Flame-retardant OSB aerogel spraying plate and manufacturing method thereof

By preparing hydrophobic flame retardant agel under normal pressure and electrostatically spraying it on OSB boards, combining acidic flame retardant and silane polycondensation technology to form a flame retardant closely fixed in the silane framework, the smoke gas in the prior art is solved Problems and high cost problems have achieved efficient and simple improvement of flame retardant performance and smoke suppression effects.

CN118895070APending Publication Date: 2024-11-05DEHUA TB NEW DECORATION MATERIAL CO LTD

Patent Information

Application Number
CN202411093293.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

When the prior art improves the flame retardant performance of artificial boards, it cannot effectively solve the flue gas problem, and the process is complex and the cost is high. The traditional flame retardant coating has poor durability and low production efficiency, which cannot meet the production needs of flame retardant plywood.

Method used

Prepared with hydrophobic flame retardant agel under normal pressure, sprayed on the surface of OSB boards through electrostatic spraying technology, combined with acidic flame retardants such as ammonium sulfate and boric acid, and hydrolyzed with ammonium polyphosphate and ammonium water to form a tightly fixed in the silane polycondensation framework. The flame retardant is used to exchange solvents with n-hexane, which reduces density and improves porosity. Components such as expanded graphite and zinc borate are added to form a dense porous structure, which improves flame retardant and heat insulation performance and smoke suppression effect.

Benefits of technology

Achieve simple and efficient preparation of flame retardant OSB aerogel spray board, improves flame retardant and heat insulation performance, reduces smoke production, avoids moisture absorption problems of traditional flame retardants, and improves the anti-hygroscopic performance and anti-hygroscopic resistance of the product. Mold properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004987169610000101
    Figure BDA0004987169610000101
  • Figure BDA0004987169610000102
    Figure BDA0004987169610000102
  • Figure BDA0004987169610000111
    Figure BDA0004987169610000111
Patent Text Reader

Abstract

The invention belongs to the field of normal-pressure preparation of flame-retardant aerogel and manufacturing of flame-retardant plates, and particularly relates to a flame-retardant OSB aerogel spraying plate and a manufacturing method thereof.The spraying plate is prepared by spraying aerogel flame-retardant paint to the surface of a plate in an electrostatic spraying mode and then curing a coating, the spraying plate comprises two parts, the first part is an OSB base material, the second part is an OSB base material, and the third part is an OSB base material; the second part is a flame-retardant coating with a flame-retardant effect, and the flame-retardant coating is formed by spraying an aerogel coating with a flame-retardant effect. The hydrophobic flame-retardant aerogel adopted by the invention is prepared by adopting an air dry oven at normal pressure, freeze drying and supercritical drying technologies are not needed, the preparation process is simple and convenient, the energy consumption is low, and the product yield is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of normal pressure preparation of flame retardant gas gel and flame retardant board manufacturing, and specifically relates to a flame retardant OSB aerogel spraying board and a manufacturing method thereof. Background Art

[0002] At a time when fires in high-rise buildings are frequent and fires in public places continue to threaten people's lives and property, consumers are paying more and more attention to the flame retardant properties of building materials. In fire accident statistics, the number of people killed by thick smoke is 4 to 5 times that of those burned. In a fire, thick smoke spreads faster than flames, becoming the "first killer" in the fire scene. However, there are currently few studies on smoke in the flame retardant research of artificial boards, and most of them only study flame retardant properties. At present, there are three main methods for improving the flame retardant properties of artificial boards: impregnation flame retardant, inorganic adhesive layer flame retardant method, and flame retardant coating flame retardant method.

