Conductive adhesive as well as preparation method and application thereof

By using conductive adhesives in lead-acid batteries, the modified carbon materials with thiol and carboxyl groups on the surface are used to modify the surface to form chemical bonds with lead elements, the problems of large internal resistance and poor acid and alkali resistance in traditional lead-acid batteries are solved, and the problem of significant improvement is improved. Cycle life and performance of the battery.

CN118895093AActive Publication Date: 2024-11-05DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310505208.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05
Estimated Expiration
2043-05-05

AI Technical Summary

Technical Problem

The energy density and power density of traditional lead-acid batteries are low and have short cycle life, which cannot meet the technical requirements of new energy vehicles. The commonly used adhesives have large internal resistance and poor acid and alkali resistance, which leads to the bipolar plate being easily turtled after drying. Cracked and shed.

Method used

The surface of the conductive adhesive is modified with a modified carbon material loaded with a large amount of thiol and carboxyl groups, which can form chemical bonds with lead elements, enhance bond strength, and remain stable after drying, reducing internal resistance and contact resistance.

Benefits of technology

It effectively avoids cracking and shedding problems of bipolar plates, improves the cycle life of the battery, and can run at room temperature for more than 6 times that of traditional lead-acid batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a conductive adhesive as well as a preparation method and application thereof. The conductive adhesive comprises an organic polymer, a modified carbon material, high hydrogen evolution overpotential metal and N-methyl pyrrolidone; the surface of the modified carbon material is modified with sulfydryl, carboxyl and methyl. The surface of the carbon material in the conductive adhesive is modified and loaded with a large amount of sulfydryl and carboxyl and a small amount of methyl, the sulfydryl and carboxyl can be effectively complexed with lead element, and the methyl serves as an electron withdrawing group and is used for regulating and controlling the complexing strength to a moderate condition. The binder having a strong complexing effect with the lead element can be chemically bonded with effective performance between the bipolar plate and the lead paste, the binding strength is improved, cracks and falling conditions are avoided after the surface of the lead bipolar plate is coated with the binder and dried, the carbon layer has certain stretching and volume change capacity, the contact area between the carbon layer and the lead paste can be increased, and the lead paste can be effectively protected. And the contact resistance between the lead plaster and the bipolar plate is effectively reduced, and various properties of the bipolar battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a conductive adhesive and a preparation method and application thereof, belonging to the field of bipolar lead-carbon batteries. Background Art

[0002] With the advancement of science and technology, the problems of energy consumption and environmental pollution have gradually surfaced. In order to solve these problems, secondary battery energy storage technology (such as lead-acid batteries, lithium-ion batteries, metal-air batteries, fuel cells, etc.) has begun to develop rapidly. Among these energy storage systems, although lead-acid batteries have a history of more than 100 years, they still occupy a high market share (>70%). The reason why lead-acid batteries occupy such a large market share in the field of energy storage technology is mainly because of their low production and recycling costs, mature technology, and high safety and reliability. However, compared with other energy storage technologies, traditional lead-acid batteries still cannot meet the technical requirements of new energy vehicles due to their low energy density, low power density and short cycle life. For this reason, several new types of lead-acid batteries have emerged, providing a new direction for the development of lead-acid batteries.

[0003] Lead-carbon battery is a new type of lead-acid battery. It has both the capacitance characteristics of carbon materials and the battery characteristics of lead-acid batteries. This type of battery has the characteristics of resistance to large current shocks and long cycle life. Bipolar lead-carbon battery is a new type of lead-carbon battery, consisting of a series of stacked bipolar plates and diaphragms between the plates. A bipolar plate is an electrode that is coated with positive and negative active materials on both the positive and negative sides of the same substrate. Current can flow vertically through the active material. This structure can reduce the internal resistance of the battery, resulting in a significant improvement in the current transmission efficiency and charge and discharge performance of the battery. Commonly used binders in the process of coating active materials on the front and back of bipolar plates include polymer binders (such as ethylene vinyl alcohol resin and vinyl alcohol resin) and ceramic-based binders (such as calcium aluminate, etc.). Although these binders can effectively fix the positive and negative active materials of the bipolar plate together and ensure stable operation of the battery, their disadvantages are large internal resistance, poor acid and alkali resistance, poor expansion and contraction resistance, and the inability to form effective chemical bonds with the lead element in the lead paste or lead plate due to the physical or chemical properties of the binder itself. As a result, the bipolar plates coated with conventional binders are prone to cracking and falling off after drying, making it impossible for the active materials in the cured and dried lead paste to stably bond to its surface. Summary of the invention

