Environment-friendly carbon black color paste and preparation process thereof
By optimizing the raw material formulation and preparation process of carbon black paste, and by using a variety of additives and fine filtration, the problems of uneven dispersion and high pollution in traditional carbon black paste have been solved, and the stability and environmental friendliness have been improved.
Patent Information
- Application Number
- CN202411013550.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional carbon black paste preparation processes often involve the use of a single dispersant, resulting in uneven dispersion, poor stability, limited effectiveness of additives, and high energy consumption and serious pollution.
The preparation process is optimized by using a combination of various dispersants, stabilizers, preservatives, antistatic agents, thickeners and defoamers, including stirring and filtration steps, to form a uniform carbon black slurry and remove impurities.
It improves the stability and tinting strength of carbon black paste, reduces production energy consumption and pollution, extends product shelf life, and meets the requirements of sustainable development.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon black slurry preparation, and in particular to an environmentally friendly carbon black slurry and a preparation process thereof. Background Art
[0002] With the rapid development of industrialization and urbanization, carbon black slurry, as an important industrial raw material, has been widely used in coatings, inks, rubber and other fields. However, there are many problems in the preparation process of traditional carbon black slurry, which not only affects the performance of the product, but also causes serious pollution to the environment.
[0003] (1) In the traditional carbon black slurry preparation process, the selection of dispersants is often relatively simple and the dispersing effect is poor, which leads to uneven dispersion of carbon black powder in the system and easy agglomeration, thereby affecting the stability and coloring power of the carbon black slurry. At the same time, due to improper selection of dispersants, it may also cause changes in the viscosity of the system, making the fluidity of the carbon black slurry worse, which brings inconvenience to subsequent processing.
[0004] (2) Secondly, the additives in traditional processes have limited effects and can only stabilize the carbon black slurry to a certain extent. However, over time, the stability of the carbon black slurry will gradually decrease, resulting in a decline in product quality. In addition, the addition of additives may also introduce new impurities, which will have an adverse effect on the purity of the product.
[0005] (3) The traditional carbon black pulp preparation process also has the problems of high energy consumption and heavy pollution. During the preparation process, a large amount of energy and raw materials are consumed, and a large amount of wastewater, waste gas and waste residue are generated, causing serious pollution to the environment. This not only increases production costs, but also violates the concept of sustainable development. Summary of the invention
[0006] The present invention not only improves the performance and quality of carbon black slurry by optimizing the raw material formula and the preparation process, but also reduces the production cost and environmental pollution, and has important practical application value and promotion significance.
[0007] The technical solution adopted by the present invention is: an environmentally friendly carbon black slurry, composed of the following raw materials in parts by weight: 25-40 parts of carbon black powder, 5-8 parts of dispersant, 3-6 parts of stabilizer, 1-3 parts of preservative, 1-2 parts of antistatic agent, 0.5-2 parts of thickener, 2-4 parts of defoaming agent, and 60-80 parts of deionized water.
[0008] As a further improvement of the present invention, the dispersant is one or more of nonionic polyacrylamide, sodium lauryl sulfate, fatty alcohol polyoxyethylene ether, sodium lignin sulfonate, and polyvinyl pyrrolidone K-30.
[0009] As a further improvement of the present invention, the stabilizer is one or more of hydroxyethyl methacrylate, methyl methacrylate, ethyl acrylate, isooctyl acrylate, and waterborne polyurethane.
[0010] As a further improvement of the present invention, the preservative is one or more of sodium benzoate, potassium sorbate, propionate, methyl parahydroxybenzoate, benzalkonium chloride, and cetyltrimethylammonium chloride.
[0011] As a further improvement of the present invention, the antistatic agent is one or more of glyceryl stearate and polyoxyethylene sorbitan monolaurate.
[0012] As a further improvement of the present invention, the thickener is one or more of hydroxyethyl cellulose, hydroxypropyl methyl cellulose, sodium carboxymethyl cellulose, and xanthan gum.
[0013] As a further improvement of the present invention, the defoaming agent is one or more of polysiloxane, silicone emulsion, and polyether-modified silicone oil.