[0003] The impregnation method is a common method used for wood flame retardancy, which has a simple treatment process, high flame retardancy efficiency and good flame retardancy effect. For example, a wood flame retardant impregnation treatment method mentioned in CN202210698997.7 uses a multiple impregnation method to impregnate the flame retardant into the wood in batches, and combines inside the wood to form new compounds. However, since its impregnation component contains highly hygroscopic inorganic salts such as ammonium phosphate, it cannot solve the problem of high moisture absorption of the product. The inorganic adhesive layer flame retardant method generally uses silicate substances, which use their own adhesiveness after water loss to combine the wood units together, and rely on the flame retardant and heat-insulating properties of the inorganic material itself to give the board flame retardant properties. For example: CN202110095861.2 mentioned a high-temperature resistant inorganic adhesive, whose base liquid uses sodium silicate or potassium silicate inorganic silicates, which are combined with plasticizers and additives. Although this type of inorganic adhesive has excellent flame retardant and anti-hygroscopic properties, it is prone to defects such as short active period, high finished product density, and transportation difficulties when used in combination with artificial boards. The above flame retardant treatment process cannot solve the problem of smoke generated by wood materials during combustion. The smoke production of the products is mostly only S2 level, which cannot achieve the purpose of smoke suppression.

[0004] From the development history of flame retardant of artificial board, flame retardant coating is the ultimate direction of development. Its operation process is simple and its applicability is strong. It can meet the flame retardant requirements of various substrates, but the cost of flame retardant coating is generally high. For example, CN102218883B mentions a silicon-containing flame retardant coating used in wood-plastic board. It uses epoxy resin as the matrix, and adds silicon-based flame retardant to it and then coats it on the surface of the board to give the board flame retardant properties. This type of flame retardant coating has poor durability and only uses heat absorption and heat insulation. The flame retardant effect is poor, the coating dries slowly, and the production efficiency is low, which cannot meet the production needs of flame-retardant plywood.

[0005] Aerogel is known as the "lightest solid in the world". Its ultra-low density and super thermal insulation properties make it widely used in the fields of spacecraft thermal insulation materials, thermal insulation clothing, etc., but materials that combine aerogel with wood are rare. In CN201510138085.4, it is mentioned that ammonium polyphosphate and silane precursor solution are mixed together and impregnated in wood, and condensation is formed inside the wood to form aerogel, which ultimately gives the wood flame retardant and thermal insulation properties. However, this type of method has a complex preparation process, serious loss of raw materials, high production costs, and low practicality. Summary of the invention

[0006] In order to solve the defects and shortcomings in the above-mentioned prior art, the present invention provides a flame-retardant OSB aerogel sprayed board and a preparation method thereof, which is prepared by a blast drying oven under normal pressure without freeze drying and supercritical drying technology, has a simple preparation process, low energy consumption and high product yield.

[0007] The technical solution of the present invention is a flame-retardant OSB aerogel sprayed board, which is prepared by spraying an aerogel flame-retardant coating onto the surface of the board by electrostatic spraying and then curing the coating. The sprayed board comprises two parts. The first part is an OSB substrate, and the second part is a flame-retardant coating with a flame-retardant effect. The flame-retardant coating is sprayed with an aerogel coating with a flame-retardant effect.

[0008] Preferably, the spray plate uses two or three of methyltriethoxysilane, dimethyldiethoxysilane and tetraethoxysilane as precursors, a mixed solution of boric acid, ammonium sulfate and oxalic acid as an acid regulator, and a mixed solution of ammonium polyphosphate and ammonia water as an alkali regulator.

[0009] Preferably, the flame retardant coating is composed of a base liquid, an aerogel mixed liquid, ammonium polyphosphate, dipentaerythritol, kaolin, aluminum hydroxide, molybdenum trioxide, zinc borate, expanded graphite, and a silane coupling agent.

[0010] Preferably, the flame retardant coating contains 60-80 parts by mass of base liquid, 30-60 parts by mass of aerogel mixed liquid, 1-3 parts of expanded graphite, 5-10 parts of dipentaerythritol, 15-30 parts of ammonium polyphosphate, 5-10 parts of zinc borate, 5-10 parts of aluminum hydroxide, 6-8 parts of molybdenum trioxide, 5-10 parts of kaolin, and 0.1-0.5 parts of silane coupling agent.

[0011] Preferably, the base liquid of the flame retardant coating may be any one of melamine resin, epoxy resin and polyvinyl acetate emulsion.

[0012] Preferably, the specific preparation method of the acid regulator is to add 10 parts by mass of ammonium sulfate, 4 parts by mass of boric acid and 4 parts by mass of oxalic acid into 100 parts by mass of pure water.

[0013] Preferably, the specific preparation method of the alkali regulator is to add 4 parts by mass of ammonium polyphosphate and 17 parts by mass of ammonia water to 100 parts by mass of pure water.