[0004] The present invention proposes a conductive adhesive for effectively bonding a lead bipolar plate to a cured lead paste, wherein the conductive carbon material surface in the adhesive is modified to load a large amount of thiol and carboxyl groups and a small amount of methyl groups, wherein the thiol and carboxyl groups can effectively complex with the lead element, and the methyl group is used as an electron-withdrawing group to adjust the complex strength to a moderate condition. This adhesive with a strong complexing effect with the lead element can form an effective chemical bond between the bipolar plate and the lead paste, increase the bonding strength, and after being coated on the surface of the lead bipolar plate and dried, no cracks or falling off occur. The carbon layer has a certain ability to expand and contract and change volume, which can increase its contact area with the lead paste, effectively reduce the contact resistance between the lead paste and the bipolar plate, and improve the various performances of the bipolar battery.

[0005] According to one aspect of the present application, there is provided a conductive adhesive, comprising an organic polymer, a modified carbon material, a metal with a high hydrogen evolution overpotential, and N-methylpyrrolidone;

[0006] The surface of the modified carbon material is modified with mercapto groups, carboxyl groups and methyl groups.

[0007] Optionally, the conductive adhesive comprises, by mass:

[0008] 1 to 50 parts of organic polymer;

[0009] 50-100 parts of modified carbon material;

[0010] 0.05 to 10 parts of metal with high hydrogen evolution overpotential;

[0011] 500 to 2000 parts of N-methylpyrrolidone.

[0012] Optionally, the organic polymer is selected from at least one of polyvinylidene fluoride and polytetrafluoroethylene.

[0013] Optionally, the high hydrogen evolution overpotential metal is a simple substance or a compound;

[0014] The metal element of the high hydrogen evolution overpotential metal is selected from at least one of lead, bismuth, zinc, gallium, indium, mercury, titanium and tin.

[0015] Optionally, the preparation method of the modified carbon material is:

[0016] Placing the compound containing thiol and carboxyl groups in a reducing atmosphere for reduction to obtain the modified carbon material;

[0017] The reducing atmosphere includes a methyl-containing compound and a reducing gas.

[0018] Optionally, the compound containing mercapto and carboxyl groups is selected from at least one of mercaptosuccinic acid, dimercaptosuccinic acid, mercaptopolyethylene glycol carboxyl, and 1-1'-mercaptocarboxyldiimidazole.

[0019] Optionally, the molecular weight of the methyl-containing compound is 16-500.

[0020] Optionally, the methyl-containing compound is selected from at least one of methane, ethane and butane.

[0021] Optionally, the reducing gas is selected from at least one of hydrogen and ammonia.

[0022] Optionally, the mass ratio of the thiol and carboxyl compounds to the volume of the reducing atmosphere is 1 g: 0.001 to 200 mL.

[0023] Optionally, the molar ratio of the methyl compound to the reducing gas in the reducing atmosphere is 0.01 to 100:1.

[0024] Optionally, the molar ratio of the methyl compound to the reducing gas in the reducing atmosphere is any value of 0.01:1, 0.1:1, 1:1, 10:1, 50:1, 100:1, or a range between two values.

[0025] Optionally, the reduction conditions are: temperature 200-1500° C., time 1-24 h.

[0026] Optionally, the specific surface area of ​​the modified carbon material is 50 to 3000 m 2 / g.

[0027] According to another aspect of the present application, a method for preparing a conductive adhesive is provided, comprising the following steps:

[0028] The organic polymer, the modified carbon material, the metal with high hydrogen evolution overpotential and N-methylpyrrolidone are ground for 0.5 to 48 hours to obtain the conductive adhesive.