[0014] A process for preparing an environmentally friendly carbon black slurry comprises the following steps:
[0015] Step 1: Weigh carbon black powder, dispersant, stabilizer, preservative, antistatic agent, thickener, defoamer, and deionized water according to weight proportions;
[0016] Step 2: Put the dispersant, stabilizer, preservative, antistatic agent, thickener, and defoamer into a mixing tank, add deionized water, and stir evenly to form a premixed solution;
[0017] Step 3: gradually add carbon black powder into the premixed liquid, and continue stirring to make the carbon black powder completely dispersed in the premixed liquid to form a uniform carbon black slurry initial liquid;
[0018] Step 4: Filter the prepared carbon black slurry liquid, and filter out impurities and non-dispersed carbon black particles in the carbon black slurry liquid through a sieve to obtain pure carbon black slurry.
[0019] As a further improvement of the present invention, the stirring speed in step 2 is controlled at 500-1000 rpm, and the stirring time is 10-20 minutes; the stirring speed in step 3 is controlled at 1200-2000 rpm, and the stirring time is 40-60 minutes.
[0020] As a further improvement of the present invention, the mesh size of the sieve in step 4 is 300 meshes.
[0021] Compared with the traditional carbon black slurry preparation technology, the environmentally friendly carbon black slurry and its preparation process of the present invention have the following significant advantages:
[0022] (1) The present invention optimizes the type and amount of dispersant to make the carbon black powder more evenly dispersed in the premixed liquid, effectively avoiding the occurrence of agglomeration; not only the stability and tinting power of the carbon black slurry are improved, but also the fluidity of the carbon black slurry is significantly improved, providing convenience for subsequent processing operations.
[0023] (2) Other additives are added to the present invention, including dispersants, stabilizers, preservatives, antistatic agents, thickeners and defoaming agents, so that the stability of the carbon black slurry is significantly improved. After long-term storage or use, the performance of the carbon black slurry remains stable, effectively extending the shelf life and service life of the product.
[0024] (3) In the preparation process of the present invention, impurities and non-dispersed carbon black particles in the carbon black slurry are effectively removed through a fine filtering step, thereby ensuring the purity of the product.
[0025] (4) Compared with the traditional process, the preparation process of the present invention has lower energy consumption and less pollution. Through reasonable raw material ratio and process optimization, it not only reduces the production cost, but also meets the requirements of sustainable development, which is of great significance for promoting the green development of the carbon black pulp industry. DETAILED DESCRIPTION
[0026] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0027] The invention provides an environmentally friendly carbon black slurry, which is composed of the following raw materials in parts by weight: 25-40 parts of carbon black powder, 5-8 parts of dispersant, 3-6 parts of stabilizer, 1-3 parts of preservative, 1-2 parts of antistatic agent, 0.5-2 parts of thickener, 2-4 parts of defoamer and 60-80 parts of deionized water.
[0028] The dispersant in the present invention is one or more of nonionic polyacrylamide, sodium lauryl sulfate, fatty alcohol polyoxyethylene ether, sodium lignin sulfonate, and polyvinyl pyrrolidone K-30 to ensure uniform dispersion of carbon black particles in the color paste.
[0029] The stabilizer in the present invention is one or more of hydroxyethyl methacrylate, methyl methacrylate, ethyl acrylate, isooctyl acrylate and waterborne polyurethane to improve the stability and durability of the color paste.
[0030] The preservative in the present invention is one or more of sodium benzoate, potassium sorbate, propionate, methyl paraben, benzalkonium chloride, and cetyltrimethylammonium chloride to extend the shelf life of the color paste.
[0031] The antistatic agent in the present invention is one or more of glyceryl stearate and polyoxyethylene sorbitan monolaurate, so as to reduce the surface resistance of the color paste and improve its antistatic performance.
[0032] The thickener in the present invention is one or more of hydroxyethyl cellulose, hydroxypropyl methyl cellulose, sodium carboxymethyl cellulose and xanthan gum to adjust the viscosity and fluidity of the color paste.
[0033] The defoaming agent in the present invention is one or more of polysiloxane, organosilicon emulsion and polyether modified silicone oil to eliminate the foam generated in the preparation process.