[0014] Preferably, the OSB substrate is an artificial board prepared by using narrow, long, flat large-piece wood chips through directional paving technology, and the surface of the OSB board needs to be initially sanded before subsequent spraying treatment.

[0015] Preferably, the methyltriethoxysilane, dimethyldiethoxysilane, tetraethoxysilane and n-hexane are analytical grade reagents.

[0016] A method for manufacturing a flame retardant OSB aerogel sprayed board, the steps are as follows:

[0017] Step S1. Add 0.5-1% of hexadecyltrimethylammonium chloride (CTAC) surfactant and 10-25% of anhydrous ethanol to pure water, stir and mix, and record as solution A;

[0018] Step S2. Place solution A in a magnetic stirrer and stir for 10-15 minutes, take it out after CTAC is completely dissolved, add a mixed silane precursor solution thereto, wherein the molar ratio of silane to water is between 10-40, add a mixed solution of ammonium sulfate, boric acid, and oxalic acid thereto to adjust the pH to 2-3, and mark the solution as B, seal the container, place it in a magnetic stirrer and stir for 2-3 hours, take it out after the turbid emulsion becomes clear and transparent again, adjust the pH to 7 with a mixed solution of ammonium polyphosphate and ammonia water, and let it stand for 2 hours to gel;

[0019] Step S3. Add 2-3 times the volume of anhydrous ethanol to the wet gel, and place it in a constant temperature and humidity chamber for aging. The temperature of the constant temperature and humidity chamber is set to 35°C and the humidity is set to 90%. The anhydrous ethanol is replaced every 12 hours for aging for 36 hours.

[0020] Step S4. Pour out the aged solution, add 1-2 times the volume of the wet gel n-hexane solution to the aged solution for solvent exchange, exchange once every 8 hours, and repeat 3 times;

[0021] Step S5. The wet gel after the solvent exchange is taken out and dried in a blast drying oven to finally obtain an aerogel with a flame retardant effect. The aerogel is crushed into a powder with uniform particles and sieved for later use;

[0022] Step S6. Add 10-25 parts by mass of aerogel powder and 3-5 parts by mass of silica powder to a mixed solution of anhydrous ethanol and pure water, add 0.1-1 parts by mass of CTAC and 0.1-0.5 parts by mass of a defoamer, and stir evenly with a magnetic stirrer to prepare an aerogel mixed solution;

[0023] Step S7. Perform multiple sanding processes on the OSB substrate to ensure the surface flatness of the substrate, remove the oil film layer on the surface of the substrate, and improve the adhesion of the coating;

[0024] Step S8: Electrostatic spraying is used to evenly spray the board, and after the coating is cured, the desired flame-retardant OSB aerogel sprayed board can be obtained.

[0025] Compared with the prior art, the present invention provides a flame-retardant OSB aerogel spraying board and a preparation method thereof, which has the following advantages over other flame-retardant coating boards and aerogel coatings:

[0026] 1. The hydrophobic, flame-retardant gel used in the present invention is prepared in a blast drying oven under normal pressure, without freeze drying and supercritical drying technology, and has a simple preparation process, low energy consumption and high product yield;

[0027] 2. In order to improve the flame retardant properties of aerogel, the present invention innovatively combines acidic flame retardants such as ammonium sulfate and boric acid with traditional acidic regulator oxalic acid solution to hydrolyze silane hydrolyzate, and uses ammonium polyphosphate and ammonia water as alkaline regulators to polycondense the hydrolyzed silane, so that the flame retardant is tightly fixed in the SISi gel skeleton after drying. Thanks to the presence of methyl groups in the silane precursor, the aerogel has a certain hydrophobicity, so that the flame retardant wrapped in the aerogel is not affected by moisture, that is, the flame retardant properties of the aerogel are improved while avoiding the defect of easy moisture absorption of traditional flame retardants;

[0028] 3. The present invention uses n-hexane as a solvent exchange agent. After aging, n-hexane is used to replace the water in the wet gel capillaries. Thanks to the hydrophobicity of the methyl groups in n-hexane, the capillary force caused by water evaporation during the drying process is reduced, the collapse of the capillaries is avoided, the porosity of the aerogel is improved, and the density of the aerogel is reduced, thereby improving the flame retardant and heat insulation properties of the aerogel;

[0029] 4. The aerogel mixed liquid in the flame retardant coating mentioned in the present invention is the main component. The main function of the aerogel is the flame retardant effect of SIOSi and the heat insulation performance brought by its porosity. In addition, due to the porous structure of the aerogel, the smoke generated by combustion can be adsorbed to reduce the final smoke production, thereby achieving the purpose of smoke suppression.