[0029] According to another aspect of the present application, there is provided a use of the above-mentioned conductive adhesive or the conductive adhesive obtained according to the above-mentioned preparation method in a bipolar lead-carbon battery.

[0030] The beneficial effects of this application include:

[0031] 1) The conductive adhesive provided in the present application is modified by loading a large amount of thiol and carboxyl groups and a small amount of methyl groups on the surface of the carbon material, wherein the thiol and carboxyl groups can effectively complex with the lead element, and the methyl group is used as an electron-withdrawing group to adjust the complex strength to a moderate condition. This adhesive with a strong complexing effect with the lead element can form an effective chemical bond between the bipolar plate and the lead paste, and increasing the bonding strength can effectively bond the lead paste to the bipolar plate substrate, avoid problems such as cracking of the conductive glue and shedding of the lead paste, effectively reduce the internal resistance between the active substance and the bipolar plate, and improve battery performance.

[0032] 2) The preparation method of the conductive adhesive provided in this application is simple to prepare. DETAILED DESCRIPTION

[0033] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0034] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0035] Example 1

[0036] Step 1: Prepare the bipolar plate conductive adhesive by the following method:

[0037] 1. The modified carbon material with thiol, carboxyl and methyl groups on the surface was prepared by the following method: 500 g of mercaptosuccinic acid was kept at 900 °C for 5 h in a hydrogen-methane mixture with a molar ratio of 1:1. The specific surface area of ​​the prepared modified carbon material was 1300 m 2 / g.

[0038] 2. Preparation of conductive adhesive:

[0039] 10 g of PVDF, 70 g of the modified carbon material prepared in step 1, 5 g of metal elemental lead with high hydrogen evolution overpotential, and 1000 g of NMP were fully mixed and ground for 12 hours.

[0040] Step 2: Preparation of bipolar lead-carbon battery

[0041] The flow lead-carbon battery was prepared by the following steps:

[0042] 1. Preparation of negative electrode:

[0043] (1) 600 g of lead powder, 9 g of carbon material, 8.4 g of barium sulfate, and 0.3 g of polypropylene short fibers with a length of 5 mm and a diameter of 0.5-1.5 μm were premixed in a high-speed mixer, and 84 g of deionized water was added to the premixed powder while stirring, and the stirring was continued for 10 min to obtain a lead paste;

[0044] (2) Scrape the high hydrogen evolution conductive adhesive prepared in step 1 on both sides of the bipolar plate, and scrape the lead paste on the surface of the bipolar plate grid coated with the conductive adhesive. The grid size is 70 mm long, 50 mm wide, and 2 mm thick;

[0045] 2. Preparation of the positive electrode: Prepare the positive electrode of the lead-acid battery according to the same process steps as the negative electrode preparation steps (1) and (2), except that no carbon material is added during the preparation of the positive electrode, and the positive electrode is scraped onto the other side of the bipolar plate coated with the conductive binder prepared in step 1;

[0046] 3. Preparation of end electrodes: Scrape the negative lead paste prepared in step (1) and the positive lead paste prepared in step (2) onto one side of the bipolar plate coated with the conductive adhesive prepared in step 1, and do not coat the other side with any active material. The bipolar plate coated with lead paste and the end plates on both sides are cured and dried together, with a curing temperature of 40°C, a humidity of 80%, and a curing time of 20 hours; the drying temperature is 80°C and the time is 24 hours;

[0047] 4. Preparation of lead-carbon battery: Place 5 bipolar plates and two end plates in a way that the positive and negative electrodes are opposite to each other, and place the lead-acid battery AGM diaphragm between the plates. Press each plate and diaphragm tightly and put them into the battery box in a tight assembly. The two ends of the battery box contain through-hole flow channels for the electrolyte. The battery box is 76mm long, 40mm wide, and 100mm high. Inject 80.3g of sulfuric acid electrolyte with a density of 1.275g / ml into the battery box;

[0048] The battery was subjected to a normal temperature life test under the following test conditions: at 25°C, the battery was discharged at a constant current of 4.2A for 59 seconds, discharged at 18A for 1 second, and charged at a constant current and voltage of 6.3A and 2.3V for 60 seconds. The battery was cycled 3600 times, then left to rest for 40 hours, and then the cycle was restarted after 40 hours. The termination condition of the life test was that the battery voltage dropped below 1.2V.

