Copper sulfide composite aluminum-silicon aerogel material as well as preparation method and application thereof

By using copper sulfide composite aluminum-silicon aerogel materials in the aerospace field, uniformly distribute copper sulfide microspheres in aluminum-silicon aerogels, the problem of light weight caused by high density of copper sulfide materials is solved, and high temperature heat insulation is achieved The improvement of wave absorption performance meets the application needs of the aerospace field.

CN118895097APending Publication Date: 2024-11-05NEW MATERIAL INST OF SHANDONG ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410929567.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing copper sulfide materials are dense and cannot meet the needs of lightweight, high-temperature heat insulation, corrosion resistance and wave absorption performance in the fields of aerospace, especially on radar radomes and stealth fighters.

Method used

Copper sulfide composite aluminum-silicon aerogel material is used to uniformly distribute copper sulfide microspheres in aluminum-silicon aerogel to increase the composite amount and specific surface area, reduce density, enhance wave absorption performance and high-temperature heat insulation ability.

Benefits of technology

It has achieved copper sulfide composite materials with strong oxidation resistance, corrosion resistance and stability in the aerospace field, and has reduced density and improved wave absorption performance, meeting the needs of high-temperature heat insulation and wave absorption performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895097A_ABST
    Figure CN118895097A_ABST
Patent Text Reader

Abstract

The invention discloses a copper sulfide composite aluminum-silicon aerogel material and a preparation method and application thereof.The preparation method comprises the steps that a synchronous sol technology is adopted, an Al2O3 component is evenly dispersed in SiO2, and an aluminum-silicon sol precursor is formed; and then introducing the copper sulfide microspheres into an aluminum-silicon sol precursor to form a copper sulfide composite aluminum-silicon-aluminum-silicon material, and performing aging treatment and CO2 supercritical drying treatment to prepare the copper sulfide composite aluminum-silicon aerogel material. The copper sulphide composite aluminum-silicon aerogel material is composed of copper sulphide microspheres and aluminum-silicon aerogel, the copper sulphide microspheres are evenly distributed inside and on the surface of the aluminum-silicon aerogel, and the copper sulphide composite aluminum-silicon aerogel material has the unique advantages of being light, wide in absorption bandwidth, high in absorption capacity and the like, integrates the thinness and the lightness and can achieve the excellent wave absorption performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of inorganic functional materials, and specifically relates to a copper sulfide composite aluminum silicon aerogel material and a preparation method and application thereof. Background Art

[0002] With the rapid development of modern science and technology, aerospace, stealth fighter and radar antenna cover technology are becoming more and more mature, but the requirements for thermal insulation, higher temperature resistance, light weight and wave absorption performance of aircraft surfaces are also constantly increasing, in order to prevent the temperature increase caused by aerodynamic heating from damaging electronic components and ensure that electromagnetic waves can be effectively received.

[0003] With the in-depth research on new and efficient absorbing materials, people have been pursuing "wide, strong, light and thin" electromagnetic wave absorbers in recent years. Therefore, copper sulfide, which has special microstructure, wide action spectrum, high resistivity, corrosion resistance and other characteristics and can effectively absorb electromagnetic waves, especially in the microwave frequency band, is used in electromagnetic wave absorbers. At the same time, copper sulfide shows good stability in high temperature, oxidizing environment or harsh environment, and can maintain stable absorbing performance in a wide temperature range, so it is widely used in the field of high temperature technology. However, the density of copper sulfide is too large, and its use will greatly increase the weight of the product.

[0004] In the prior art, copper sulfide materials are prepared into thin layer structures or other metal ions are introduced as competitive reaction ions to participate in the reaction between copper ions and sulfide ions, in order to regulate the composition, interface and defects of the material through competitive reaction, so as to improve the material's wave absorption performance and reduce the product density. However, it still cannot be used in fields such as aerospace, especially in radar antenna covers and stealth fighters. Summary of the invention

[0005] The purpose of the present invention is to provide a copper sulfide composite aluminum-silicon aerogel material and a preparation method and application thereof. In the copper sulfide composite aluminum-silicon aerogel material provided by the present invention, the aluminum-silicon aerogel material can provide a larger specific surface area and interface, which helps to increase the composite amount of copper sulfide, and achieves strong wave absorbing performance while being resistant to high temperature and heat-insulating, thereby meeting the needs of aerospace and other fields, especially in radar antenna covers and stealth fighters.

