Method for producing ultra-pure industrial pure iron

Through the pretreatment of molten iron and reblowing converter smelting technology, combined with ladle furnace refining and vacuum treatment, the problem of high gas and impurities content in the production of high-purity industrial pure iron in the existing technology is solved, and the continuous production with low cost and high efficiency is achieved. Meets the composition requirements of high purity iron.

CN118895402APending Publication Date: 2024-11-05BENGANG STEEL PLATES CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411047968.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art is difficult to produce high-purity industrial pure iron with extremely low gas content, low phosphorus and sulfur, ultra-low carbon and low silicon, and the process is complex and the cost is high, so it cannot meet the needs of high-purity iron.

Method used

The "three-de-treat" pretreatment technology is adopted to use the "three-dereat" pretreatment, including desulfurization, dephosphorization, and desiliconization. Combined with the smelting of the reblowing converter, ladle furnace refining and vacuum treatment, the decarbonization, degassing and desulfurization tasks are distributed to different processes, and the coupling reaction is used. Theories are used to desulfurize and dephosphorize the agent materials such as magnesium powder and lime powder, control the composition and temperature of molten iron, and achieve low-cost and high-efficiency continuous production.

Benefits of technology

It realizes the production of industrial pure iron with extremely low gas content and low impurity elements, improves production efficiency and molten steel quality, reduces costs, meets the composition requirements of high-purity iron, and is suitable for the manufacturing of high-precision products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974035080000081
    Figure BDA0004974035080000081
Patent Text Reader

Abstract

The invention relates to a production method of ultra-pure industrial pure iron. The production method comprises the following steps: pretreatment of molten iron: carrying out'three-removal 'pretreatment on the molten iron; a total iron method and a double-slag method are adopted for smelting, and converter tapping C is controlled to be larger than or equal to 0.10%. Ladle furnace refining (LF) is carried out, wherein slagging is carried out twice; carrying out calcium treatment before leaving the station, and keeping the soft blowing time for 10-15 minutes; and the temperature of molten steel is controlled to be 1650-1690 DEG C. Vacuum treatment (RH); and continuous casting: the superheat degree of a tundish is controlled to be 15-25 DEG C, the secondary cooling straightening temperature is controlled to be 940-960 DEG C, and it is guaranteed that Mn / S is larger than or equal to 12. According to the method, the tasks of decarburization, degassing, desulfurization, dephosphorization and demanganization in steelmaking are allocated to different processes and different time to be completed by utilizing existing conventional smelting equipment, the control targets of the purity, the surface quality, the internal quality and residual elements of the high-quality industrial pure iron can be stably, efficiently and synergistically achieved, and low-cost and high-efficiency continuous production is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of iron and steel metallurgy, and in particular to a new type of ultra-pure industrial pure iron for the metallurgical industry. In particular, it relates to a method for producing ultra-pure industrial pure iron with extremely low gas content, low phosphorus and sulfur, ultra-low carbon and low silicon. Industrial pure iron is an important raw material for smelting high-grade precision alloys, high-temperature alloys, ultra-low carbon stainless steel, electric heating alloys and the like. Background Art

[0002] Industrial pure iron is a type of steel, which contains 99.50% to 99.90% iron, with a carbon content of less than 0.04%. The lower the content of other impurities, the better. Generally speaking, industrial pure iron has the characteristics of good conductivity, soft texture, high toughness, and excellent electromagnetic properties. It is an important raw material for smelting precision alloys, high-temperature alloys, ultra-low carbon stainless steel, amorphous alloys, and electric heating alloys. From the perspective of electromagnetic properties, the higher the purity of industrial pure iron, the better the electromagnetic properties, but the process of producing high-purity iron is very complicated and the cost is high.

[0003] At present, industrial pure iron can be divided into electric arc furnace, oxygen converter and other methods of production based on production equipment. The difference between the two is:

[0004] 1) The minimum carbon content of pure iron in electric arc furnace is 0.025%, and the nitrogen content is relatively high. Due to the influence of carbon addition of graphite electrode, pure iron with lower carbon content cannot be produced.

[0005] 2) Oxygen converter pure iron can produce low-carbon pure iron with a carbon content of less than 0.01%, but its oxygen content is high and its nitrogen content is low, so it can only produce industrial pure iron of good quality.