[0049] The initial voltage of the assembled lead-carbon battery at room temperature is 2.302V when fully charged, and the battery can run 45010 cycles in the room temperature life test. Compared with the test results of the bipolar lead-carbon battery without adding the bipolar plate conductive binder, that is, comparative example 1 under the same test conditions (7211 cycles), the room temperature cycle life of the prepared lead-carbon battery can reach 6.24 times the life of the traditional lead-acid battery.

[0050] Example 2

[0051] According to the conditions of Example 1, the amount of modified carbon material added in step 2 of step 1 was changed to 50 g. The assembled bipolar lead-carbon battery had a starting voltage of 2.289 V when fully charged, and could run 46,506 cycles of life test. Compared with the test results of a lead-carbon battery without a conductive binder under the same test conditions (7,211 cycles), the life of the bipolar lead-carbon battery can reach 6.45 times that of a traditional lead-acid battery.

[0052] Example 3

[0053] According to the conditions of Example 1, the amount of modified carbon material added in step 2 of step 1 was changed to 100 g. The assembled bipolar lead-carbon battery had a starting voltage of 2.262 V when fully charged, and could run 46,160 cycles of life test. Compared with the test results of a lead-carbon battery without a conductive binder under the same test conditions (7,211 cycles), the life of the bipolar lead-carbon battery can reach 6.40 times that of a traditional lead-acid battery.

[0054] Example 4

[0055] According to the conditions of Example 1, the amount of PVDF added in step 2 of step 1 was changed to 1g. The assembled bipolar lead-carbon battery had a starting voltage of 2.236V in a fully charged state, and could run a life test of 42084 cycles. Compared with the test results of a lead-carbon battery without a conductive binder under the same test conditions (7211 cycles), the life of the bipolar lead-carbon battery can reach 5.84 times that of a traditional lead-acid battery.

[0056] Example 5

[0057] According to the conditions of Example 1, the amount of PVDF added in step 2 of step 1 was changed to 50 g. The assembled bipolar lead-carbon battery had a starting voltage of 2.277 V when fully charged, and could run 41,436 cycles of life test. Compared with the test results of a lead-carbon battery without a conductive binder under the same test conditions (7,211 cycles), the life of the bipolar lead-carbon battery can reach 5.75 times that of a traditional lead-acid battery.

[0058] Example 6

[0059] According to the conditions of Example 1, the molar ratio of the hydrogen-methane mixture in step 1 of step 1 is changed to 10:1. The assembled bipolar lead-carbon battery has a starting voltage of 2.248V in a fully charged state, and can run 36024 cycles of life test. Compared with the test results of a lead-carbon battery without a conductive binder under the same test conditions (7211 cycles), the life of the bipolar lead-carbon battery can reach 5.00 times that of a traditional lead-acid battery.

[0060] Comparative Example 1

[0061] Bipolar lead-carbon battery without conductive binder: According to the requirements of Example 1, other conditions are not changed, and no conductive binder is added, and the bipolar lead-carbon battery is directly assembled. The assembled bipolar lead-carbon battery has a starting voltage of 2.109V in a fully charged state, and can run 7211 cycles of life test.

[0062] Comparative Example 2

[0063] According to the conditions of Example 1, the mercaptosuccinic acid in step 1 of step 1 was replaced with the same mass of mercaptoethanol. Since the precursor material does not contain a carboxyl group, its complexing ability with the bipolar plate substrate and lead paste is not strong. After the conductive adhesive is made, the lead paste cracks and falls off, resulting in the assembled bipolar lead-carbon battery having a starting voltage of 2.107V in a fully charged state, and can run 3621 cycles of life test.