[0034] A preparation process of an environmentally friendly carbon black slurry comprises the following steps: weighing carbon black powder, a dispersant, a stabilizer, a preservative, an antistatic agent, a thickener, a defoamer and deionized water according to weight proportions; putting the dispersant, the stabilizer, the preservative, the antistatic agent, the thickener and the defoamer into a mixing tank, adding deionized water, controlling the stirring speed at 500-1000 rpm for 10-20 minutes, and forming a premixed liquid; gradually adding the carbon black powder into the premixed liquid, controlling the stirring speed at 1200-2000 rpm for 40-60 minutes, and making the carbon black powder completely dispersed in the premixed liquid to form a uniform carbon black slurry initial liquid; filtering the prepared carbon black slurry initial liquid, filtering out impurities and non-dispersed carbon black particles in the carbon black slurry initial liquid through a 300-mesh sieve, and obtaining a pure carbon black slurry.
[0035] Example 1
[0036] This embodiment 1 provides a process for preparing an environmentally friendly carbon black slurry, and the specific steps are as follows:
[0037] (i) According to weight, weigh 35 parts of carbon black powder, 6 parts of nonionic polyacrylamide, 4 parts of methyl methacrylate, 2 parts of sodium benzoate, 1.5 parts of glyceryl stearate, 1 part of hydroxyethyl cellulose, 3 parts of silicone emulsion, and 70 parts of deionized water;
[0038] (ii) placing nonionic polyacrylamide, methyl methacrylate, sodium benzoate, glyceryl stearate, hydroxyethyl cellulose, and silicone emulsion into a mixing tank, adding deionized water, controlling the stirring speed to 800 rpm, and the stirring time to 15 minutes to form a premixed solution;
[0039] (iii) gradually adding carbon black powder into the premixed liquid, controlling the stirring speed to 1600 rpm and the stirring time to 50 minutes, so that the carbon black powder is completely dispersed in the premixed liquid to form a uniform carbon black slurry initial liquid;
[0040] (iv) filtering the prepared carbon black slurry liquid, filtering out impurities and non-dispersed carbon black particles in the carbon black slurry liquid through a 300-mesh sieve to obtain pure carbon black slurry.
[0041] Example 2
[0042] This embodiment 2 provides a process for preparing an environmentally friendly carbon black slurry, and the specific steps are as follows:
[0043] (i) According to weight, weigh 30 parts of carbon black powder, 7 parts of nonionic polyacrylamide, 5 parts of methyl methacrylate, 2.5 parts of sodium benzoate, 1.5 parts of glyceryl stearate, 1.5 parts of hydroxyethyl cellulose, 2.5 parts of silicone emulsion, and 62 parts of deionized water;
[0044] (ii) placing nonionic polyacrylamide, methyl methacrylate, sodium benzoate, glyceryl stearate, hydroxyethyl cellulose, and silicone emulsion into a mixing tank, adding deionized water, controlling the stirring speed to 800 rpm, and the stirring time to 15 minutes to form a premixed solution;
[0045] (iii) gradually adding carbon black powder into the premixed liquid, controlling the stirring speed to 1600 rpm and the stirring time to 50 minutes, so that the carbon black powder is completely dispersed in the premixed liquid to form a uniform carbon black slurry initial liquid;
[0046] (iv) filtering the prepared carbon black slurry liquid, filtering out impurities and non-dispersed carbon black particles in the carbon black slurry liquid through a 300-mesh sieve to obtain pure carbon black slurry.
[0047] Example 3
[0048] This embodiment 3 provides a preparation process of an environmentally friendly carbon black slurry, and the specific steps are as follows:
[0049] (i) According to weight, weigh 35 parts of carbon black powder, 6 parts of nonionic polyacrylamide, 4 parts of methyl methacrylate, 2 parts of sodium benzoate, 1.5 parts of glyceryl stearate, 1 part of hydroxyethyl cellulose, 3 parts of silicone emulsion, and 70 parts of deionized water;
[0050] (ii) placing nonionic polyacrylamide, methyl methacrylate, sodium benzoate, glyceryl stearate, hydroxyethyl cellulose, and silicone emulsion into a mixing tank, adding deionized water, controlling the stirring speed to 600 rpm, and the stirring time to 18 minutes to form a premixed solution;
[0051] (iii) gradually adding carbon black powder into the premixed liquid, controlling the stirring speed to 1800 rpm and the stirring time to 45 minutes, so that the carbon black powder is completely dispersed in the premixed liquid to form a uniform carbon black slurry initial liquid;
[0052] (iv) filtering the prepared carbon black slurry liquid, filtering out impurities and non-dispersed carbon black particles in the carbon black slurry liquid through a 300-mesh sieve to obtain pure carbon black slurry.
