Surface treatment agent for copper foil and surface treatment method thereof

Through the surface treatment technology of nanoparticle-enhanced silane coupling agent and graphene and other materials, the problems of environmental pollution and insufficient performance in traditional copper foil processes are solved, and higher mechanical strength, corrosion resistance and electrical conductivity are achieved. It is suitable for use in traditional copper foil processes. Demand for high-performance electronic products.

CN118895076APending Publication Date: 2024-11-05JIANGXI NORD COPPER FOIL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410828152.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Traditional copper foil manufacturing and surface treatment processes have problems such as environmental pollution, high energy consumption and insufficient performance, which is difficult to meet the needs of environmental protection regulations and high-performance electronic equipment in modern society.

Method used

The surface treatment agent of nanoparticle enhanced silane coupling agent, bio-based epoxy resin, intelligent curing agent and graphene additive is carried out in combination with ultrasonic cleaning, plasma treatment, electrospray coating and multi-stage curing technology. deal with.

Benefits of technology

It significantly reduces environmental pollution and energy consumption, improves the mechanical strength, corrosion resistance and electrical conductivity of copper foil, is suitable for the needs of high-performance electronic products, and optimizes the flexibility and cost of the production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895076A_ABST
    Figure CN118895076A_ABST
Patent Text Reader

Abstract

The invention relates to the field of material science and electronic engineering, and discloses a copper foil surface treating agent which comprises the following components in percentage by weight: 1%-5% of a nanoparticle enhanced silane coupling agent, 50%-80% of bio-based epoxy resin, 10%-15% of an intelligent curing agent, 15%-30% of a multifunctional solvent and 0.5%-2% of a graphene additive, the invention also discloses a surface treatment method of the surface treatment agent for the copper foil, which comprises the following steps: S1, pretreatment and surface activation: ultrasonic cleaning: deeply cleaning the copper foil for 10-15 minutes by using an ultrasonic bath and a bio-based solvent at the temperature of 50-60 DEG C, setting the ultrasonic frequency at 35-45 kHz, removing surface impurities and microcosmically activating the copper surface. By using the bio-based epoxy resin and the bio-based solvent, the dependence on traditional chemicals is reduced, the environmental pollution and the consumption of non-renewable resources are reduced, and by using the nanoparticle enhanced silane coupling agent and the graphene additive, the mechanical strength, the corrosion resistance and the conductivity of the copper foil are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of material science and electronic engineering, and in particular to a surface treatment agent for copper foil and a surface treatment method thereof. Background Art

[0002] Copper foil is an indispensable conductive material in electronic products, printed circuit boards (PCBs), lithium batteries and other fields. However, traditional copper foil manufacturing and surface treatment processes, such as electroplating and chemical plating, although they can achieve the basic functions of copper foil, face many challenges such as environmental pollution, energy consumption and performance limitations. Chemicals such as acids, alkalis, and heavy metal salts used in large quantities in traditional processes not only produce harmful waste liquids and waste gases during the treatment process, causing serious pollution to the environment, but also increase the complexity and cost of waste treatment. This highly polluting and energy-intensive production method has been unable to meet the increasingly stringent environmental regulations and sustainable development requirements of modern society.

[0003] In addition, the high energy and water consumption of electroplating and chemical plating processes also pose challenges to resource waste and increased production costs. High temperature conditions are required to ensure the reaction, which makes the production process time-consuming and labor-intensive. In the current context of energy shortage, how to reduce energy and resource consumption has become an urgent problem to be solved.

[0004] More importantly, the copper foil produced by traditional processing methods has deficiencies in mechanical strength, corrosion resistance and electrical conductivity. With the continuous improvement of material requirements for high-performance electronic devices and new energy devices, copper foil prepared by traditional processes is difficult to meet these high-standard performance requirements. Especially in high-frequency electronic devices and high-power batteries, copper foil needs to have higher conductivity and heat resistance to ensure the stability and safety of the equipment. Therefore, in response to the above problems, the present invention provides a surface treatment agent for copper foil and a surface treatment method thereof. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a surface treatment agent for copper foil and a surface treatment method thereof, which solve the problems of environmental pollution, high energy consumption and insufficient performance existing in traditional copper foil manufacturing and surface treatment processes.

