet are first subjected to coating modification treatment, which is specifically as follows: the specific coating operation steps are shown in the above-mentioned embodiment 15;
[0210] Coating modification of the first mica microsheet: first coat the mica microsheet with a coating layer and a protective layer. First, heat 50g of mica slurry to 70-80°C, add an appropriate amount of alkali solution while stirring evenly, control the pH to 12-12.5, then gradually add 40g of titanium salt (titanium tetrachloride), and after sufficient reaction (6h), hydrated titanium dioxide can be deposited on the surface of the mica sheet. After filtering, drying and calcining at 900°C for 2h, the target product (the first coating layer) can be obtained. Then take 50g of mica slurry and control the temperature at 70-80°C, then add 10g of zirconium nitrate or zirconium sulfate, boil and reflux for about 1h, then filter, water-solidify and dry, heat to 950°C and calcine for half an hour to obtain the target product (the first protective layer);
[0211] The coating modification of the second mica micro-sheet is as follows: first, the mica micro-sheet is coated with a coating layer and a protective layer. First, 50g of mica slurry is heated to 70-80°C, and an appropriate amount of alkali solution is added under uniform stirring to control the pH to 12-12.5. Then, 20g of titanium salt (titanium tetrachloride) is gradually added. After sufficient reaction (6h), hydrated titanium dioxide can be deposited on the surface of the mica sheet. After filtering, drying and calcining at high temperature of 900°C for 2h, the target product (second coating layer) can be obtained. Then, 50g of mica slurry is taken and the temperature is controlled at 70-80°C, and then 4g of zirconium nitrate or zirconium sulfate is added, and the boiling reflux is maintained for about 1h. After that, it is filtered, dried by water system, and heated to 950°C and calcined for half an hour to obtain the target product (second protective layer).
[0212] The first mica micro-sheet and the second mica micro-sheet that have been coated and modified are used as preparation raw materials.
[0213] The rest of the preparation methods and parameters were the same as those in Example 1.
[0214] Embodiment 17
[0215] The difference between this embodiment and embodiment 1 is that the silicone resin substrate of this embodiment is further doped with titanium dioxide particles (with an average particle size of 500 nm).
[0216] In the preparation method, the raw materials are as follows, by weight:
[0217]
[0218] The above-mentioned raw materials in parts by weight are mixed and solidified to obtain the white ink.
[0219] Embodiment 18
[0220] The difference between this embodiment and embodiment 1 is that the silicone resin substrate of this embodiment is further doped with zirconium dioxide particles (with an average particle size of 20 nm).
[0221] In the preparation method, the raw materials are as follows, by weight:
[0222]
[0223] The above-mentioned raw materials in parts by weight are mixed and solidified to obtain the white ink.
[0224] Embodiment 19
[0225] The difference between this embodiment and embodiment 1 is that the silicone resin substrate of this embodiment is further doped with titanium dioxide particles (average particle size of 100 nm) and zirconium dioxide particles (average particle size of 50 nm);
[0226] When the total mass of the titanium dioxide particles and the zirconium dioxide particles is 100%, the mass proportion of the titanium dioxide particles is 60%, and the mass proportion of the zirconium dioxide particles is 40%.
[0227] In the preparation method, the raw materials are as follows, by weight:
[0228]
[0229]
[0230] The above-mentioned raw materials in parts by weight are mixed and solidified to obtain the white ink.
[0231] Comparative Example 1
[0232] The difference between this comparative example and Example 1 is that the white ink provided in this comparative example does not contain mica microflakes.
[0233] In the preparation method, no mica micro-flakes are added to the preparation raw materials.
[0234] The rest of the preparation methods and parameters were the same as those in Example 1.
[0235] [Performance test]
[0236] The performance of the white ink provided in Examples 1-19 and Comparative Example 1 was tested:
[0237] (a) Reflectivity: The reflectivity value of the white ink coating was tested using a Konica Minolta CM-3600A spectrophotometer;
[0238] (b) Whiteness value: The whiteness value of the white ink coating was tested using Shanghai Yuefeng SBDY-3 whiteness meter;
[0239] (c) Yellowing resistance: The cured white ink sample was placed in a 200°C oven for 5 minutes, and then the reflectivity was tested using a Konica Minolta CM-3600A spectrophotometer. The yellowing resistance was evaluated by the change in reflectivity.
[0240] The test results of Examples 1-5 and Comparative Example 1 are shown in Table 1.
[0241] Table 1
[0242]
[0243]
[0244] From Table 1, we can get:
[0245] From the data results of Example 1, Example 4 and Example 5, it can be seen that if too much mica micro-flakes are added to the white ink, the light reflection performance of the material will be affected, while if too little mica micro-flakes are added, the reflectivity will decrease.
[0246] From the data results of Example 1 and Comparative Example 1, it can be seen that the whiteness value and yellowing resistance of the material are significantly improved by doping mica microflakes into the white ink of the present invention.