[0053] Example 4
[0054] This embodiment 4 provides a preparation process of an environmentally friendly carbon black slurry, and the specific steps are as follows:
[0055] (i) According to weight, weigh 35 parts of carbon black powder, 6 parts of sodium lauryl sulfate, 4 parts of waterborne polyurethane, 2 parts of potassium sorbate, 1.5 parts of glyceryl stearate, 1 part of xanthan gum, 3 parts of silicone emulsion, and 70 parts of deionized water;
[0056] (ii) placing sodium lauryl sulfate, waterborne polyurethane, potassium sorbate, glyceryl stearate, xanthan gum, and silicone emulsion into a mixing tank, adding deionized water, controlling the stirring speed to 800 rpm for 15 minutes, and forming a premixed solution;
[0057] (iii) gradually adding carbon black powder into the premixed liquid, controlling the stirring speed to 1600 rpm and the stirring time to 50 minutes, so that the carbon black powder is completely dispersed in the premixed liquid to form a uniform carbon black slurry initial liquid;
[0058] (iv) filtering the prepared carbon black slurry liquid, filtering out impurities and non-dispersed carbon black particles in the carbon black slurry liquid through a 300-mesh sieve to obtain pure carbon black slurry.
[0059] Example 5
[0060] This embodiment 5 provides a process for preparing an environmentally friendly carbon black slurry, and the specific steps are as follows:
[0061] (i) According to weight proportions, weigh 35 parts of carbon black powder, 4 parts of nonionic polyacrylamide, 2 parts of sodium lignin sulfonate, 2 parts of methyl methacrylate, 2 parts of waterborne polyurethane, 2 parts of sodium benzoate, 1.5 parts of polyoxyethylene sorbitan monolaurate, 1 part of hydroxyethyl cellulose, 2 parts of organosilicon emulsion, 1 part of polyether-modified silicone oil, and 70 parts of deionized water;
[0062] (ii) placing nonionic polyacrylamide and sodium lignin sulfonate, methyl methacrylate and waterborne polyurethane, sodium benzoate, polyoxyethylene sorbitan monolaurate, hydroxyethyl cellulose, silicone emulsion and polyether modified silicone oil into a mixing tank, adding deionized water, controlling the stirring speed to 800 rpm, and the stirring time to 15 minutes to form a premixed solution;
[0063] (iii) gradually adding carbon black powder into the premixed liquid, controlling the stirring speed to 1600 rpm and the stirring time to 50 minutes, so that the carbon black powder is completely dispersed in the premixed liquid to form a uniform carbon black slurry initial liquid;
[0064] (iv) filtering the prepared carbon black slurry liquid, filtering out impurities and non-dispersed carbon black particles in the carbon black slurry liquid through a 300-mesh sieve to obtain pure carbon black slurry.
[0065] Performance Testing
[0066] The carbon black slurry obtained in the above Examples 1-5 was subjected to performance tests, specifically including: (1) measuring the pH value of the carbon black slurry; (2) placing the carbon black slurry in a 105°C oven for 3 hours and measuring its solid content; (3) using an NDJ-1 rotary viscosity tester to measure the viscosity of the carbon black slurry; (4) after maintaining the carbon black slurry at -18°C for 24 hours and then at 48°C for 24 hours, placing the carbon black slurry at room temperature for 2 hours, and observing the state of the carbon black slurry; (5) centrifuging the slurry at 3000 rpm for 30 minutes, and observing whether there is precipitation at the bottom of the centrifuge tube.