[0006] With the rapid development of science and technology, people are becoming more and more demanding on materials. Developing high-purity iron preparation technology can improve the purity of iron and its product performance, increase product technology content and added value. Industrial pure iron is roughly divided into three categories and four grades: high aluminum, low aluminum and amorphous special. Among them, low aluminum industrial pure iron needs to adopt oxygen-containing casting technology when it is produced. With the continuous popularization of green concepts, the increasing attention paid to the ecological environment around the world, and the introduction of new national macroeconomic control policies, enterprises are facing increasing pressure to save energy and reduce emissions.

[0007] Chinese patent CN117265210A discloses a "method for preparing industrial pure iron", which contains C≤0.01%, Si≤0.01%, Mn≤0.05%, P≤0.01%, S≤0.010%, Al0.03-0.05%, total oxygen≤0.005%, and the rest is Fe. This invention has the disadvantages of long process and high oxygen content in continuous casting billet, which easily causes defects in casting billet.

[0008] Chinese patent CN101353753A discloses "an ultra-low carbon high-purity industrial pure iron and its preparation method", including the following chemical elements in weight percentage: C≤0.008%, Si≤0.05%, Mn≤0.05%, P≤0.005%, S≤0.002%, Al≤0.055%. It is smelted in an electric arc furnace, decarbonized by AOD oxygen blowing, and finally cast into steel ingots. The production cycle is long, and it is produced by die casting. The mold is demolded after cooling for 10 hours. The production efficiency is low and continuous production cannot be formed.

[0009] Chinese patent CN113512619A discloses "a method for producing industrial pure iron", including that the weight percentage of impurities in the iron is not more than 0.15%, among which C≤0.005%, Si≤0.01%, Mn≤0.05%, P≤0.010%, S≤0.002%, Al≤0.010%, N≤0.0040%, and Mn / S≥10; the invention has a high content of impurity elements and gases and cannot be used to produce high-precision products. Summary of the invention

[0010] The purpose of the present invention is to provide a method for producing ultra-pure industrial pure iron with ultra-low carbon, low impurity content and extremely low gas content, and to achieve low-cost and high-efficiency continuous production using existing conventional smelting equipment.

[0011] In order to achieve the above object, the present invention adopts the following technical solutions:

[0012] A method for producing ultra-pure industrial pure iron, characterized by comprising the following method steps:

[0013] 1) Before pretreatment of molten iron, the contents of C≥2.1%, Si 0.25wt%-0.50wt%, Mn≤0.10wt%, P≤0.080wt%, S≤0.030wt% and the temperature of molten iron are controlled to be ≥1300°C; the total amount of impurity elements in the molten iron is not more than 0.10wt%, wherein Ti≤0.03wt%, Cr≤0.03wt%, Ni≤0.01wt%, Cu≤0.01wt%, and Pb, As, Sn, Sb and Bi are all ≤0.0003wt%.

[0014] Hot metal pretreatment: Hot metal undergoes "three de-" pretreatment, including desulfurization, dephosphorization, and desiliconization. Desiliconization, dephosphorization, and desulfurization are performed using coupled reaction theory. The first step is desiliconization, which is performed using a hot metal tank. The silicon in the hot metal is removed to 0.10wt% to 0.15wt% using a desiliconizer, and the slag is removed. The desiliconizer is a mixture of 82 to 88 parts of iron scale, 8 to 12 parts of lime, and 3 to 8 parts of fluorite. The second step is desulfurization. The amount of desulfurizer and stirring time are adjusted according to the sulfur content of the molten iron before treatment. Magnesium powder and lime powder are added in a mass ratio of 1: (3.0-4.0). The reaction of magnesium in molten iron is: Mg(s)→Mg(l)→Mg(g)→[Mg]. After melting, gasification and dissolution, the dissolved magnesium in the molten iron reacts with sulfur: Mg(s)+[S]=MgS(s), so that the sulfur in the molten iron is ≤0.003wt%. The third step is dephosphorization. The stirring of the molten pool is strengthened. FeO slag is used for dephosphorization. TFe in the slag is controlled to be ≤5%, R=2-2.5. After pretreatment, the phosphorus content of the molten iron is ≤0.003%.

[0015] The molten iron undergoes "three-removal" pretreatment to reduce the lime slag material required to remove silicon and phosphorus during the converter steelmaking blowing process, reduce the amount of slag, reduce slag overflow and splashing, etc., control the redox components during the "three-removal" reaction process, and use the slag overflow process during the blowing period to timely remove the slag produced in each reaction period and realize online slag modification. The erosion of the slag on the furnace lining is also reduced, and the furnace age is significantly improved. At the same time, the converter blowing time is shortened, the converter production efficiency is improved, the iron loss is reduced, and the quality of the molten steel is effectively improved.