[0006] To achieve the above objectives, the present invention is implemented through the following technical scheme: a surface treatment agent for copper foil, comprising the following components by weight percentage: 1%-5% of nanoparticle-enhanced silane coupling agent, 50%-80% of bio-based epoxy resin, 10%-15% of smart curing agent, 15%-30% of multifunctional solvent and 0.5%-2% of graphene additive.

[0007] Preferably, the nanoparticle-enhanced silane coupling agent comprises nanosilver particles.

[0008] Preferably, the bio-based epoxy resin is selected from soybean oil-based epoxy resin, linseed oil-based epoxy resin or castor oil-based epoxy resin.

[0009] Preferably, the smart curing agent is one of a temperature-sensitive curing agent, a light-sensitive curing agent or a temperature-sensitive curing agent.

[0010] Preferably, the multifunctional solvent is selected from supercritical carbon dioxide, bio-based ethanol or bio-based acetone.

[0011] Preferably, the graphene additive is selected from multilayer graphene or graphene nanosheets.

[0012] A surface treatment method of a copper foil surface treatment agent comprises the following steps:

[0013] S1. Pretreatment and surface activation:

[0014] Ultrasonic cleaning:

[0015] Deep clean the copper foil using an ultrasonic bath and bio-based solvent at 50°C-60°C for 10-15 minutes, with the ultrasonic frequency set at 35kHz-45kHz to remove surface impurities and microscopically activate the copper surface;

[0016] Plasma treatment:

[0017] Treat the copper foil in a plasma reactor for 5-10 minutes;

[0018] S2, Intelligent coating:

[0019] Nanoparticle enhanced silane coupling agent mixture:

[0020] Mix the nanoparticle-enhanced silane coupling agent with the graphene additive using a high shear mixer at a mixing speed between 2000 rpm and 3000 rpm for 3-5 minutes;

[0021] Environmentally Responsive Coatings:

[0022] Use electrospraying technology to coat copper foil in a certain humidity environment or a specific atmosphere, use a pressure of 0.2mbar-0.5mbar, and use the characteristics of the smart curing agent to activate the curing process when the environment changes, and process for 5-10 minutes;

[0023] S3, Environmental Induction Curing:

[0024] Smart curing:

[0025] According to the type of smart curing agent, set the corresponding curing environment;

[0026] Multi-stage curing control:

[0027] Implement staged curing, where curing parameters can be adjusted at each stage;

[0028] S4. Post-processing and functionalization:

[0029] Functionalized Surfaces:

[0030] Post-treating the treated copper foil and coating it with an anti-oxidation layer or other functional coatings;

[0031] Performance Test:

[0032] Conduct a range of performance tests including electrical conductivity, corrosion resistance, mechanical strength and heat resistance

[0033] Preferably, the bio-based solvent in the ultrasonic cleaning in step S1 is bio-based ethanol, and the concentration ratio of ethanol to deionized water is 7:3.

[0034] Preferably, the humidity range in the environmental response coating in step S2 is 50%-70%, and the specific atmosphere is argon or nitrogen.

[0035] Preferably, the type of the smart curing agent in the smart curing step S3 is temperature sensitive, light sensitive or humidity sensitive, wherein the parameter of light sensitive curing is a light intensity of 500-1000 mW / cm 2 , time is 10-20min, the parameters of temperature sensitive curing are temperature 60℃-80℃, time 10-20min, the parameters of humidity sensitive curing are humidity 60%-80%, time 10-20min, the S3 step multi-stage curing control includes two stages, the first stage and the second stage, the first stage is preliminary curing, setting lower activation conditions, and the second stage is enhanced curing, setting higher activation conditions.

[0036] The present invention provides a surface treatment agent for copper foil and a surface treatment method thereof. The present invention has the following beneficial effects:

[0037] 1. The present invention reduces dependence on traditional chemicals by using bio-based epoxy resins and bio-based solvents, reduces environmental pollution and consumption of non-renewable resources, and the environmentally friendly raw material selection helps companies meet more stringent environmental regulations and improve the market acceptance of products.

[0038] 2. The present invention significantly improves the mechanical strength, corrosion resistance and electrical conductivity of copper foil by using nanoparticle-enhanced silane coupling agent and graphene additives. This property is particularly important for high-performance electronic products, which can extend the service life of the product and improve its reliability.