[0067] serial number pH Solid content Viscosity state Is there precipitation? Example 1 8.34 30.28% 434mPa.s Restore fluid status No precipitation Example 2 8.49 32.41% 378mPa.s Restore fluid status No precipitation Example 3 8.57 28.07% 427mPa.s Restore fluid status No precipitation Example 4 8.51 29.23% 395mPa.s Restore fluid status No precipitation Example 5 8.38 31.59% 413mPa.s Restore fluid status No precipitation
[0068] It can be seen from the above table that the carbon black slurry prepared by the present invention has good performance. (1) The carbon black slurries obtained in Examples 1-5 are maintained within a relatively favorable range in terms of pH value, solid content, viscosity, etc., indicating that these carbon black slurries have good stability and processability. (2) In the state test, the carbon black slurries obtained in Examples 1-5 can all return to a liquid state after undergoing temperature cycling, without obvious precipitation or solidification, which further proves that these carbon black slurries have excellent temperature resistance. (3) In the centrifugation test, the carbon black slurries obtained in Examples 1-5 did not precipitate after high-speed centrifugation, indicating that the carbon black powder was well dispersed in the premix to form a stable carbon black slurry.
[0069] In summary, the preparation process of the environmentally friendly carbon black slurry provided by the present invention is simple and easy to operate. The obtained carbon black slurry has good stability, temperature resistance and processability, and is suitable for various fields requiring carbon black slurry, such as coatings, inks, plastics, etc. At the same time, the carbon black slurry of the present invention also has the advantages of being environmentally friendly, non-toxic, and odorless, which meets the needs of modern industry for environmentally friendly materials.
[0070] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An environmentally friendly carbon black slurry, characterized in that: The invention is composed of the following raw materials in parts by weight: 25-40 parts of carbon black powder, 5-8 parts of dispersant, 3-6 parts of stabilizer, 1-3 parts of preservative, 1-2 parts of antistatic agent, 0.5-2 parts of thickener, 2-4 parts of defoamer and 60-80 parts of deionized water.
2. The environmentally friendly carbon black slurry according to claim 1, characterized in that: The dispersant is one or more of nonionic polyacrylamide, sodium lauryl sulfate, fatty alcohol polyoxyethylene ether, sodium lignin sulfonate, and polyvinyl pyrrolidone K-30.
3. The environmentally friendly carbon black slurry according to claim 1, characterized in that: The stabilizer is one or more of hydroxyethyl methacrylate, methyl methacrylate, ethyl acrylate, isooctyl acrylate, and waterborne polyurethane.
4. The environmentally friendly carbon black slurry according to claim 1, characterized in that: The preservative is one or more of sodium benzoate, potassium sorbate, propionate, methyl parahydroxybenzoate, benzalkonium chloride, and cetyltrimethylammonium chloride.
5. The environmentally friendly carbon black slurry according to claim 1, characterized in that: The antistatic agent is one or more of glyceryl stearate and polyoxyethylene sorbitan monolaurate.
6. The environmentally friendly carbon black slurry according to claim 1, characterized in that: The thickener is one or more of hydroxyethyl cellulose, hydroxypropyl methyl cellulose, sodium carboxymethyl cellulose and xanthan gum.
7. The environmentally friendly carbon black slurry according to claim 1, characterized in that: The defoaming agent is one or more of polysiloxane, silicone emulsion, and polyether modified silicone oil.
8. A process for preparing an environmentally friendly carbon black slurry, characterized in that: The following steps are involved: Step 1: Weigh carbon black powder, dispersant, stabilizer, preservative, antistatic agent, thickener, defoamer, and deionized water according to weight proportions; Step 2: Put the dispersant, stabilizer, preservative, antistatic agent, thickener, and defoamer into a mixing tank, add deionized water, and stir evenly to form a premixed solution; Step 3: gradually add carbon black powder into the premixed liquid, and continue stirring to make the carbon black powder completely dispersed in the premixed liquid to form a uniform carbon black slurry initial liquid; Step 4: Filter the prepared carbon black slurry liquid, and filter out impurities and non-dispersed carbon black particles in the carbon black slurry liquid through a sieve to obtain pure carbon black slurry.
9. The process for preparing an environmentally friendly carbon black slurry according to claim 8, characterized in that: The stirring speed in the step 2 is controlled at 500-1000 rpm, and the stirring time is 10-20 minutes; the stirring speed in the step 3 is controlled at 1200-2000 rpm, and the stirring time is 40-60 minutes.
10. The process for preparing an environmentally friendly carbon black slurry according to claim 8, characterized in that: The mesh size of the sieve in step 4 is 300 meshes.