[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0007] In the first aspect, an embodiment of the present invention provides a copper sulfide composite aluminum-silicon aerogel material, wherein the copper sulfide composite aluminum-silicon aerogel material is composed of copper sulfide microspheres and silicon-aluminum aerogel, wherein the copper sulfide microspheres are evenly distributed inside and on the surface of the aluminum-silicon aerogel, and the density of the copper sulfide composite aluminum-silicon aerogel material is 0.06 to 0.42 g / cm 3, with a specific surface area of ​​302.5 to 623.4 m 2 / g.

[0008] In some embodiments of the present invention, in the copper sulfide composite aluminum silicate aerogel material, the aluminum silicate aerogel is Al2O3-SiO2 aerogel; wherein the molar ratio of Al to Si is 1:(5-7.5).

[0009] In some embodiments of the present invention, in the copper sulfide composite aluminum silicate aerogel material, the molar ratio of copper sulfide microspheres to aluminum silicate aerogel is (0.008-0.010):1.

[0010] The copper sulfide microspheres in the synthesized copper sulfide composite aluminum silicate aerogel material of the present invention are evenly distributed inside and on the surface of the aluminum silicate aerogel, which can significantly improve the composite of the copper sulfide microspheres and the aluminum silicate aerogel. The copper sulfide composite aluminum silicate aerogel material has strong antioxidant and corrosion resistance, strong stability and wave absorbing performance.

[0011] In a second aspect, an embodiment of the present invention provides a method for preparing a copper sulfide composite aluminum-silicon aerogel material, comprising the following steps:

[0012] Step 1: Preparation of copper sulfide microspheres

[0013] The copper source and the sulfur source are dissolved in ethylene glycol respectively to form a copper source solution and a sulfur source solution; then, the sulfur source solution is added to the copper source solution, and the mixture is stirred evenly to form a mixed solution; the mixed solution is subjected to a hydrothermal reaction, and copper sulfide microspheres are obtained after centrifugation and drying.

[0014] Step 2: Preparation of aluminum silica sol precursor

[0015] The aluminum source and the silicon source are dissolved in a solvent consisting of anhydrous ethanol and deionized water, and then stirred evenly to obtain an aluminum silica sol precursor.

[0016] Step 3: Preparation of copper sulfide composite aluminum silica sol

[0017] The copper sulfide microspheres in step 1 are dispersed in the aluminum silica sol precursor in step 2, propylene oxide is added under ultrasonic stirring, and the copper sulfide composite aluminum silica sol is obtained after continuing stirring.

[0018] Step 4: Aging

[0019] The copper sulfide composite aluminum silica sol in step 3 is immersed in ethanol for aging and solvent replacement. The immersion time is 5 to 7 days, and the ethanol is replaced every 24 hours to obtain the copper sulfide composite aluminum silica sol after aging treatment.

[0020] Step 5: Drying

[0021] The copper sulfide composite aluminum silicate sol after aging treatment in step 4 is subjected to CO2 supercritical drying treatment to obtain a copper sulfide composite aluminum silicate aerogel material.

[0022] In some embodiments of the present invention, in step 1, the molar ratio of the copper source to the sulfur source is 1:(4-6); preferably, the copper source is copper sulfate or copper chloride dihydrate; or, the sulfur source is thioacetamide or thiourea;

[0023] Or, the stirring time is 0.5 to 1.5 h, and the stirring speed is 300 to 600 r / min;

[0024] Or, the temperature of the hydrothermal reaction is 150-170°C and the time is 5-6h;

[0025] Alternatively, the drying is vacuum drying at a drying temperature of 50-60°C.

[0026] In some embodiments of the present invention, in step 2, the volume ratio of the silicon source, anhydrous ethanol, and deionized water is 1: (30.7-62): (32.1-33); preferably, the silicon source is one or more of ethyl orthosilicate, methyl orthosilicate, sodium silicate, methyltriethoxysilane, or methyltrimethoxysilane;

[0027] Alternatively, the stirring time is 0.5 to 1.5 h, the stirring speed is 300 to 600 r / min, and the solution temperature is 25 to 40°C.