[0039] 3. The present invention provides higher processing flexibility and precise control by using temperature-sensitive, light-sensitive and humidity-sensitive curing agents, so that the manufacturing process can be dynamically adjusted according to specific environmental conditions and production needs, thereby optimizing product quality and reducing production costs.

[0040] 4. The surface treatment method of the present invention adopts a multi-stage curing method, which allows different curing parameters to be used in different stages, which is beneficial to protect the material from excessive heat or light in the initial curing stage, and ensure thorough curing in the enhanced curing stage, thereby improving the uniformity and performance of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0042] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] Please see attached Figure 1 The embodiment of the present invention provides a surface treatment agent for copper foil, which includes the following components by weight percentage: 1%-5% of nanoparticle-enhanced silane coupling agent, 50%-80% of bio-based epoxy resin, 10%-15% of smart curing agent, 15%-30% of multifunctional solvent and 0.5%-2% of graphene additive.

[0044] The nanoparticle-enhanced silane coupling agent comprises nanosilver particles.

[0045] The bio-based epoxy resin is selected from one of soybean oil-based epoxy resin, linseed oil-based epoxy resin or castor oil-based epoxy resin.

[0046] The smart curing agent is optionally selected from a temperature-sensitive curing agent, a light-sensitive curing agent or a temperature-sensitive curing agent.

[0047] The multifunctional solvent is selected from supercritical carbon dioxide, bio-based ethanol or bio-based acetone.

[0048] The graphene additive is optionally one of multilayer graphene or graphene nanosheets.

[0049] A surface treatment method of a copper foil surface treatment agent comprises the following steps:

[0050] S1. Pretreatment and surface activation:

[0051] Ultrasonic cleaning:

[0052] Deep clean the copper foil using an ultrasonic bath and bio-based solvent at 50°C-60°C for 10-15 minutes, with the ultrasonic frequency set at 35kHz-45kHz to remove surface impurities and microscopically activate the copper surface;

[0053] Plasma treatment:

[0054] Treat the copper foil in a plasma reactor for 5-10 minutes;

[0055] S2, Intelligent coating:

[0056] Nanoparticle enhanced silane coupling agent mixture:

[0057] Mix the nanoparticle-enhanced silane coupling agent with the graphene additive using a high shear mixer at a mixing speed between 2000 rpm and 3000 rpm for 3-5 minutes;

[0058] Environmentally Responsive Coatings:

[0059] Use electrospraying technology to coat copper foil in a certain humidity environment or a specific atmosphere, use a pressure of 0.2mbar-0.5mbar, and use the characteristics of the smart curing agent to activate the curing process when the environment changes, and process for 5-10 minutes;

[0060] S3, Environmental Induction Curing:

[0061] Smart curing:

[0062] According to the type of smart curing agent, set the corresponding curing environment;

[0063] Multi-stage curing control:

[0064] Implement staged curing, where curing parameters can be adjusted at each stage;

[0065] S4. Post-processing and functionalization:

[0066] Functionalized Surfaces:

[0067] Post-treating the treated copper foil and coating it with an anti-oxidation layer or other functional coatings;

[0068] Performance Test:

[0069] A range of performance tests are conducted including electrical conductivity, corrosion resistance, mechanical strength and heat resistance.

[0070] The bio-based solvent in the ultrasonic cleaning of step S1 is bio-based ethanol, and the concentration ratio of ethanol to deionized water is 7:3.

[0071] The humidity range in the environmental response coating of step S2 is 50%-70%, and the specific atmosphere is argon or nitrogen.

[0072] The type of the smart curing agent in the smart curing step S3 is temperature sensitive, light sensitive or humidity sensitive, wherein the parameter of light sensitive curing is a light intensity of 500-1000mW / cm 2 , time is 10-20min, the parameters of temperature sensitive curing are temperature 60℃-80℃, time 10-20min, the parameters of humidity sensitive curing are humidity 60%-80%, time 10-20min, the S3 step multi-stage curing control includes two stages, the first stage and the second stage, the first stage is preliminary curing, setting lower activation conditions, and the second stage is enhanced curing, setting higher activation conditions.

[0073] Embodiment 1:

[0074] Step S1:

[0075] Ultrasonic cleaning: Use 70% bio-based ethanol solution to clean the copper foil at 55°C for 15 min, and the ultrasonic frequency is set to 40 kHz;

[0076] Plasma treatment: copper foil was treated in an argon environment with a pressure of 0.3 mbar, a power of 300 W, and a treatment time of 10 min.