[0016] 2) Converter smelting: adopt full iron method and double slag method for smelting, for the first slag making, iron ore, limestone and fluorite are added to make pre-slag in the early stage of the converter, slag pouring operation is carried out when the blowing time reaches 6-8 minutes and the molten pool temperature is 1380-1420°C, Si-containing slag is added for deoxidation, and then the second slag making is carried out, dolomite, iron ore and lime are added to make post-slag, and the blowing is continued to 1590-1620°C for steelmaking, and the basicity of the final slag is controlled to be 2.8-3.0 and the FeO content is 8wt%-12wt%; aluminum particles are added for deoxidation during the converter steelmaking process, and pre-melted slag and lime are added for slag washing; the slag layer thickness is controlled to be 25-35mm after the second slide plate slag blocking steelmaking; the converter steelmaking C is controlled to be ≥0.10%.

[0017] 3) Ladle furnace refining (LF): two slag making processes are adopted. In the first slag making process, pre-melted slag and lime are added to make white slag, and aluminum is added for deoxidation. The white slag time is kept for 10 to 15 minutes, and S in the steel is ≤ 0.0008wt%, O ≤ 0.0010wt%; then the slag removal operation is carried out to control the slag layer thickness to 25 to 35mm, and then pre-melted slag and lime are added to make slag again to control the slag basicity R = 1.2 to 1.5; calcium treatment is carried out before leaving the station, and the soft blowing time is kept for 10 to 15 minutes; the molten steel temperature is controlled to be 1650 to 1690°C.

[0018] 4) Vacuum treatment (RH): After the molten steel enters the station, it is evacuated to less than 140Pa and oxygen blowing and decarburization are started. When the vacuum degree is 50-60Pa, argon stirring is added and the oxygen is maintained for 15-20min. The target oxygen is controlled between 200-250ppm. Aluminum wire is added for deoxidation. The cycle time is 5-10min. The oxygen content after breaking the air is controlled between 20-40ppm and the carbon content is ≤0.001%. Aluminum particles are sprinkled in the molten steel before leaving the station, Mg treatment is performed to fully spheroidize the inclusions, and a carbon-free covering agent is added to ensure that the soft blowing + calming time reaches 20-25min.

[0019] 5) Continuous casting: Protective pouring is adopted throughout the whole process, and ultra-low carbon protective slag and carbon-free covering agent are used; the superheat of the tundish is controlled at 15-25°C, and the secondary cooling and straightening temperature is controlled at 940-960°C to ensure that Mn / S is ≥12.

[0020] The Si-containing slag material is one or more of acidic slag material, silica and silicon carbide.

[0021] The iron-water ratio is ≥95%; carbon-free tundish and carbon-free ladle are selected.

[0022] Industrial pure iron produced by the method for producing ultra-pure industrial pure iron, the chemical components of the industrial pure iron are as follows by weight percentage: C≤0.001%, Si≤0.005%, Mn≤0.02%, P≤0.0008%, S≤0.0008%, Al≤0.01%, in addition, O≤0.0010%, N≤0.0010% in the steel, alloy elements Nb≤0.0030%, Ti≤0.0030%, Cr≤0.01%, Ni≤0.01%, Cu≤0.01% in the steel, in addition, the residual elements Pb, As, Sn, Sb, Bi in the steel are all ≤0.0003%, and the rest is Fe.