[0028] In some embodiments of the present invention, in step 3, the volume ratio of the silicon source to propylene oxide is 1:(14-16);

[0029] Or, the molar ratio of the aluminum source to the silicon source is 1:(5-7.5); the aluminum source is aluminum chloride hexahydrate or aluminum sol;

[0030] Or, the ultrasonic time is 0.5 to 1.5 h, the stirring time is 5 to 10 min, the stirring speed is 300 to 600 r / min, and the solution temperature is 25 to 40°C.

[0031] In some embodiments of the present invention, in step 5, the pressure of the drying kettle in the CO2 supercritical drying is 10.5-11.5 MPa, the temperature of the drying kettle is 45-55°C, and the drying time is 5-6 hours.

[0032] The copper sulfide composite aluminum-silicon aerogel material prepared by the present invention has stronger dielectric loss and stronger electromagnetic wave attenuation capability, and can meet the requirements of high temperature resistance and heat insulation while having good wave absorbing performance.

[0033] Therefore, the third aspect of the present invention provides the use of the above-mentioned copper sulfide composite aluminum silicate aerogel material in an absorbing material. Preferably, the copper sulfide composite aluminum silicate aerogel material is used in the aerospace field, in stealth fighters or radar antenna covers.

[0034] In a fourth aspect, an embodiment of the present invention provides an absorbing material, which takes paraffin as a matrix and fills the paraffin with a copper sulfide composite aluminum-silicon aerogel material.

[0035] The absorbent prepared by the present invention has the unique advantages of light weight, wide absorption bandwidth and strong absorption capacity, and is "thin and light" in one, and can achieve excellent absorbing performance.

[0036] The beneficial effects of the above embodiments of the present invention are as follows:

[0037] (1) The present application adopts a synchronous sol process to uniformly disperse the Al2O3 component in SiO2, thereby improving the high-temperature thermal stability of the alumina aerogel and increasing the specific surface area of ​​the sol formed by a single component, which is conducive to further compounding with copper sulfide.

[0038] (2) The present application uses ethylene glycol as a solvent, which is easier to recycle and reuse than deionized water, thereby reducing the impact on the environment; it increases the solubility of the copper source and sulfuric acid, thereby increasing the chemical reaction rate and reducing the occurrence of side reactions caused by hydrolysis of compounds during the reaction.

[0039] (3) The present invention introduces copper sulfide microspheres into an aluminum-silicon aerogel precursor to form a copper sulfide composite aluminum-silicon sol, and can evenly disperse high-density copper sulfide microspheres in the composite aluminum-silicon sol. Under the premise of ensuring the wave absorption performance, the density of the product is significantly reduced and the specific surface area of ​​the product is increased compared to a single copper sulfide microsphere; at the same time, the high-temperature thermal insulation performance is improved.

[0040] (4) The copper sulfide composite aluminum-silicon aerogel material prepared in the present application has strong anti-oxidation, corrosion resistance and strong stability, and is a light-weight, broadband, and highly absorbing absorbing material.

[0041] (5) The preparation method of the present application has the advantages of cheap and readily available reaction raw materials and no introduction of difficult-to-remove impurities, simple operation steps, high raw material utilization rate, simple production equipment, and low energy consumption, which is conducive to the industrial promotion of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0043] Figure 1This is a physical picture of the copper sulfide composite aluminum-silicon aerogel material prepared in Example 1 of the present invention;

[0044] Figure 2 This is a scanning electron microscope image of the copper sulfide composite aluminum-silicon aerogel material prepared in Example 2 of the present invention;

[0045] Figure 3 This is the N2 adsorption-desorption curve of the copper sulfide composite aluminum-silicon aerogel material prepared in Example 3 of the present invention.

[0046] The diagrams are for illustrative purposes only. DETAILED DESCRIPTION

[0047] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0048] Example 1

[0049] CuCl2·2H2O (6mmol) was dissolved in 30mL ethylene glycol (EG) to form a CuCl2 solution; CH4N2S (24mmol) was dissolved in 30mL ethylene glycol (EG) to form a CH4N2S solution. Then, the CH4N2S solution was added to the CuCl2 solution to form a mixed solution, and the mixture was stirred continuously for 0.5h until the mixed solution became transparent. The mixed solution was transferred to a 100mL hydrothermal kettle and kept at 150℃ in a muffle furnace for 5h; the product was collected by multiple centrifugation with distilled water and anhydrous ethanol, and the collected product was dried in a vacuum oven at 50℃ to obtain copper sulfide microspheres.