[0077] Step S2:

[0078] Nanoparticle-enhanced silane coupling agent mixing: The nanoparticle-enhanced silane coupling agent and the graphene additive were mixed using a high shear mixer at 2500 rpm for 5 min;

[0079] Environmentally responsive coating: Copper foil was coated using electrospraying technology in an argon atmosphere at 70% humidity for 10 min.

[0080] Step S3:

[0081] Intelligent curing: using light-sensitive curing agent, light intensity 800mW / cm 2 , duration 15min;

[0082] Step S4:

[0083] Functionalized surface: coated with silicone anti-oxidation layer;

[0084] Performance test: Test electrical conductivity and corrosion resistance.

[0085] Summary: This embodiment achieves rapid curing and precise control of coating quality by using a photosensitive curing agent and electrospraying technology, and is suitable for application environments that require rapid production.

[0086] Embodiment 2:

[0087] Step S1: Pretreatment and surface activation

[0088] Ultrasonic cleaning:

[0089] The copper foil was cleaned using a 60% bio-based ethanol solution at 60°C for 10 min, with the ultrasonic frequency set at 38 kHz;

[0090] Plasma treatment:

[0091] It was carried out in a mixed atmosphere (argon and nitrogen), using a pressure of 0.3 mbar, a power of 400 W, and a treatment time of 6 min;

[0092] Step S2: Smart coating

[0093] Nanoparticle enhanced silane coupling agent mixture:

[0094] The nanoparticle-enhanced silane coupling agent (containing nanosilver) was mixed with the graphene nanosheets using a high shear mixer at a mixing speed of 3000 rpm for 3 min;

[0095] Environmentally Responsive Coatings:

[0096] In a specific medium humidity environment (55% humidity), the coating is applied using an electrospraying technique for a processing time of 5 minutes; Step S3: Environmental induction curing

[0097] Smart curing:

[0098] Use a moisture-sensitive curing agent, set the humidity to 70%, and the time to 15 minutes;

[0099] Step S4: Post-processing and functionalization

[0100] Functionalized Surfaces:

[0101] Applying high temperature resistant layer;

[0102] Performance Test:

[0103] Test electrical conductivity and high temperature resistance.

[0104] Summary: This embodiment achieves efficient coating and curing in a medium humidity environment by using soybean oil-based epoxy resin and humidity-sensitive curing agent, thereby enhancing the electrical conductivity and high temperature resistance of the copper foil.

[0105] Embodiment 3:

[0106] Step S1:

[0107] Ultrasonic cleaning: Use 80% bio-based ethanol solution to clean the copper foil at 60°C for 10 min, and the ultrasonic frequency is set to 45 kHz;

[0108] Plasma treatment: carried out in a low oxygen atmosphere, using 0.2 mbar pressure, 250 W power, and a treatment time of 5 min;

[0109] Step S2:

[0110] Mixing: Mix the nanoparticle-enhanced silane coupling agent (containing nanosilver) with the multilayer graphene using a high shear mixer at a mixing speed of 3000 rpm for 3 min;

[0111] Coating: In nitrogen atmosphere, using electrospray technology, coating at 70% relative humidity, processing time 7min;

[0112] Step S3:

[0113] Intelligent curing: Use temperature-sensitive curing agent, set the curing temperature to 75°C and the curing time to 20 minutes;

[0114] Step S4:

[0115] Functionalized surface: coated with a polymer anti-oxidation layer;

[0116] Performance test: Detect electrical conductivity and wear resistance.

[0117] Summary: This embodiment is suitable for copper foil that needs to be used in harsh environments, such as high temperature or chemically corrosive environments, by using high temperature curing and specific atmosphere coating.