[0064] Comparative Example 3

[0065] According to the conditions of Example 1, the mercaptosuccinic acid in step 1 of step 1 was replaced with the same mass of succinic acid. Since the precursor material does not contain a mercapto group, its complexing ability with the bipolar plate substrate and lead paste is not strong. After the conductive adhesive is made, the lead paste cracks and falls off, resulting in the assembled bipolar lead-carbon battery having a starting voltage of 2.005V in a fully charged state, and can run 4293 cycles of life test.

[0066] Comparative Example 4

[0067] According to the conditions of Example 1, the methane hydrogen mixture in step 1 of step 1 was replaced with a nitrogen hydrogen mixture of the same molar ratio. Since the prepared modified carbon material does not contain methyl, its complexing ability with the bipolar plate substrate and lead paste is poor, and the lead paste cracks and falls off after being made into a conductive adhesive. The assembled bipolar lead-carbon battery has a starting voltage of 2.246V in a fully charged state, and can run 6053 cycles of life test.

[0068] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A conductive adhesive, characterized in that: Including organic polymers, modified carbon materials, high hydrogen evolution overpotential metals and N-methylpyrrolidone; The surface of the modified carbon material is modified with mercapto groups, carboxyl groups and methyl groups.

2. The conductive adhesive according to claim 1, wherein: The conductive adhesive comprises, by mass: 1 to 50 parts of organic polymer; 50-100 parts of modified carbon material; 0.05 to 10 parts of metal with high hydrogen evolution overpotential; 500 to 2000 parts of N-methylpyrrolidone.

3. The conductive adhesive according to claim 1, wherein: The organic polymer is selected from at least one of polyvinylidene fluoride and polytetrafluoroethylene; Preferably, the metal with high hydrogen evolution overpotential is a single substance or a compound; The metal element of the high hydrogen evolution overpotential metal is selected from at least one of lead, bismuth, zinc, gallium, indium, mercury, titanium and tin.

4. The conductive adhesive according to claim 1, wherein: The preparation method of the modified carbon material is: Placing the compound containing thiol and carboxyl groups in a reducing atmosphere for reduction to obtain the modified carbon material; The reducing atmosphere includes a methyl-containing compound and a reducing gas.

5. The conductive adhesive according to claim 4, characterized in that: The compound containing mercapto and carboxyl groups is selected from at least one of mercaptosuccinic acid, dimercaptosuccinic acid, mercaptopolyethylene glycol carboxyl, and 1-1'-mercaptocarboxyldiimidazole.

6. The conductive adhesive according to claim 4, characterized in that: The molecular weight of the methyl-containing compound is 16 to 500; Preferably, the methyl-containing compound is selected from at least one of methane, ethane and butane; Preferably, the reducing gas is selected from at least one of hydrogen and ammonia.

7. The conductive adhesive according to claim 4, characterized in that: The mass ratio of the thiol and carboxyl compounds to the reducing atmosphere is 1 g: 0.001 to 200 mL; Preferably, the molar ratio of the methyl compound to the reducing gas in the reducing atmosphere is 0.01 to 100:1; Preferably, the reduction conditions are: temperature 200-1500° C., time 1-24 h.

8. The conductive adhesive according to claim 4, characterized in that: The specific surface area of ​​the modified carbon material is 50 to 3000 m 2 / g.

9. A method for preparing the conductive adhesive according to any one of claims 1 to 8, characterized in that: The following steps are involved: The organic polymer, the modified carbon material, the metal with high hydrogen evolution overpotential and N-methylpyrrolidone are ground for 0.5 to 48 hours to obtain the conductive adhesive.

10. Use of the conductive adhesive according to any one of claims 1 to 8 or the conductive adhesive obtained by the preparation method according to claim 9 in a bipolar lead-carbon battery.

Citation Information

Patent Citations

  • Process for producing carbon material

    CN101945821A

  • Carbon material-filled binding agent for lithium battery and preparation method of carbon material-filled binding agent

    CN104269558A

  • Preparation method for mesoporous active carbon fibers used for lead-carbon battery

    CN106025246A

  • Lead plaster, battery plate and preparation method and application thereof

    CN111224097A

  • Negative electrode lead paste of lead storage battery and preparation method of negative electrode lead paste

    CN114243000A