[0030] 5. In the flame-retardant coating mentioned in the present invention, ammonium polyphosphate, dipentaerythritol, and expanded graphite are important components of the expanded flame-retardant coating, which can form a dense and porous carbon layer and play a role in heat insulation and flame retardancy, while the role of zinc borate and molybdenum trioxide is to act as smoke suppression fillers. When combined with the porous aerogel, the flame-retardant coating can have an excellent smoke suppression effect. Kaolin contains elements such as oxygen, silicon, and aluminum, among which aluminum oxide is an important oxidant. Its extremely high combustion temperature and barrier effect can reduce the heat released by combustion. In kaolin, aluminum oxide can form a protective aluminum oxide layer from bottom to top under the high temperature of fire. Aluminum hydroxide can also be dehydrated at high temperature to form aluminum oxide and water to further weaken the oxygen content. The formed aluminum oxide can reinforce the expanded carbon layer, thereby avoiding the collapse of the expanded carbon layer under the impact of flames.

[0031] 6. The OSB board used in the method of the present invention is a particle-based artificial board prepared from narrow long flat wood chips. After hot pressing, it needs to be sanded by 2 heavy sanding machines and 2 light sanding machines to ensure the flatness of the board surface, thereby ensuring the final thickness uniformity of the coating. DETAILED DESCRIPTION

[0032] The technical solution proposed by the present invention will be described in more detail below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments described in the present invention and cannot represent the required technical methods described in the present invention. Technical variations made based on the present invention are all within the technical protection scope of the present invention.

[0033] Example 1

[0034] A flame retardant OSB aerogel spraying board is prepared by using methyltrimethoxysilane and dimethyldiethoxysilane as a precursor solution.

[0035] A method for manufacturing a flame retardant OSB aerogel sprayed board, the steps are as follows:

[0036] S1. Add 1 part by mass of hexadecyltrimethylammonium chloride (CTAC) surfactant and 15 parts by mass of anhydrous ethanol to 100 parts by mass of pure water, put them on a magnetic stirrer and mix them evenly. After CTAC is completely dissolved, it is recorded as solution A.

[0037] S2, adding 10 parts by mass of ammonium sulfate, 4 parts by mass of boric acid, and 4 parts by mass of oxalic acid to 100 parts by mass of pure water to prepare an acid regulator;

[0038] S3, add methyltriethoxysilane and dimethyldiethoxysilane in a molar ratio of 4:3 and a water-silicon molar ratio of 15 to solution A, add an acid regulator dropwise thereto to adjust the pH to 3, continue stirring for 2 hours, and take out the solution after it becomes clear and transparent;

[0039] S4. Add an alkaline catalyst to the silane hydrolyzate, adjust the pH to 7, and let it stand for 2 hours to gel.

[0040] S5. Add anhydrous ethanol twice the volume of the wet gel to the wet gel and place it in a constant temperature and humidity chamber for aging. The temperature of the constant temperature and humidity chamber is set to 35° C. and the humidity is set to 90%. The anhydrous ethanol is replaced every 12 hours for 36 hours of aging.

[0041] S6. Pour out the aging solution and add a hexane solution with a volume that is 1 times the volume of the wet gel to perform solvent exchange. Do this every 8 hours and repeat for 3 times.

[0042] S7. Take out the wet gel after solvent exchange, cover the surface of the wet gel with a film and pierce several fine holes for exhaust, and use a forced air drying oven to dry it. The drying procedure is 40°C, 60°C, 80°C, and 100°C for 2 hours each. Grind the dried aerogel into powder and pass it through a 200-mesh sieve for later use.