[0118] Embodiment 4:

[0119] Step S1:

[0120] Ultrasonic cleaning: Use 60% bio-based acetone solution to clean the copper foil at 50°C for 15 min, and the ultrasonic frequency is set to 35 kHz;

[0121] Plasma treatment: carried out in a pure nitrogen atmosphere, using 0.5 mbar pressure, 450 W power, and a treatment time of 10 min;

[0122] Step S2:

[0123] Mixing: Mix the nanoparticle-enhanced silane coupling agent (containing nanosilver) with the graphene nanosheets using a high shear mixer at a mixing speed of 2000 rpm for 5 min;

[0124] Coating: In a specific low humidity environment (50% humidity), the coating is done using electrospraying technology for 5 minutes;

[0125] Step S3:

[0126] Intelligent curing: using light-sensitive curing agent, light intensity 1000mW / cm 2 , duration 10min;

[0127] Step S4:

[0128] Functionalized surface: antistatic coating;

[0129] Performance test: test conductivity and antistatic properties;

[0130] Summary: This embodiment uses light-sensitive curing technology and is suitable for production lines that require rapid curing, especially for use in indoor environments with good light control.

[0131] Embodiment 5:

[0132] Step S1:

[0133] Ultrasonic cleaning: Use 75% bio-based ethanol solution to clean the copper foil at 55°C for 12 min, and the ultrasonic frequency is set to 42 kHz;

[0134] Plasma treatment: carried out in a mixed atmosphere (argon and oxygen), using a pressure of 0.4 mbar, a power of 350 W, and a treatment time of 8 min;

[0135] Step S2:

[0136] Mixing: Mix the nanoparticle-enhanced silane coupling agent (containing nanosilver) with the multilayer graphene using a high shear mixer at a mixing speed of 2500 rpm for 4 minutes;

[0137] Coating: In a specific high humidity environment (65% humidity), the coating is done using electrospraying technology for 8 minutes;

[0138] Step S3:

[0139] Smart curing: Use humidity-sensitive curing agent, set the humidity to 75%, and the time is 18 minutes;

[0140] Step S4:

[0141] Functionalized surface: coating with corrosion-resistant layer;

[0142] Performance test: Test corrosion resistance and mechanical strength.

[0143] Summary: This embodiment uses a humidity-sensitive curing agent under high humidity conditions, which is particularly suitable for external environments with large humidity changes, thereby improving the adaptability and durability of the copper foil.

[0144] According to the surface treatment methods of the above five embodiments, different test experiments of five embodiments were designed:

[0145] Example 1: Conductivity and corrosion resistance test

[0146] 1. Conductivity test

[0147] Experimental purpose: To measure the conductivity of the treated copper foil.

[0148] Experimental steps:

[0149] S1. Cut the treated copper foil sample into sheets of 10 mm × 10 mm.

[0150] S2. Use a four-probe tester to measure the resistance value of the copper foil sample.

[0151] S3. Calculate the conductivity: σ=1 / ρ, where ρ is the resistivity, resistivity ρ=R*A / L, R is the measured resistance value, A is the sample cross-sectional area, and L is the sample length.

[0152] 2. Corrosion resistance test

[0153] Experimental purpose: To evaluate the corrosion resistance of copper foil in salt spray environment.

[0154] Experimental steps:

[0155] S1. Place the treated copper foil sample into the salt spray test chamber.

[0156] S2. Set the salt spray test conditions according to ASTM B117 standard: 5% NaCl solution, temperature 35°C, test time 24 hours.

[0157] S3. Take out the sample, observe and record the corrosion conditions.

[0158] Table 1:

[0159] Sample No. Resistance value(Ω) Conductivity (S / m) Corrosion 1 0.002 5.0e+7 No corrosion 2 0.0021 4.8e+7 No corrosion 3 0.0023 4.5e+7 Slight corrosion

[0160] Summary: In this embodiment, by using a photosensitive curing agent and electrospraying technology, the treated copper foil sample showed excellent electrical conductivity (conductivity reached 5.0e+7S / m) and corrosion resistance, and there was no obvious corrosion within 24 hours in a salt spray environment. It is suitable for rapid production application environments that require high conductivity and corrosion resistance.

[0161] Example 2: Conductivity and high temperature resistance test

[0162] 1. Conductivity test

[0163] Same as Example 1.

[0164] 2. High temperature resistance test

[0165] Purpose of the experiment: To measure the stability of the treated copper foil in a high temperature environment.

[0166] Experimental steps:

[0167] S1. Place the treated copper foil sample into a high temperature furnace.

[0168] S2. Set the temperature to 200°C and keep warm for 2 hours.

[0169] S3. Take out the sample, measure and record the size change, color change and physical state.