[0050] 22.17 g of aluminum chloride hexahydrate, 2.8 ml of ethyl orthosilicate, 86 ml of anhydrous ethanol and 90 ml of deionized water were mixed evenly, and after sealing, stirred at 300 r / min for 0.5 h to obtain an aluminum silica sol precursor.

[0051] Disperse 15mg of dried copper sulfide microspheres in the aluminum silica sol precursor, stir for 5min after ultrasonic treatment for 0.5h, add 42ml of 1,2-propylene oxide to the beaker, continue stirring at room temperature for 5min to obtain copper sulfide composite aluminum silica sol, and then soak it in anhydrous ethanol for 5 days to completely replace the water in the copper sulfide composite aluminum silica sol with ethanol. The replaced copper sulfide composite aluminum silica sol is placed in a CO2 supercritical drying device for drying, wherein the drying kettle pressure is controlled to 10.5MPa, the temperature is set to 45°C, and the drying time is 5h to obtain a copper sulfide composite aluminum silica aerogel material (labeled as 1-CuS-SiO2-Al2O3 aerogel).

[0052] 1-The density of CuS-SiO2-Al2O3 aerogel is 0.06g / cm 3 , with a specific surface area of ​​302.5m 2 / g.

[0053] Figure 1 This is the physical picture of 1-CuS-SiO2-Al2O3 aerogel. Figure 1 It can be seen that the 1-CuS-SiO2-Al2O3 composite aerogel is a blue translucent block.

[0054] Example 2

[0055] CuCl2·2H2O (6mmol) was dissolved in 30mL ethylene glycol (EG) to form a CuCl2 solution; CH4N2S (30mmol) was dispersed in another 30ml EG to form a CH4N2S solution. Then, the CH4N2S solution was added to the CuCl2 solution to form a mixed solution, and the mixture was stirred continuously for 0.5h until the mixed solution became transparent. The mixed solution was transferred to a hydrothermal kettle (100mL) and kept at 160°C in a muffle furnace for 5.5h; the product was collected by multiple centrifugation with distilled water and anhydrous ethanol, and the collected product was dried in a vacuum oven at 55°C to obtain copper sulfide microspheres.

[0056] 24.16 g of aluminum chloride hexahydrate, 2.8 ml of ethyl orthosilicate, 150 ml of anhydrous ethanol and 92 ml of deionized water were mixed evenly, sealed and stirred at 400 r / min for 1 h to obtain an aluminum silica sol precursor.

[0057] 15mg of dried copper sulfide microspheres were dispersed in the aluminum silica sol precursor, and stirred for 7min after ultrasonic treatment for 1h. 42ml of 1,2-propylene oxide was added to the beaker, and the composite sol was obtained after stirring at room temperature for 7min. The composite sol was then immersed in anhydrous ethanol for 6 days to completely replace the water in the sol with ethanol. The replaced composite sol was placed in a CO2 supercritical drying device for drying, wherein the drying kettle pressure was controlled at 11.5MPa, the temperature was set to 50℃, and the drying time was 5.5h to obtain a copper sulfide composite aluminum silicate aerogel material (labeled as 2-CuS-SiO2-Al2O3 aerogel).

[0058] The density of 2-CuS-SiO2-Al2O3 aerogel is 0.23g / cm 3 , with a specific surface area of ​​413.3m 2 / g.

[0059] Figure 2 This is a scanning electron microscope image of the 2-CuS-SiO2-Al2O3 aerogel material prepared in Example 2. It can be seen that the copper sulfide microspheres are evenly distributed in the pores and surface of the alumina-silica aerogel.

[0060] Example 3

[0061] CuCl2·2H2O (6mmol) was dissolved in 30mL ethylene glycol (EG) to form a CuCl2 solution; CH4N2S (36mmol) was dissolved in 30mL ethylene glycol (EG) to form a CH4N2S solution. Then, the CH4N2S solution was added to the CuCl2 solution to form a mixed solution, and the mixture was stirred continuously for 1.5h until the mixed solution became transparent. The mixed solution was transferred to a hydrothermal kettle (100mL) and kept at 170°C in a muffle furnace for 6h; the product was collected by multiple centrifugation with distilled water and anhydrous ethanol, and the collected product was dried in a vacuum oven at 60°C to obtain copper sulfide microspheres.