[0043] S8. Add 15 parts by mass of aerogel and 3 parts by mass of silica powder to a mixed solution of 8 parts by mass of anhydrous ethanol and 40 parts by mass of pure water, add 0.2 parts by mass of CTAC and 0.1 parts by mass of a defoaming agent thereto, stir evenly using a magnetic stirrer to prepare an aerogel mixed solution.

[0044] S9. Add 40 parts of aerogel mixed liquid, 1 part of expanded graphite, 5 parts of dipentaerythritol, 25 parts of ammonium polyphosphate, 5 parts of zinc borate, 5 parts of aluminum hydroxide, 8 parts of molybdenum trioxide, 5 parts of kaolin and 0.3 parts of silane coupling agent to 60 parts of white latex, stir well and set aside.

[0045] S10. Perform 4 sanding processes on the OSB substrate to ensure the surface flatness of the substrate, remove the oil film layer on the substrate surface, and improve the adhesion of the paint.

[0046] S11. The board is evenly sprayed by electrostatic spraying, with a total coating thickness of 1 mm. After the coating is cured, the required flame-retardant OSB aerogel sprayed board can be obtained.

[0047] Example 2

[0048] A flame retardant OSB aerogel spraying board is prepared by using dimethyldiethoxysilane and tetraethoxysilane as a precursor solution.

[0049] A method for manufacturing a flame retardant OSB aerogel sprayed board, the steps are as follows:

[0050] S1. Add 1 part by mass of hexadecyltrimethylammonium chloride (CTAC) surfactant and 15 parts by mass of anhydrous ethanol to 100 parts by mass of pure water, put them on a magnetic stirrer and mix them evenly. After CTAC is completely dissolved, it is recorded as solution A.

[0051] S2, adding 10 parts by mass of ammonium sulfate, 4 parts by mass of boric acid, and 4 parts by mass of oxalic acid to 100 parts by mass of pure water to prepare an acid regulator;

[0052] S3, dimethyldiethoxysilane and tetraethoxysilane are added to solution A in a molar ratio of 17:10 and a water-silicon molar ratio of 40, and an acid regulator is added dropwise to adjust the pH to 3, and stirring is continued for 2 hours. After the solution becomes clear and transparent, it is taken out;

[0053] S4. Add an alkaline catalyst to the silane hydrolyzate, adjust the pH to 7, and let it stand for 2 hours to gel.

[0054] S5. Add 1.5 times the volume of anhydrous ethanol to the wet gel and place it in a constant temperature and humidity chamber for aging. The temperature of the constant temperature and humidity chamber is set to 35° C. and the humidity is set to 90%. The anhydrous ethanol is replaced every 12 hours for aging for 24 hours.

[0055] S6. Pour out the aging solution and add a hexane solution twice the volume of the wet gel to perform solvent exchange. Do this every 8 hours and repeat for 3 times.

[0056] S7. Take out the wet gel after solvent exchange, cover the surface of the wet gel with a film and pierce several fine holes for exhaust, and dry it in a blast drying oven. The drying procedure is 60°C and 80°C for 10 hours each. Grind the dried aerogel into powder and pass it through a 200-mesh sieve for later use.

[0057] S8. Add 15 parts by mass of aerogel and 3 parts by mass of silica powder to a mixed solution of 8 parts by mass of anhydrous ethanol and 50 parts by mass of pure water, add 0.3 parts by mass of CTAC and 0.15 parts by mass of a defoaming agent thereto, stir evenly using a magnetic stirrer to prepare an aerogel mixed solution.

[0058] S9. Add 40 parts of aerogel mixed liquid, 1 part of expanded graphite, 8 parts of dipentaerythritol, 20 parts of ammonium polyphosphate, 4 parts of zinc borate, 4 parts of aluminum hydroxide, 6 parts of molybdenum trioxide, 8 parts of kaolin, 0.5 parts of silane coupling agent and 3 parts of flour to 60 parts of white latex, stir well and set aside.

[0059] S10. Perform 4 sanding processes on the OSB substrate to ensure the surface flatness of the substrate, remove the oil film layer on the substrate surface, and improve the adhesion of the paint.

[0060] S11. The board is evenly sprayed by electrostatic spraying, with a total coating thickness of 1 mm. After the coating is cured, the required flame-retardant OSB aerogel sprayed board can be obtained.