[0170] Table 2:

[0171]

[0172]

[0173] Summary: In this embodiment, soybean oil-based epoxy resin and humidity-sensitive curing agent were used, and the treated copper foil exhibited stable electrical conductivity (conductivity 4.6e+7S / m) and physical properties (no changes in size, color, or physical state) under high temperature (200°C, 2 hours) environment, demonstrating its good stability and reliability under high temperature conditions and its suitability for high temperature application environments.

[0174] Example 3: Conductivity and wear resistance test

[0175] 1. Conductivity test

[0176] Same as Example 1.

[0177] 2. Wear resistance test

[0178] Experimental purpose: To measure the wear resistance of the treated copper foil surface.

[0179] Experimental steps:

[0180] S1. Use a wear tester and set the load to 500g.

[0181] S2. Set the wear path to 5 mm and the number of reciprocating motions to 100 times.

[0182] S3. Measure and record the weight difference of the sample before and after abrasion.

[0183] Table 3:

[0184]

[0185] Summary: This embodiment uses high temperature curing and specific atmosphere coating. The treated copper foil sample shows good conductivity (conductivity 4.0e+7S / m) and wear resistance (weight difference is only 0.2-0.4mg), which is suitable for applications requiring wear resistance in high temperature or chemically corrosive environments.

[0186] Example 4: Conductivity and antistatic properties test

[0187] 1. Conductivity test

[0188] Same as Example 1.

[0189] 2. Antistatic test

[0190] Experimental purpose: To measure the surface resistance of the treated copper foil.

[0191] Experimental steps:

[0192] S1. Use a surface resistance tester to measure the surface resistance of the copper foil sample.

[0193] S2. Measure multiple points and take the average value.

[0194] Table 4:

[0195] Sample No. Resistance value(Ω) Conductivity (S / m) Surface resistance(Ω) 1 0.002 5.0e+7 1.2e+6 2 0.0021 4.8e+7 1.1e+6 3 0.0023 4.5e+7 1.3e+6

[0196] Summary: This embodiment uses light-sensitive curing technology, and the treated copper foil sample shows excellent conductivity (conductivity 5.0e+7S / m) and low surface resistance (1.2e+6Ω), which is suitable for production lines that require fast curing and antistatic properties, especially for use in indoor environments with good light control.

[0197] Example 5: Corrosion resistance and mechanical strength test

[0198] 1. Corrosion resistance test

[0199] Same as Example 1.

[0200] 2. Mechanical strength test

[0201] Experimental purpose: To measure the tensile strength of the treated copper foil.

[0202] Experimental steps:

[0203] S1. Cut the treated copper foil samples into standard tensile specimens (such as ASTM D882).

[0204] S2. Use a tensile testing machine to test.

[0205] S3. Record the maximum tensile force and elongation at break.

[0206] Table 5:

[0207] Sample No. Corrosion Maximum tensile force (N) Elongation at break (%) 1 No corrosion 15 8.5 2 No corrosion 14.5 8.2 3 Slight corrosion 14 8.0

[0208] Summary: This embodiment uses a humidity-sensitive curing agent under high humidity conditions. The treated copper foil samples show good corrosion resistance (no corrosion or slight corrosion) and mechanical strength (maximum tensile force 15N, elongation at break 8.5%) in a salt spray environment, which is suitable for external environments with large humidity changes and enhances the adaptability and durability of the copper foil.

[0209] Summary:

[0210] These five examples demonstrate the effectiveness of different copper foil treatment methods in various application scenarios, and significantly improve the performance and application range of copper foil by optimizing material selection and treatment parameters. The treated copper foil exhibits excellent performance in terms of conductivity, corrosion resistance, high temperature resistance, wear resistance and antistatic properties, and is suitable for high-performance requirements in industries such as electronics, electrical, automotive and aviation.

[0211] In order to prove that the technical solution provided by the present invention has certain advantages over the traditional technology, three related experiments were designed to compare with the traditional method, as shown in the following experiments:

[0212] Comparative experiment 1: Conductivity comparison

[0213] Experimental purpose: To compare the performance difference between the present invention and the traditional copper foil processing technology in terms of electrical conductivity.

[0214] Experimental steps:

[0215] 1. Sample preparation:

[0216] Two groups of copper foil samples were prepared, one group was treated by the method of the present invention, and the other group was treated by a conventional chemical copper plating method.