[0062] Mix 25.12 g of aluminum chloride hexahydrate, 2.8 ml of tetraethyl orthosilicate, 174 ml of anhydrous ethanol and 93 ml of deionized water evenly, seal and stir at 600 r / min for 1.5 h to obtain a SiO2-Al2O3 sol precursor.

[0063] 15mg of dried copper sulfide microspheres were dispersed in the SiO2-Al2O3 sol precursor, and stirred for 10min after ultrasonic treatment for 1.5h. 42ml of 1,2-propylene oxide was added to the beaker, and the composite sol was obtained after stirring at room temperature for 10min. The composite sol was then immersed in anhydrous ethanol for 7 days to completely replace the water in the sol with ethanol. The replaced composite sol was placed in a CO2 supercritical drying device for drying, wherein the drying kettle pressure was controlled at 11.5MPa, the temperature was set to 55℃, and the drying time was 6h to obtain a copper sulfide composite aluminum silicon aerogel material (labeled as 3CuS-SiO2-Al2O3 aerogel).

[0064] The density of 3-CuS-SiO2-Al2O3 aerogel is 0.42 g / cm 3 , with a specific surface area of ​​623.4m 2 / g.

[0065] Figure 3 This is the N2 adsorption-desorption curve of the 3-CuS-SiO2-Al2O3 aerogel material prepared in Example 3. The hysteresis loop shows that part of the composite material exhibits the characteristics of a mesoporous material.

[0066] Comparative Example 1

[0067] The difference from Example 1 is that the CuS-SiO2 aerogel material is prepared. The specific preparation process is as follows:

[0068] CuCl2·2H2O (6mmol) was dissolved in 30mL ethylene glycol (EG) to form a CuCl2 solution; CH4N2S (24mmol) was dissolved in 30mL ethylene glycol (EG) to form a CH4N2S solution. Then, the CH4N2S solution was added to the CuCl2 solution to form a mixed solution, and the mixture was stirred continuously for 0.5h until the mixed solution became transparent. The mixed solution was transferred to a hydrothermal kettle (100mL) and kept at 150°C in a muffle furnace for 5h; the product was collected by multiple centrifugation with distilled water and anhydrous ethanol, and the collected product was dried in a vacuum oven at 50°C to obtain copper sulfide microspheres.

[0069] Mix 45 ml of ethyl silicate, 186 ml of anhydrous ethanol, 14 ml of deionized water, and 0.6 ml of 1 mol hydrochloric acid evenly, seal, and stir at 300 r / min for 0.5 h to obtain a SiO2 sol precursor.

[0070] Disperse 15mg of dried copper sulfide microspheres in SiO2 sol precursor, stir for 5min after ultrasonic treatment for 0.5h, add 6ml of ammonia water into a beaker, continue stirring at room temperature for 5min to obtain a composite sol, and then soak it in anhydrous ethanol for 5 days to completely replace the water in the sol with ethanol. The replaced composite sol is placed in a CO2 supercritical drying device for drying, wherein the drying kettle pressure is controlled at 10.5MPa, the temperature is set to 45℃, and the drying time is 5h to obtain a copper sulfide composite aluminum aerogel material (labeled as CuS-SiO2 aerogel).

[0071] The density of CuS-SiO2 aerogel is 0.21g / cm 3 , the specific surface area is 342.5m2 / g.

[0072] Comparative Example 2

[0073] The difference from Example 1 is that the CuS-Al2O3 aerogel material is prepared. The specific preparation process is as follows:

[0074] CuCl2·2H2O (6mmol) was dissolved in 30mL ethylene glycol (EG) to form a CuCl2 solution; CH4N2S (24mmol) was dissolved in 30mL ethylene glycol (EG) to form a CH4N2S solution. Then, the CH4N2S solution was added to the CuCl2 solution to form a mixed solution, and the mixture was stirred continuously for 0.5h until the mixed solution became transparent. The mixed solution was transferred to a hydrothermal kettle (100mL) and kept at 150°C in a muffle furnace for 5h; the product was collected by multiple centrifugation with distilled water and anhydrous ethanol, and the collected product was dried in a vacuum oven at 50°C to obtain copper sulfide microspheres.