[0061] Example 3

[0062] A flame retardant OSB aerogel spraying board is prepared by using methyltriethoxysilane, dimethyldiethoxysilane and tetraethoxysilane as a precursor solution.

[0063] A method for manufacturing a flame retardant OSB aerogel sprayed board, the steps are as follows:

[0064] S1. Add 1 part by mass of hexadecyltrimethylammonium chloride (CTAC) surfactant and 15 parts by mass of anhydrous ethanol to 100 parts by mass of pure water, put them on a magnetic stirrer and mix them evenly. After CTAC is completely dissolved, it is recorded as solution A.

[0065] S2, adding 10 parts by mass of ammonium sulfate, 4 parts by mass of boric acid, and 4 parts by mass of oxalic acid to 100 parts by mass of pure water to prepare an acid regulator;

[0066] S3, adding methyltriethoxysilane, dimethyldiethoxysilane and tetraethoxysilane in a molar ratio of 16:49:10 and a water-silicon molar ratio of 13 to solution A, adding an acid regulator dropwise therein to adjust the pH to 3, and continuing stirring for 3 hours before taking out;

[0067] S4. Add an alkaline catalyst to the silane hydrolyzate, adjust the pH to 7, and let it stand for 2 hours to gel.

[0068] S5. Add 1.5 times the volume of anhydrous ethanol to the wet gel and place it in a constant temperature and humidity chamber for aging. The temperature of the constant temperature and humidity chamber is set to 30° C. and the humidity is set to 90%. The anhydrous ethanol is replaced every 12 hours for aging for 24 hours.

[0069] S6. Pour out the aging solution and add a hexane solution twice the volume of the wet gel to perform solvent exchange. Do this every 8 hours and repeat for 3 times.

[0070] S7. Take out the wet gel after solvent exchange, cover the surface of the wet gel with a film and pierce several fine holes for exhaust, and use a forced air drying oven to dry it. The drying procedure is 40°C, 60°C, 80°C, and 100°C for 2 hours each. Grind the dried aerogel into powder and pass it through a 200-mesh sieve for later use.

[0071] S8. Add 25 parts by mass of aerogel and 5 parts by mass of silica powder to a mixed solution of 4 parts by mass of anhydrous ethanol and 75 parts by mass of pure water, add 0.5 parts by mass of CTAC and 0.1 parts by mass of a defoaming agent thereto, and stir evenly using a magnetic stirrer to prepare an aerogel mixed solution.

[0072] S9. Add 60 parts of aerogel mixed liquid, 1 part of expanded graphite, 10 parts of dipentaerythritol, 30 parts of ammonium polyphosphate, 4 parts of zinc borate, 6 parts of aluminum hydroxide, 8 parts of molybdenum trioxide, 10 parts of kaolin and 0.3 parts of silane coupling agent to 80 parts of white latex, stir well and set aside.

[0073] S10. Perform 4 sanding processes on the OSB substrate to ensure the surface flatness of the substrate, remove the oil film layer on the substrate surface, and improve the adhesion of the paint.

[0074] S9. The board is evenly sprayed by electrostatic spraying, with a total coating thickness of 1 mm. After the coating is cured, the required flame-retardant OSB aerogel spray board can be obtained.

[0075] Comparative Example

[0076] Here are the steps:

[0077] S1. Preparation of flame retardant solution for dipping: add 10 parts of purchased phosphate flame retardant to 100 parts by mass of water;

[0078] S2. Select veneers with no scars, insect bites or other defects on the surface as the impregnation raw materials, put the veneers neatly into the vacuum pressure impregnation tank, and pour the prepared flame retardant solution into the liquid storage tank. Set the vacuum degree to -0.06Mpa, the vacuum time to 30min, and after the vacuum is completed, perform pressurized impregnation with a pressure of 0.8Mpa and a pressurized impregnation time of 2h. After the pressurized impregnation is completed, take out the veneer for atmospheric drying and dry the veneer to a moisture content of less than 25%.

[0079] S3, base board assembly: the dried single board is staggered and glued, and the glue amount is about 200g / ㎡.