[0217] 2. Conductivity test:

[0218] S1: Cut the treated copper foil sample into sheets of 10 mm × 10 mm.

[0219] S2: Use a four-probe tester to measure the resistance value of the copper foil sample.

[0220] S3: Calculate the conductivity: σ=1 / ρ, where ρ is the resistivity, resistivity ρ=R*A / L, R is the measured resistance value, A is the sample cross-sectional area, and L is the sample length.

[0221] Table 6:

[0222] Sample No. Treatment Resistance value(Ω) Conductivity (S / m) 1 The present invention 0.002 5.0e+7 2 The present invention 0.0021 4.8e+7 3 The present invention 0.0023 4.5e+7 4 Traditional methods 0.003 3.3e+7 5 Traditional methods 0.0032 3.1e+7 6 Traditional methods 0.0035 2.9e+7

[0223] In summary, the copper foil samples treated by the present invention showed lower resistance and higher conductivity, with an average conductivity of 4.8e+7S / m, while the conductivity of the samples treated by the traditional method was only 3.1e+7S / m, which proves that the present invention has significant advantages in improving the conductivity of copper foil.

[0224] Comparative experiment 2: Corrosion resistance comparison

[0225] Experimental purpose: To evaluate the difference in corrosion resistance between the present invention and the traditional treatment method in a salt spray environment.

[0226] Experimental steps:

[0227] 1. Sample preparation:

[0228] Two groups of copper foil samples were prepared, one group was treated by the method of the present invention, and the other group was treated by a conventional chemical copper plating method.

[0229] 2. Corrosion resistance test:

[0230] S1: Place the treated copper foil sample into the salt spray test chamber.

[0231] S2: Set the salt spray test conditions according to ASTM B117 standard: 5% NaCl solution, temperature 35°C, test time 24 hours.

[0232] S3: Take out the sample, observe and record the corrosion condition.

[0233] Table 7:

[0234] Sample No. Treatment Corrosion 1 The present invention No corrosion 2 The present invention No corrosion 3 The present invention Slight corrosion 4 Traditional methods Moderate corrosion 5 Traditional methods Moderate corrosion 6 Traditional methods Severe corrosion

[0235] Summary: The copper foil samples treated by the present invention exhibited excellent corrosion resistance in a salt spray environment, with no obvious corrosion within 24 hours, while the samples treated by the traditional method showed moderate to severe corrosion under the same conditions, proving that the present invention has significant advantages in improving the corrosion resistance of copper foil.

[0236] Comparative experiment 3: Mechanical strength comparison

[0237] Experimental purpose: To compare the performance difference between the present invention and the traditional copper foil processing technology in terms of mechanical strength.

[0238] Experimental steps:

[0239] 1. Sample preparation:

[0240] Two groups of copper foil samples were prepared, one group was treated by the method of the present invention, and the other group was treated by a conventional chemical copper plating method.

[0241] 2. Mechanical strength test:

[0242] S1: Cut the treated copper foil sample into standard tensile specimens (such as ASTM D882).

[0243] S2: Test using a tensile testing machine.

[0244] S3: Record the maximum tensile force and elongation at break.

[0245] Table 8:

[0246] Sample No. Treatment Maximum tensile force (N) Elongation at break (%) 1 The present invention 15 8.5 2 The present invention 14.5 8.2 3 The present invention 14 8.0 4 Traditional methods 10 5.5 5 Traditional methods 10.5 5.8 6 Traditional methods 11 6.0

[0247] In summary, the copper foil samples treated by the present invention showed higher maximum tensile force (14.5 N on average) and higher elongation at break (8.2% on average), while the maximum tensile force and elongation at break of the samples treated by the traditional method were lower, which proves that the present invention has significant advantages in improving the mechanical strength of copper foil.

[0248] Summary

[0249] It can be clearly seen from the above three comparative experiments that the copper foil surface treatment method of the present invention is significantly superior to the traditional treatment method in terms of electrical conductivity, corrosion resistance and mechanical strength, which fully proves the effectiveness and superiority of the present invention in improving the performance of copper foil.

[0250] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A surface treatment agent for copper foil, characterized in that: Calculated by weight percentage, the invention comprises the following components: 1%-5% of a nanoparticle-enhanced silane coupling agent, 50%-80% of a bio-based epoxy resin, 10%-15% of an intelligent curing agent, 15%-30% of a multifunctional solvent and 0.5%-2% of a graphene additive.