[0075] Mix 22.17 g of aluminum chloride hexahydrate, 86 ml of anhydrous ethanol and 90 ml of deionized water evenly, seal and stir at 300 r / min for 0.5 h to obtain an Al2O3 sol precursor.

[0076] 15mg of dried copper sulfide microspheres were dispersed in the Al2O3 sol precursor, ultrasonicated for 0.5h and stirred for 5min, and 42ml of 1,2-propylene oxide was added to the beaker, and stirred for 5min at room temperature to obtain a composite sol, which was then immersed in anhydrous ethanol for 5 days to completely replace the water in the sol with ethanol. The replaced composite sol was placed in a CO2 supercritical drying device for drying, where the drying kettle pressure was controlled at 10.5MPa, the temperature was set to 45°C, and the drying time was 5h to obtain a copper sulfide composite silicon aerogel material (labeled as CuS-Al2O3 composite aerogel).

[0077] The density of CuS-Al2O3 composite aerogel is 0.33 g / cm 3 , with a specific surface area of ​​250.6m 2 / g.

[0078] Thermal conductivity of aerogel samples (unit: W·m) at different temperatures for samples of Examples 1-3 of the present invention, samples of Comparative Examples 1-2 and alumina-silicon aerogel -1 ·K -1 ) as shown in the following table,

[0079] 25℃ 600℃ 1000℃ Example 1 0.0235 0.058 0.0994 Example 2 0.0251 0.0426 0.0901 Example 3 0.0279 0.0311 0.0812 Comparative Example 1 0.0209 0.0533 0.112 Comparative Example 2 0.0217 0.0541 0.136 Alumina-Silica Aerogel 0.0216 0.0596 0.0801

[0080] Microwave absorption performance measurement

[0081] With paraffin as the matrix, the copper sulfide composite aluminum-silicon aerogel material prepared in Example 3 was filled in the paraffin, with filling rates of 2wt% and 6wt% respectively, to form an annular ring with an inner diameter of 3.44mm and an outer diameter of 6.00mm. The complex magnetic permeability and complex dielectric constant were measured using a coaxial vector network analyzer (model Agilent PNA-N5244A), where the calculation formula of the complex dielectric constant is as follows:

[0082] ε r =ε'-jε"

[0083] In the formula, ε r represents the complex dielectric constant, ε' represents the real part of the dielectric constant, ε" represents the imaginary part of the dielectric constant, and j is the imaginary unit.

[0084] The test results show that when the filling rate is 2wt%, the minimum reflection loss of the absorber at 2.0mm is -42.2dB, the effective absorption bandwidth is 4.5GHz, and the widest EAB is 8.44GHz at 2.8mm.

[0085] When the filling rate is 6wt%, the absorption bandwidth of the absorber at 2.5mm is 6.16GHz; and the minimum reflection loss at 2.0mm is -51.2dB.

[0086] Taking paraffin as the matrix, the aerogel materials prepared in Comparative Examples 1 and 2 were filled in the paraffin respectively. Other test conditions were the same as those of the absorber prepared in Example 3, which will not be repeated here.

[0087] The results show that in comparative example 1, when the filling rate is 2wt%, the minimum reflection loss of the absorber at 2.0mm is -21.3dB, and the effective absorption bandwidth is 2.3GHz. When the filling rate is 6wt%, the absorption bandwidth of the absorber at 2.5mm is 4.21GHz;

[0088] In comparative example 2, when the filling rate is 2wt%, the minimum reflection loss of the absorber at 2.0mm is -24.2dB, and the effective absorption bandwidth is 3.1GHz. When the filling rate is 6wt%, the absorption bandwidth of the absorber at 2.5mm is 4.66GHz.

[0089] It can be seen that copper sulfide composite aluminum silicate aerogel material has unique advantages such as light weight, wide absorption bandwidth and strong absorption capacity. It combines "thin and light" in one and can achieve excellent wave absorbing performance.

[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A copper sulfide composite aluminum-silicon aerogel material, characterized in that: The copper sulfide composite aluminum-silicon aerogel material is composed of copper sulfide microspheres and aluminum-silicon aerogel. The copper sulfide microspheres are evenly distributed inside and on the surface of the aluminum-silicon aerogel. The density of the copper sulfide composite aluminum-silicon aerogel material is 0.06-0.42 g / cm 3 , with a specific surface area of ​​302.5 to 623.4 m 2 / g.