[0080] S4, cold pressing and hot pressing of substrate: cold pressing unit pressure 0.65Mpa, cold pressing time 2h, hot pressing pressure 0.7Mpa, hot pressing time: 12min, hot pressing temperature: 125℃;

[0081] S7, base material fabric: cut the base material and use the technical wood veneer for fabric, the fabric glue amount is 100g / ㎡, cold pressing for 30 minutes, cold pressing unit pressure is 0.7Mpa. Hot pressing temperature is 115℃, hot pressing pressure is 0.7Mpa, and hot pressing time is 5min. After hot pressing, the required control group test sample can be obtained.

[0082] Test results

[0083] In order to highlight the advantages of the present invention, the present invention prepares a control group sample according to the manufacturing method of the conventional flame retardant board, and the improvement of the present invention is highlighted by comparing the test results of Examples 1-3 with the comparative example. By conducting hygroscopic performance tests (test standard is LY / T 3036-2018), monomer combustion test (judgment standard is GB 8624-2012), formaldehyde emission test (reference standard GB / T39600-2021), mildew resistance grade test (JC / T 2039-2010), and metal corrosion resistance test (AWPA E12-20·) on the examples and the control group, it can be clearly seen that the examples have good anti-hygroscopic performance, excellent flame retardant performance, good thermal insulation performance, good smoke suppression effect, good metal corrosion resistance and mildew resistance.

[0084] The flame retardant properties of the flame retardant coating were tested by ignition experiments. After burning the surface coating by the flame spray method, it was found that the coating generated a 7mm thick expanded carbon layer after 60s of fire. After scraping off the expanded carbon layer, the flame retardant coating was not burned through. The corresponding char layer of the wood layer of the flame retardant plywood is 3mm.

[0085] Hygroscopicity:

[0086] name Day 1 Day 2 Day 3 Day 4 Day 5 Day 6 Day 7 Example 1 6.46% 11.08% 14.29% 14.87% 15.48% 15.18% 15.42% Example 2 6.33% 10.96% 14.23% 14.80% 15.26% 15.19% 15.20% Example 3 5.88% 10.47% 14.34% 15.14% 15.43% 15.45% 15.24% Comparison Example 5.77% 13.49% 20.44% 23.89% 24.96% 27.07% 29.18%

[0087] Other physical and chemical properties:

[0088]

[0089] Flame retardant properties:

[0090] Single combustion test results

[0091]

[0092]

[0093] The above are some embodiments of the present invention. Although the content of the present invention has been described in detail through the above embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be obvious to those skilled in the art for various modifications and substitutions of the present invention. Therefore, the protection scope of the present invention should be limited by the attached claims.

Claims

1. A flame retardant OSB aerogel sprayed board, It is characterized in that The sprayed board is prepared by spraying aerogel flame retardant coating onto the surface of the board by electrostatic spraying and then curing the coating. It consists of two parts. The first part is an OSB substrate, and the second part is a flame retardant coating with a flame retardant effect. The flame retardant coating is sprayed with aerogel coating with a flame retardant effect.

2. The flame retardant OSB aerogel sprayed board according to claim 1, It is characterized in that The spraying plate uses two or three of methyltriethoxysilane, dimethyldiethoxysilane and tetraethoxysilane as precursors, a mixed solution of boric acid, ammonium sulfate and oxalic acid as an acid regulator, and a mixed solution of ammonium polyphosphate and ammonia water as an alkali regulator.

3. The flame retardant OSB aerogel sprayed board according to claim 2, It is characterized in that The flame retardant coating consists of base liquid, aerogel mixed liquid, ammonium polyphosphate, dipentaerythritol, kaolin, aluminum hydroxide, molybdenum trioxide, zinc borate, expanded graphite and silane coupling agent components.

4. The flame retardant OSB aerogel sprayed board according to claim 3, It is characterized in that The flame retardant coating contains 60-80 parts by mass of base liquid, 30-60 parts by mass of aerogel mixed liquid, 1-3 parts of expanded graphite, 5-10 parts of dipentaerythritol, 15-30 parts of ammonium polyphosphate, 5-10 parts of zinc borate, 5-10 parts of aluminum hydroxide, 6-8 parts of molybdenum trioxide, 5-10 parts of kaolin and 0.1-0.5 parts of silane coupling agent.