[0023] Principle description: The molten iron of the present invention adopts a "three-removal" pretreatment process, strictly limits the composition of the molten iron entering the converter, adopts top and bottom double-blowing converter smelting during steelmaking, and adopts a two-time slag making process for the converter. Limestone and fluorite are added to the front slag, and the molten iron undergoes an oxidation reaction to produce FeO, which is beneficial to melting the slag and reducing the consumption of oxygen. Since CO and CO2 gases generated by the reaction of C and O play a stirring role on the slag, the kinetic conditions of the P removal reaction are increased, and the P removal efficiency and reaction interface are increased. At the same time, for the Mn removal reaction, the more SiO2 in the steel and the addition of Si-containing slag for deoxidation make the slag basicity low or even acidic in the early stage of blowing, which is beneficial to the Mn removal reaction; after the first slag pouring, iron ore, lime and dolomite are added for secondary slag making to increase the slag basicity, which is beneficial to the thermodynamics of the S removal reaction. To prevent P from returning and ensure sufficient FeO in the steel; during the refining process, a higher C content is controlled to ensure a slight positive pressure to prevent negative pressure from causing molten steel to absorb N, and to ensure a lower O content in the molten steel, which is conducive to reducing the burden of subsequent deoxidation and white slag making and reducing the generation of oxide inclusions. A higher C content is conducive to improving the desulfurization reaction during the LF refining process, and can also improve the denitrification capacity during the RH vacuum treatment process. LF ladle furnace refining adopts two slag making. The first white slag is desulfurized to an extremely low level before slag removal. Then the second slag making is reasonably controlled to CaO+MgO / Al2O3+SiO2 to ensure that the secondary slag has good fluidity and the ability to absorb subsequent deoxidation products. Then it is sent to the RH vacuum treatment station for a long time of deep treatment, first blowing oxygen for decarburization and then deoxidizing with Al wire, followed by Mg treatment. While obtaining ultra-low carbon, the oxygen content and inclusion morphology are strictly controlled. Aluminum particles are thrown into the steel before leaving the station, and a carbon-free covering agent is added to ensure a soft blowing + calming time of 20 to 25 minutes, effectively reducing the oxygen in the steel and allowing the inclusions to fully float and be removed. The continuous casting process adopts appropriate superheat and straightening temperature, while ensuring Mn / S ≥ 12, to obtain continuous casting billets with high surface quality and internal quality, avoiding the occurrence of center looseness, center segregation and corner transverse cracks.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention provides a process method for producing ultra-pure industrial pure iron through "three removals" pretreatment of molten iron. The combined blowing converter, ladle furnace refining, RH vacuum treatment and slab continuous casting are conventional equipment of existing steel enterprises. The requirements for raw and auxiliary materials are easy to meet. According to the principles of metallurgical dynamics and thermodynamics, the tasks of steelmaking decarbonization, degassing, desulfurization, dephosphorization and demanganese are allocated to different processes and at different times to be completed. The control targets of purity, surface quality, internal quality and residual elements of high-quality industrial pure iron can be achieved stably, efficiently and synergistically. Therefore, the present invention has good popularization and application value.

[0026] The present invention aims to solve the problem that the oxygen content of pure iron in oxygen converter is high and high-quality pure iron cannot be produced; solve the production problem of low-aluminum industrial pure iron; use existing conventional smelting equipment to achieve low-cost and high-efficiency continuous production; use vacuum decarburization technology to make industrial pure iron have extremely low carbon content; through the research of refining and demanganization technology, further reduce the manganese content in steel to meet the composition requirements of industrial pure iron; control deoxidation to obtain qualified continuous casting slabs. Pure iron requires the content of each element as low as possible, including the deoxidizing element aluminum. For the casting of pure iron, the control of the deoxidation degree is extremely important, that is, to ensure the composition requirements and meet the production process requirements to obtain qualified continuous casting slabs. DETAILED DESCRIPTION

[0027] The specific implementation modes of the present invention are further described below in conjunction with the embodiments.

[0028] The embodiments are produced according to the production process steps of combined blowing converter smelting, ladle furnace refining, RH vacuum treatment, and slab continuous casting of the present invention; a carbon-free ladle and a carbon-free tundish are used, and the selected raw and auxiliary materials and main components are shown in Table 1. The key process steps of each embodiment are as follows:

[0029] Embodiment 1:

[0030] 1. Molten iron composition: C 2.1%, Si 0.26%, Mn 0.06%, P 0.05%, S 0.022%, molten iron temperature 1320℃, impurity element content of molten iron: Ti 0.012%, Cr 0.015%, Ni 0.006%, Cu 0.006%, in addition, residual elements Pb 0.0001%, As 0.00012%, Sn 0.00011%, Sb 0.0001%, Bi 0.00012% are required.

[0031] 2. The molten iron is pretreated with "three desulfurizations", including dephosphorization and desiliconization, and the coupled reaction theory is used to carry out desiliconization, dephosphorization and desulfurization. The first step is to use a molten iron tank for desiliconization. The desiliconization agent is a mixture of 85 parts of iron sheet, 10 parts of lime and 5 parts of fluorite, so that the silicon content in the molten iron is 0.10%, and the slag is scraped off; the second step is to add magnesium powder and lime powder in a ratio of 1:3.5. The reaction of magnesium in the molten iron is: Mg(s)→Mg(l)→Mg(g)→[Mg]. After melting, gasification and dissolution, the dissolved magnesium in the molten iron reacts with sulfur: Mg(s)+[S]=MgS(s), so that the S content in the molten iron is 0.001%; ​​the third step is to strengthen the stirring of the molten pool, develop a low-FeO slag dephosphorization process, control TFe2% in the slag, R=2.1, and the P content of the molten iron after pretreatment is 0.0012%.