[0247] The test results of Example 1, Examples 6-9 and Comparative Example 1 are shown in Table 2.
[0248] Table 2
[0249]
[0250]
[0251] From Table 2, we can get:
[0252] From the data results of Example 1 and Examples 6-9, it can be seen that the mica microflakes in the resin matrix are oriented and distributed, which effectively improves the utilization rate of light, thereby greatly improving the reflectivity; and the angle α between the plane where the surface of each mica microflake is located and the first direction is ≥45°, which can better realize the utilization of light and reduce light loss.
[0253] The test results of Example 1, Examples 10-16 and Comparative Example 1 are shown in Table 3.
[0254] Table 3
[0255] Reflectivity(%) Whiteness value Yellowing resistance Example 1 95.23% 93.7% excellent Example 10 95.81% 95.80% excellent Embodiment 11 98.78% 98.52% excellent Example 12 94.18% 92.98% excellent Embodiment 13 93.25% 92.78% excellent Embodiment 14 96.23% 94.98% excellent Embodiment 15 97.20% 95.45% excellent Example 16 98.35 96.23% excellent Comparative Example 1 85.75% 88.7% generally
[0256] From Table 3, we can get:
[0257] From the data results of Example 1 and Example 10, it can be seen that the coating of the titanium dioxide particle coating layer on the surface of the mica micro-sheet not only has a whitening effect, but also improves the reflectivity of the material;
[0258] From the data results of Example 1 and Examples 11-13, it can be seen that in the present invention, mica micro-flakes of different sizes are selected for mixed doping, and the larger mica micro-flakes play a dominant role to form a reflective layer, and the smaller mica micro-flakes are filled into the gaps to enhance the light utilization rate and reduce the light leakage phenomenon, thereby improving the reflectivity; while only using large-sized mica micro-flakes will inevitably produce larger gaps and cause light leakage, thereby reducing the light utilization rate; and all small-sized mica micro-flakes are easy to form agglomerations, which also results in poor light efficiency;
[0259] From the data results of Example 10 and Examples 14-16, it can be seen that if the surface of the mica microsheet is only coated with titanium dioxide particles, particle agglomeration may occur, and large gaps will be formed in the coating layer, causing scattering and light leakage, resulting in limited reflectivity improvement effect; while by filling with zirconium dioxide particles or coating as a separate protective layer, the utilization rate of light is improved, light loss is avoided, and a significant improvement in reflectivity is achieved.
[0260] The data results of Example 1, Examples 17-19 and Comparative Example 1 are shown in Table 4.
[0261] Table 4
[0262] Reflectivity(%) Whiteness value Yellowing resistance Example 1 95.23% 93.7% excellent Embodiment 17 98.78% 94.66% excellent Embodiment 18 97.86% 95.67% excellent Embodiment 19 99.15% 96.25% excellent Comparative Example 1 85.75% 88.7% generally
[0263] From Table 4, we can get:
[0264] From the data results of Examples 1 and 17-19, it can be seen that in addition to doping with mica microflakes, the present invention further dopes titanium dioxide particles and / or zirconium dioxide particles in the resin matrix, which improves whiteness while enhancing reflectivity and heat resistance.
[0265] To sum up, in the present invention, the mica microflakes have a layered structure inside and are lamellar crystals, which have the advantages of high temperature resistance, insulation, acid and alkali corrosion resistance and good gloss. When they are doped into the resin matrix of white ink, the optical properties (reflectivity) of the white ink are significantly improved, and the high-temperature stability is also improved; further, by orienting and distributing the mica microflakes; or surface modifying the mica microflakes; or adding doped particles to the resin matrix, the utilization rate of light is improved, the loss of light is reduced, the reflectivity of the white ink is greatly improved, and the whitening effect is achieved.
[0266] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A white ink, characterized in that: The white ink includes a resin matrix and mica microflakes doped in the resin matrix.
2. The white ink according to claim 1, characterized in that: The angle between the plane where the surface of the mica micro-sheet is located and the first direction is α; wherein, α≥45°, and the first direction is perpendicular to the plane where the surface of the resin substrate is located.
3. The white ink according to claim 2, characterized in that: α=90°。 4. The white ink according to claim 1, characterized in that: N mica micro-sheets are arranged adjacent to each other in the second direction, and the angle between the plane where the surface of each mica micro-sheet is located and the first direction is the same; wherein, N≥2, the first direction is perpendicular to the plane where the surface of the resin substrate is located, the first direction is parallel to the second direction, or the first direction intersects with the second direction.
5. The white ink according to claim 4, characterized in that: The angle between the plane where the surface of each mica micro-sheet is located and the first direction is greater than or equal to 45°.
6. The white ink according to claim 1, characterized in that: The surface of the mica microsheet also includes a coating layer, and the coating layer includes titanium dioxide particles.