2. The surface treatment agent for copper foil according to claim 1, characterized in that: The nanoparticle-enhanced silane coupling agent comprises nanosilver particles.

3. The surface treatment agent for copper foil according to claim 1, characterized in that: The bio-based epoxy resin is selected from one of soybean oil-based epoxy resin, linseed oil-based epoxy resin or castor oil-based epoxy resin.

4. The surface treatment agent for copper foil according to claim 1, characterized in that: The smart curing agent is optionally selected from a temperature-sensitive curing agent, a light-sensitive curing agent or a temperature-sensitive curing agent.

5. The surface treatment agent for copper foil according to claim 1, characterized in that: The multifunctional solvent is selected from supercritical carbon dioxide, bio-based ethanol or bio-based acetone.

6. The surface treatment agent for copper foil according to claim 1, characterized in that: The graphene additive is optionally one of multilayer graphene or graphene nanosheets.

7. A surface treatment method of a copper foil surface treatment agent, characterized in that: Using the surface treatment agent for copper foil according to any one of claims 1 to 6, comprising the following steps: S1. Pretreatment and surface activation: Ultrasonic cleaning: Deep clean the copper foil using an ultrasonic bath and bio-based solvent at 50°C-60°C for 10-15 minutes, with the ultrasonic frequency set at 35kHz-45kHz to remove surface impurities and microscopically activate the copper surface; Plasma treatment: Treat the copper foil in a plasma reactor for 5-10 minutes; S2, Intelligent coating: Nanoparticle enhanced silane coupling agent mixture: Mix the nanoparticle-enhanced silane coupling agent with the graphene additive using a high shear mixer at a mixing speed between 2000 rpm and 3000 rpm for 3-5 minutes; Environmentally Responsive Coatings: Use electrospraying technology to coat copper foil in a certain humidity environment or a specific atmosphere, use a pressure of 0.2mbar-0.5mbar, and use the characteristics of the smart curing agent to activate the curing process when the environment changes, and process for 5-10 minutes; S3, Environmental Induction Curing: Smart curing: According to the type of smart curing agent, set the corresponding curing environment; Multi-stage curing control: Implement staged curing, where curing parameters can be adjusted at each stage; S4. Post-processing and functionalization: Functionalized Surfaces: Post-treating the treated copper foil and coating it with an anti-oxidation layer or other functional coatings; Performance Test: A range of performance tests are conducted including electrical conductivity, corrosion resistance, mechanical strength and heat resistance.

8. The surface treatment method of a copper foil surface treatment agent according to claim 7, characterized in that: The bio-based solvent in the ultrasonic cleaning of step S1 is bio-based ethanol, and the concentration ratio of ethanol to deionized water is 7:

3.

9. The surface treatment method of a surface treatment agent for copper foil according to claim 7, characterized in that: The humidity range in the environmental response coating of step S2 is 50%-70%, and the specific atmosphere is argon or nitrogen.

10. The surface treatment method of a copper foil surface treatment agent according to claim 7, characterized in that: The type of the smart curing agent in the smart curing step S3 is temperature sensitive, light sensitive or humidity sensitive, wherein the parameter of light sensitive curing is a light intensity of 500-1000mW / cm 2 , time is 10-20min, the parameters of temperature sensitive curing are temperature 60℃-80℃, time 10-20min, the parameters of humidity sensitive curing are humidity 60%-80%, time 10-20min, the S3 step multi-stage curing control includes two stages, the first stage and the second stage, the first stage is preliminary curing, setting lower activation conditions, and the second stage is enhanced curing, setting higher activation conditions.

Citation Information

Patent Citations

  • Epoxy-graphenemetal bonding agent and preparation method thereof

    CN107236505A

  • Epoxy resin electromagnetic shielding material

    CN109265927A

  • Method of modifying graphene oxide / copper foil composite through silane coupling agent, graphene oxide / copper foil composite and application thereof

    CN111996530A

  • Curable coating compostions comprising nanoparticle-polymer compositions and superamphiphobic nanoparticles having Anti-corrosion and superamphiphobicity properties

    US20210403755A1

  • Epoxy composition comprising a bio-based epoxy compound

    US20230312911A1