2. The copper sulfide composite aluminum-silicon aerogel material according to claim 1, characterized in that: In the copper sulfide composite aluminum silicate aerogel material, the aluminum silicate aerogel is Al2O3-SiO2 aerogel; wherein the molar ratio of Al to Si is 1:(5-7.5).

3. The copper sulfide composite aluminum-silicon aerogel material according to claim 1, characterized in that: In the copper sulfide composite aluminum silicate aerogel material, the molar ratio of copper sulfide microspheres to aluminum silicate aerogel is (0.008-0.010):

1.

4. A method for preparing the copper sulfide composite aluminum-silicon aerogel material according to claim 1, characterized in that: The steps include: Step 1: Preparation of copper sulfide microspheres Dissolving a copper source and a sulfur source in ethylene glycol respectively to form a copper source solution and a sulfur source solution; then, adding the sulfur source solution to the copper source solution, stirring evenly to form a mixed solution; The mixed solution is then subjected to a hydrothermal reaction, and copper sulfide microspheres are obtained after centrifugation and drying; Step 2: Preparation of aluminum silica sol precursor Dissolving an aluminum source and a silicon source in a solvent consisting of anhydrous ethanol and deionized water, and stirring evenly to obtain an aluminum silica sol precursor; Step 3: Preparation of copper sulfide composite aluminum silica sol Dispersing the copper sulfide microspheres in step 1 in the aluminum silica sol precursor in step 2, adding propylene oxide under ultrasonic stirring, and continuing stirring to obtain a copper sulfide composite aluminum silica sol; Step 4: Aging The copper sulfide composite aluminum silica sol in step 3 is immersed in ethanol for aging and solvent replacement. The immersion time is 5 to 7 days, and the ethanol is replaced every 24 hours to obtain the copper sulfide composite aluminum silica sol after aging treatment; Step 5: Drying The copper sulfide composite aluminum silicate sol after aging treatment in step 4 is subjected to CO2 supercritical drying treatment to obtain a copper sulfide composite aluminum silicate aerogel material.

5. A method for preparing the copper sulfide composite aluminum-silicon aerogel material according to claim 4, characterized in that: In step 1, the molar ratio of the copper source to the sulfur source is 1:(4-6); preferably, the copper source is copper sulfate or copper chloride dihydrate; or, the sulfur source is thioacetamide or thiourea; Or, the stirring time is 0.5 to 1.5 h, and the stirring speed is 300 to 600 r / min; Or, the temperature of the hydrothermal reaction is 150-170°C and the time is 5-6h; Alternatively, the drying is vacuum drying at a drying temperature of 50-60°C.

6. A method for preparing the copper sulfide composite aluminum-silicon aerogel material according to claim 4, characterized in that: Step 2, the volume ratio of silicon source, anhydrous ethanol and deionized water is 1: (30.7-62): (32.1-33); preferably, the silicon source is one or more of ethyl orthosilicate, methyl orthosilicate, sodium silicate, methyltriethoxysilane or methyltrimethoxysilane; Alternatively, the stirring time is 0.5 to 1.5 h, the stirring speed is 300 to 600 r / min, and the solution temperature is 25 to 40°C.

7. A method for preparing the copper sulfide composite aluminum-silicon aerogel material according to claim 4, characterized in that: In step 3, the volume ratio of silicon source to propylene oxide is 1:(14-16); Or, the molar ratio of the aluminum source to the silicon source is 1:(5-7.5); Or, the ultrasonic time is 0.5 to 1.5 h, the stirring time is 5 to 10 min, the stirring speed is 300 to 600 r / min, and the solution temperature is 25 to 40°C.

8. A method for preparing the copper sulfide composite aluminum-silicon aerogel material according to claim 4, characterized in that: In step 5, the pressure of the drying kettle in the CO2 supercritical drying is 10.5-11.5 MPa, the drying temperature is 45-55°C, and the drying time is 5-6 hours.

9. Application of copper sulfide composite aluminum silicon aerogel material in wave absorbing materials.

10. A wave absorbing material, characterized in that: Paraffin is used as a matrix, and the copper sulfide composite aluminum-silicon aerogel material according to claim 1 is filled in the paraffin.