7. The white ink according to claim 6, characterized in that: The coating layer has a thickness of 300 to 1000 nm.
8. The white ink according to claim 6, characterized in that: The mica micro-sheet includes a first mica micro-sheet and a second mica micro-sheet, the coating layer includes a first coating layer and a second coating layer, the first coating layer corresponds to the first mica micro-sheet, and the second coating layer corresponds to the second mica micro-sheet; wherein, The maximum long diameter of the first mica micro-sheet is different from the maximum long diameter of the second mica micro-sheet, and / or the thickness of the first coating layer is different from the thickness of the second coating layer.
9. The white ink according to claim 8, characterized in that: The maximum long diameter of the first mica micro-sheet is greater than the maximum long diameter of the second mica micro-sheet, and the thickness of the first coating layer is greater than the thickness of the second coating layer.
10. The white ink according to claim 8, characterized in that: The maximum long diameter of the first mica micro-sheet is smaller than the maximum long diameter of the second mica micro-sheet, and the thickness of the first coating layer is greater than the thickness of the second coating layer.
11. The white ink according to claim 6, characterized in that: The coating layer also includes zirconium dioxide particles, and / or The surface of the coating layer also includes a protective layer; The protective layer includes zirconium dioxide particles.
12. The white ink according to claim 11, characterized in that: The coating layer also includes zirconium dioxide particles; The zirconium dioxide particles are filled between the titanium dioxide particles; or, The zirconium dioxide particles are filled in the mesopores of the titanium dioxide particles.
13. The white ink according to claim 12, characterized in that: The filling amount of the zirconium dioxide particles in the coating layer is 10 to 20%.
14. The white ink according to claim 11, characterized in that: The thickness of the protective layer is 50-100 nm.
15. The white ink according to claim 11, characterized in that: The mica micro-sheet includes a first mica micro-sheet and a second mica micro-sheet, the coating layer includes a first coating layer and a second coating layer, the protective layer includes a first protective layer and a second protective layer, the first coating layer and the first protective layer correspond to the first mica micro-sheet, and the second coating layer and the second protective layer correspond to the second mica micro-sheet; wherein, The difference between the thickness of the first coating layer and the first protective layer of the first mica microsheet is different from the difference between the thickness of the second coating layer and the second protective layer of the second mica microsheet.
16. The white ink according to claim 15, characterized in that: The maximum long diameter of the first mica microsheet is greater than the maximum long diameter of the second mica microsheet, and the difference between the thickness of the first coating layer and the first protective layer of the first mica microsheet is greater than the difference between the thickness of the second coating layer and the second protective layer of the second mica microsheet.
17. The white ink according to claim 15, characterized in that: The maximum long diameter of the first mica microsheet is smaller than the maximum long diameter of the second mica microsheet, and the difference between the thickness of the first coating layer and the first protective layer of the first mica microsheet is smaller than the difference between the thickness of the second coating layer and the second protective layer of the second mica microsheet.
18. The white ink according to claim 1, characterized in that: The resin matrix is further doped with titanium dioxide particles and / or zirconium dioxide particles.
19. The white ink according to claim 1, characterized in that: The resin substrate includes a silicone resin substrate.
20. A method for preparing a white ink according to any one of claims 1 to 19, characterized in that: The preparation method comprises the following steps: The resin base material raw material and the mica micro-flakes are mixed and cured to obtain the white ink.
21. The preparation method according to claim 20, characterized in that: Before the mixing, the mica micro-sheets are coated with a coating layer; The coating layer includes titanium dioxide particles.
22. The preparation method according to claim 21, characterized in that: The coating layer also includes zirconium dioxide particles; The zirconium dioxide particles are filled between the titanium dioxide particles; or, The zirconium dioxide particles are filled in the mesopores of the titanium dioxide particles.
23. The preparation method according to claim 21, characterized in that: Covering the coating layer with a protective layer; The protective layer includes zirconium dioxide particles.
24. The preparation method according to claim 20, characterized in that: Before the curing, the mixed colloidal substance is subjected to distribution and orientation adjustment of mica microsheets, and the method for adjusting the distribution and orientation includes applying an electric field or a natural leveling method.
25. The preparation method according to claim 24, characterized in that: The electric field parameters of the applied electric field method include: the electric field range is 0.01 to 1000 V / m, and the frequency range is 20 to 2000 Hz; The preparation parameters of the natural leveling method include: a leveling temperature of 60 to 70° C. and a leveling time of 30 to 60 minutes.
26. The preparation method according to claim 20, characterized in that: The resin substrate raw materials include resin, coupling agent, catalyst, inhibitor and curing agent; The resin substrate raw material further includes first particles and / or second particles; the first particles include titanium dioxide particles, and the second particles include zirconium dioxide particles.
27. The preparation method according to claim 20, characterized in that: In parts by weight, the mixed raw materials include:
28. A backlight module, characterized in that: The backlight module comprises a backlight substrate and a reflective layer formed by curing the white ink as described in any one of claims 1 to 19.