[0032] After pretreatment of the molten iron, the composition of the molten iron is: C 2.1%, Si 0.10%, Mn 0.05%, P 0.0012%, S0.001%, and is added to the converter for steelmaking.

[0033] 3. Converter smelting: All-iron method and double-slag method are adopted for smelting. For the first slag making, iron ore, limestone and fluorite are added to make pre-slag in the early stage of the converter. When the blowing time is 6 minutes and the molten pool temperature is 1385, the slag is poured, and acidic slag-adjusting materials are added for deoxidation. Then the second slag making is carried out, dolomite, iron ore and lime are added to make post-slag, and the blowing is continued to 1590℃ for steelmaking. The basicity of the final slag is controlled to be 2.8 and the FeO content is 8.2%; aluminum particles are added for deoxidation during the steelmaking process, and pre-melted slag and lime are added for slag washing; the thickness of the slag layer is controlled to be 25mm after the second slide plate slag blocking steelmaking, and the converter steelmaking C is finally controlled to be 0.11%.

[0034] 4. Ladle furnace refining (LF): slagging twice. Pre-melted slag and lime are added to make white slag during the refining process, and aluminum is added for deoxidation. The white slag time is kept for 10 minutes, and the S in the steel is 0.0005% and the O is 0.0006%; then the slag removal operation is carried out, and the slag layer thickness is controlled to 25mm. Then pre-melted slag and lime are added to make slag again, and R=1.2; calcium treatment is carried out before leaving the station, and the soft blowing time is kept for 10 minutes; the molten steel temperature is controlled at 1650℃;

[0035] 5. Vacuum treatment (RH): After the molten steel enters the station, it is evacuated to 139Pa and oxygen blowing and decarburization are started. When the vacuum degree is 50Pa, argon stirring is added and the oxygen is maintained for 15 minutes. The target oxygen is controlled at 210ppm. Aluminum wire is added for deoxidation. The cycle time is 5min. The oxygen content after breaking the air is controlled at 20ppm and the carbon content is 0.0003%. Aluminum particles are sprinkled in the molten steel before leaving the station, Mg treatment is carried out to fully spheroidize the inclusions, and carbon-free covering agent is added to ensure that the soft blowing + calming time reaches 20min.

[0036] 6. Continuous casting: Protective pouring is adopted throughout the whole process, using ultra-low carbon protective slag and carbon-free covering agent; the superheat of the tundish is controlled at 15℃, and the secondary cooling straightening temperature is controlled at 941℃.

[0037] In this embodiment, the molten iron ratio is 95%.

[0038] The composition of the finished product obtained is: C0.0003%, Si0.002%, Mn0.01%, P0.0004%, S0.0002%, Al0.004%. In addition, O 0.0005%, N 0.0004%, alloy elements Nb0.001%, Ti0.001%, Cr0.008%, Ni0.006%, Cu0.006% in the steel are controlled, Mn / S=50, and the residual elements in the steel are Pb0.00011%, As0.00012%, Sn0.0001%, Sb0.00012, Bi0.00013%, and the rest is Fe.

[0039] Embodiment 2:

[0040] 1. The molten iron contains 2.3% C, 0.38% Si, 0.09% Mn, 0.065% P, 0.026% S, and the molten iron temperature is 1330°C. The impurity elements in the molten iron are Ti0.028%, Cr0.023%, Ni0.008%, and Cu0.008%. In addition, the residual elements Pb0.0002%, As0.00022%, Sn0.00023%, Sb0.00019, and Bi0.00023% are required.

[0041] 2. The molten iron is pretreated by "three desulfurizations", including dephosphorization and desiliconization. The first step is to use a molten iron tank for desiliconization. The desiliconization agent is a mixture of 85 parts of iron sheets, 10 parts of lime and 5 parts of fluorite, so that the silicon content in the molten iron is 0.12%, and the slag is scraped off; the second step is to add magnesium powder and lime powder in a ratio of 1:3.5. The reaction of magnesium in molten iron is: Mg(s)→Mg(l)→Mg(g)→[Mg]. After melting, gasification and dissolution, the dissolved magnesium in the molten iron reacts with sulfur: Mg(s)+[S]=MgS(s), so that the S content in the molten iron is 0.002%; the third step is to strengthen the stirring of the molten pool, develop a low FeO slag dephosphorization process, control the TFe in the slag to 3.5%, R=2.3, and the P content of the molten iron after pretreatment is 0.0023%.