5. The flame retardant OSB aerogel sprayed board according to claim 1, It is characterized in that The base liquid of the flame retardant coating may be any one of melamine resin, epoxy resin and polyvinyl acetate emulsion.

6. The flame retardant OSB aerogel sprayed board according to claim 4, It is characterized in that The specific preparation method of the acid regulator is as follows: 10 parts by mass of ammonium sulfate, 4 parts by mass of boric acid, and 4 parts by mass of oxalic acid are added to 100 parts by mass of pure water.

7. The flame retardant OSB aerogel sprayed board according to claim 4, It is characterized in that The specific preparation method of the alkali regulator is as follows: 4 parts by mass of ammonium polyphosphate and 17 parts by mass of ammonia water are added to 100 parts by mass of pure water.

8. The flame retardant OSB aerogel sprayed board according to claim 2, It is characterized in that The OSB substrate is an artificial board made of narrow, long, flat large pieces of wood shavings through directional paving technology. The surface of the OSB board needs to be initially sanded before subsequent spraying treatment.

9. The flame retardant OSB aerogel sprayed board according to claim 2, It is characterized in that The methyltriethoxysilane, dimethyldiethoxysilane, tetraethoxysilane and n-hexane are analytical grade reagents.

10. A method for manufacturing the flame retardant OSB aerogel sprayed board as claimed in claim 7, It is characterized in that Here are the steps: Step S1. Add 0.5-1% of hexadecyltrimethylammonium chloride (CTAC) surfactant and 10-25% of anhydrous ethanol to pure water, stir and mix, and record as solution A; Step S2. Place solution A in a magnetic stirrer and stir for 10-15 minutes, take it out after CTAC is completely dissolved, add a mixed silane precursor solution thereto, wherein the molar ratio of silane to water is between 10-40, add a mixed solution of ammonium sulfate, boric acid, and oxalic acid thereto to adjust the pH to 2-3, and mark the solution as B, seal the container, place it in a magnetic stirrer and stir for 2-3 hours, take it out after the turbid emulsion becomes clear and transparent again, adjust the pH to 7 with a mixed solution of ammonium polyphosphate and ammonia water, and let it stand for 2 hours to gel; Step S3. Add 2-3 times the volume of anhydrous ethanol to the wet gel, and place it in a constant temperature and humidity chamber for aging. The temperature of the constant temperature and humidity chamber is set to 35°C and the humidity is set to 90%. The anhydrous ethanol is replaced every 12 hours for aging for 36 hours. Step S4. Pour out the aged solution, add 1-2 times the volume of the wet gel n-hexane solution to the aged solution for solvent exchange, exchange once every 8 hours, and repeat 3 times; Step S5. The wet gel after the solvent exchange is taken out and dried in a blast drying oven to finally obtain an aerogel with a flame retardant effect. The aerogel is crushed into a powder with uniform particles and sieved for later use; Step S6. Add 10-25 parts by mass of aerogel powder and 3-5 parts by mass of silica powder to a mixed solution of anhydrous ethanol and pure water, add 0.1-1 parts by mass of CTAC and 0.1-0.5 parts by mass of a defoamer, and stir evenly with a magnetic stirrer to prepare an aerogel mixed solution; Step S7. Perform multiple sanding processes on the OSB substrate to ensure the surface flatness of the substrate, remove the oil film layer on the surface of the substrate, and improve the adhesion of the coating; Step S8: The board is evenly sprayed by electrostatic spraying, and the desired flame-retardant OSB aerogel sprayed board can be obtained after the coating is cured.

Citation Information

Patent Citations

  • Wood plastic plate coated by silicone flame retardant coating

    CN102218883B

  • Ammonium polyphosphate / SiO2 composite aerogel flame-retardant reinforced timber and preparation method thereof

    CN104760103A

  • High-temperature-resistant inorganic adhesive and preparation method thereof

    CN112898904A

  • Wood flame-retardant dipping treatment method

    CN114986634A

  • Method for preparing highly-transparent hydrophobic integrated block body silicon dioxide aerogel through normal pressure drying

    CN107686117A

Cited By

  • Flame-retardant sponge material as well as preparation method and application thereof

    CN119798962A