[0042] After the molten iron is pretreated, the molten iron composition is: C2.3%, Si0.12%, Mn0.08%, P0.0023%, S0.002%, and is added into the converter for steelmaking.

[0043] 3. Converter smelting: All-iron method and double-slag method are adopted for smelting. For the first slag making, iron ore, limestone and fluorite are added to make pre-slag in the early stage of the converter. When the blowing time is 6 minutes and the molten pool temperature is 1400°C, the slag is poured, silica is added for deoxidation and then the second slag making is carried out. Dolomite, iron ore and lime are added to make post-slag. The blowing is continued to 1610°C for steel tapping, and the basicity of the final slag is controlled to be 2.9 and the FeO content is 10.2%. Aluminum particles are added for deoxidation during the steel tapping process, and pre-melted slag and lime are added for slag washing. After the second slide plate slag blocking steel tapping, the slag layer thickness is controlled to be 31mm, and finally the converter steel tapping C is controlled to be 0.12%.

[0044] 4. Ladle furnace refining (LF): slagging twice. Pre-melted slag and lime are added to make white slag during the refining process, and aluminum is added for deoxidation. The white slag time is kept for 10 minutes, and S in the steel is ≤ 0.0008%, O ≤ 0.0010%; then the slag removal operation is carried out, and the slag layer thickness is controlled to 25mm, and then pre-melted slag and lime are added to make slag again, and R is controlled to be 1.2; calcium treatment is carried out before leaving the station, and the soft blowing time is kept for 12 minutes; the molten steel temperature is controlled to be 1650℃.

[0045] 5. Vacuum treatment (RH): After the molten steel enters the station, it is evacuated to 138Pa and oxygen blowing and decarburization are started. When the vacuum degree is 50Pa, argon stirring is added and the oxygen is maintained for 18 minutes. The oxygen is controlled at 230ppm. Aluminum wire is added for deoxidation. The cycle time is 8 minutes. The oxygen content after breaking the air is controlled at 32ppm and the carbon content is 0.0006%. Before leaving the station, aluminum particles are sprinkled in the molten steel, Mg treatment is carried out to fully spheroidize the inclusions, and a carbon-free covering agent is added to ensure that the soft blowing + calming time reaches 23 minutes.

[0046] 6. Continuous casting: Protective pouring is adopted throughout the whole process, using ultra-low carbon protective slag and carbon-free covering agent; the superheat of the tundish is controlled at 21°C, and the secondary cooling straightening temperature is controlled at 950°C.

[0047] The molten iron ratio in this embodiment is 96%.

[0048] The composition of the finished product obtained is: C0.0006%, Si0.0035%, Mn0.015%, P0.0006%, S0.0005%, Al0.006%. In addition, O0.0007%, N0.0006% in the steel, alloy elements Nb0.002%, Ti0.002%, Cr0.009%, Ni0.008%, Cu0.008% in the steel, Mn / S=30, in addition, the residual elements in the steel are Pb0.00019%, As0.00021%, Sn0.0002%, Sb0.00022, Bi0.00019%, and the rest is Fe.

[0049] Embodiment 3:

[0050] 1. Molten iron composition: C: 2.5%, Si 0.50%, Mn 0.10%, P 0.080%, S 0.030%, molten iron temperature 1350°C, impurity element content Ti 0.03%, Cr 0.029%, Ni 0.01%, Cu 0.01%, in addition, residual elements Pb 0.00029%, As 0.0003%, Sn 0.00028%, Sb 0.0003, Bi 0.0003%,

[0051] 2. The molten iron is desulfurized, dephosphorized and desiliconized. The first step is to use a molten iron tank for desiliconization. The desiliconizer is a mixture of 85 parts of iron sheets, 10 parts of lime and 5 parts of fluorite, so that the silicon content in the molten iron is 0.15%, and the slag is scraped off; the second step is to add magnesium powder and lime powder in a ratio of 1:3.5. After melting, gasification and dissolution, the dissolved magnesium in the molten iron reacts with sulfur: Mg(s)+[S]=MgS(s), so that the S content in the molten iron is 0.003%; the third step is to strengthen the stirring of the molten pool, develop a low-FeO slag dephosphorization process, control TFe5% in the slag, R=2.5, and the P content of the molten iron after pretreatment is 0.0029%.

[0052] After the molten iron is pretreated, the molten iron composition is: C2.5%, Si0.15%, Mn0.10%, P0.0029%, S0.003%, and is added into the converter for steelmaking.

[0053] 3. Converter smelting: All-iron method and double-slag method are adopted for smelting. For the first slag making, iron ore, limestone and fluorite are added to make pre-slag in the early stage of the converter. When the blowing time is 6 minutes and the molten pool temperature is 1420, the slag is poured, silicon carbide is added for deoxidation, and then the second slag making is carried out, dolomite, iron ore and lime are added to make post-slag, and the blowing is continued to 1620℃ for steelmaking, and the basicity of the final slag is controlled to 3.0 and the FeO content is controlled to 12%; aluminum particles are added for deoxidation during the steelmaking process, and pre-melted slag and lime are added for slag washing; the slag layer thickness is controlled to 35mm after the second slide plate slag blocking steelmaking, and the converter steelmaking C is finally controlled to 0.12%.

[0054] 4. Ladle furnace refining (LF): pre-melted slag and lime are added to make white slag during the refining process, and aluminum is added for deoxidation. The white slag time is maintained for 15 minutes, and the S in the steel is reduced to 0.0008% and the O to 0.0010%; then the slag removal operation is carried out, and the slag layer thickness is controlled to 35mm, and then pre-melted slag and lime are added to make slag again, and R is controlled to be 1.5; calcium treatment is carried out before leaving the station, and the soft blowing time is maintained for 15 minutes; the molten steel temperature is controlled to be 1690℃.

[0055] 5. Vacuum treatment (RH): After the molten steel enters the station, it is evacuated to 135Pa and oxygen blowing and decarburization are started. When the vacuum degree is 50Pa, argon stirring is added and the oxygen is maintained for 20 minutes. The oxygen is controlled at 250ppm. Aluminum wire is added for deoxidation. The cycle time is 10 minutes. The oxygen content after breaking the air is controlled at 40ppm and the carbon content is 0.001%. Before leaving the station, aluminum particles are sprinkled in the molten steel, Mg treatment is carried out to fully spheroidize the inclusions, and carbon-free covering agent is added to ensure that the soft blowing + calming time reaches 25 minutes.

[0056] 6. Continuous casting: Protective pouring is adopted throughout the whole process, using ultra-low carbon protective slag and carbon-free covering agent; the superheat of the tundish is controlled at 25℃, and the secondary cooling straightening temperature is controlled at 960℃.

[0057] In this embodiment, the molten iron ratio is 98%.

[0058] The composition of the finished product obtained is: C0.001%, Si0.005%, Mn0.019%, P0.0008%, S0.00076%, Al0.01%. In addition, O0.0009%, N0.0010% in the steel, alloy elements Nb0.003%, Ti0.0029%, Cr0.01%, Ni0.0099%, Cu0.01% in the steel, Mn / S=25, in addition, the residual elements in the steel are Pb0.00029%, As0.0003%, Sn0.00028%, Sb0.0003, Bi0.0003%, and the rest is Fe.

[0059] Table 1 Raw materials and main ingredients / %

[0060]

Claims

1. A method for producing ultra-pure industrial pure iron, characterized in that: The method comprises the following steps: 1) Hot metal pretreatment: The hot metal is pretreated by "three dephosphorizations". The first step is to use a hot metal tank for desiliconization, and use a desiliconizer to remove silicon from the hot metal to 0.10wt%~0.15wt%, and then scrape off the slag; the second step is desulfurization, and the amount of desulfurizer and stirring time are adjusted according to the sulfur content of the hot metal before treatment, and magnesium powder and lime powder are added to make the sulfur in the hot metal ≤0.003wt%; the third step is to strengthen the stirring of the molten pool, use FeO slag for dephosphorization, control TFe in the slag ≤5%, R=2~2.5, and the phosphorus content of the hot metal after pretreatment is ≤0.003%; 2) Converter smelting: double slag method is adopted for smelting. In the first slag making, iron ore, limestone and fluorite are added to the converter to make the pre-slag in the early stage. When the blowing is carried out for 6 to 8 minutes and the molten pool temperature is 1380 to 1420°C, the slag is poured, Si-containing slag is added for deoxidation, and then the second slag making is carried out, dolomite, iron ore and lime are added to make the post-slag, and the blowing is continued to 1590 to 1620°C for steel tapping, and the final slag basicity is controlled to be 2.8 to 3.0 and the FeO content is 8wt% to 12wt%; the converter tapping C is controlled to be ≥ 0.10%; 3) Ladle furnace refining: two slag making processes are adopted. In the first slag making process, pre-melted slag and lime are added to make white slag, and the white slag time is kept for 10-15 minutes to make S in the steel ≤ 0.0008wt%; then the slag removal operation is carried out, and then pre-melted slag and lime are added to make slag again, and the slag basicity R is controlled to be 1.2-1.5; 4) Vacuum treatment: After the molten steel enters the station, the vacuum is less than 140Pa and oxygen blowing and decarburization are started. When the vacuum degree is 50-60Pa, argon stirring is added and the oxygen is maintained for 15-20min. The target oxygen is controlled between 200-250ppm. Aluminum wire is added for deoxidation. The cycle time is 5-10min. The O content after breaking the air is controlled between 20-40ppm and the C content is ≤0.001%. Aluminum particles are sprinkled in the molten steel before leaving the station, Mg treatment is performed to fully spheroidize the inclusions, and a carbon-free covering agent is added to ensure that the soft blowing + calming time reaches 20-25min. 5) Continuous casting: The superheat of the tundish is controlled at 15-25°C, and the secondary cooling and straightening temperature is controlled at 940-960°C to ensure that Mn / S is ≥12.

2. A method for producing ultra-pure industrial pure iron according to claim 1, characterized in that: The desiliconizing agent is a mixture of 82-88 parts of iron scale, 8-12 parts of lime and 3-8 parts of fluorite.

3. A method for producing ultra-pure industrial pure iron according to claim 1, characterized in that: In the step 1), the mass ratio of magnesium powder to lime powder is 1:(3.0-4.0).

4. A method for producing ultra-pure industrial pure iron according to claim 1, characterized in that: In the step 2), aluminum particles are added for deoxidation during the converter tapping process, and pre-melted slag and lime are added for slag washing; and the thickness of the slag layer is controlled to be 25 to 35 mm after the second slide plate slag blocking tapping.

5. A method for producing ultra-pure industrial pure iron according to claim 1, characterized in that: In the step 3), aluminum is added for deoxidation during the first slag making, and O is controlled to be less than or equal to 0.0010 wt%.

6. A method for producing ultra-pure industrial pure iron according to claim 1, characterized in that: In the step 3), during the first slag making and slagging, the thickness of the slag layer is controlled to be 25 to 35 mm.

7. A method for producing ultra-pure industrial pure iron according to claim 1, characterized in that: In the step 3), calcium treatment is carried out before leaving the station, and the soft blowing time is maintained for 10 to 15 minutes; the molten steel temperature is controlled at 1650 to 1690°C.

8. A method for producing ultra-pure industrial pure iron according to claim 1, characterized in that: Before pretreatment of molten iron, C ≥ 2.1%, Si 0.25wt% ~ 0.50wt%, Mn ≤ 0.10wt%, P ≤ 0.080wt%, S ≤ 0.030wt% in the molten iron are controlled, and the molten iron temperature is controlled ≥ 1300°C; the total content of impurity elements in the molten iron is not more than 0.10wt%, among which Ti ≤ 0.03wt%, Cr ≤ 0.03wt%, Ni ≤ 0.01wt%, Cu ≤ 0.01wt%, and Pb, As, Sn, Sb, and Bi are all ≤ 0.0003wt%.

9. A method for producing ultra-pure industrial pure iron according to claim 1, characterized in that: The Si-containing slag material is one or more of acidic slag material, silica and silicon carbide.

10. Industrial pure iron produced by the method for producing ultra-pure industrial pure iron according to any one of claims 1 to 9, characterized in that: The chemical composition of the industrial pure iron is calculated by weight percentage as follows: C≤0.001%, Si≤0.005%, Mn≤0.02%, P≤0.0008%, S≤0.0008%, Al≤0.01%. In addition, O≤0.0010%, N≤0.0010% in the steel, alloy elements Nb≤0.0030%, Ti≤0.0030%, Cr≤0.01%, Ni≤0.01%, Cu≤0.01% in the steel, and residual elements Pb, As, Sn, Sb, and Bi in the steel are all ≤0.0003%, and the rest is Fe.

Citation Information

Cited By

  • Production method of industrial pure iron small square billet

    CN120738421A