Magnetic alloy with room-temperature large magnetostrictive strain, preparation method and application
By preparing Co2Cr1-xGa1+x magnetic alloy, arc melting and heat treatment technology, room temperature magnetostrictive strain of about 60ppm under low magnetic field is achieved, and the magnetostrictive strain and high cost of existing magnetostrictive alloys are solved. Problem, significantly reducing material costs and simplifying process flow.
Patent Information
- Application Number
- CN202410943729.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
The magnetostrictive strain of existing magnetostrictive alloys at room temperature is limited, and the raw materials are expensive and fragile, and require a large driving magnetic field, which limits its application range.
Co2Cr1-xGa1+x magnetic alloy is used to prepare polycrystalline ingots or strips by arc smelting and heat treatment methods, and large magnetostrictive strain at room temperature is achieved under low magnetic fields. Simple process flow and conventional equipment are used.
It has achieved room temperature magnetostrictive strain of about 60ppm at low magnetic fields, which reduces raw material costs, simplifies the process flow, and improves the stability and application potential of the material.
Smart Images

Figure CN118895560A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of material science, and in particular to a magnetic alloy with large magnetostrictive strain at room temperature, a preparation method and an application thereof. Background Art
[0002] Magnetostrictive materials (Reference 1: "Wang Hong. Research and Development of Magnetostrictive Materials and Their Displacement Sensors [D]. Chongqing University, 2007") undergo elastic deformation under the action of a magnetic field, achieving vibration output under an alternating magnetic field and nanometer-level high-precision micro-displacement output under a unidirectional magnetic field. They play an indispensable and important role in national defense and civilian high-tech fields such as high-power ultrasonic devices, naval submarine sonar, aerospace precision micro-displacement control systems, high-precision robots and various magnetic drive devices. They are a type of strategic new functional material.
[0003] According to the type of material, magnetostrictive alloy materials can be divided into Ni-based alloys, FeCo-based alloys, rare earth magnetostrictive alloys and FeGa-based alloy materials, etc.
[0004] Ni-based alloys (Reference 2: "Guangming. Nickel-based magnetostrictive alloys [J]. Metal Functional Materials, 1997, 05: 36-36") and FeCo-based alloys (Reference 3: "Yin Hongyun. Fe-Co-based Laves phase magnetostrictive materials [D]. Ningbo University") are magnetic materials with large magnetostrictive strain that were discovered earlier, but the magnetostrictive strain of their polycrystalline alloys at room temperature is only 30 to 50 ppm, which limits its application range.
[0005] have <112> and <110> TbDyFe with preferred axis orientation (Reference 4: "Zhang Shirong, Yang Hongchuan, Yu Dunbo, et al. Study on the preparation of rare earth magnetostrictive material TbDyFe by rapid crystallization-bonding method [J]. Journal of the Chinese Rare Earth Society, 2008, 26 (1): 5") rare earth giant magnetostrictive alloy material is currently widely used magnetostrictive material. The magnetostrictive strain of this rare earth magnetic alloy is as high as 1500ppm at room temperature. However, the raw materials of this rare earth magnetic alloy are expensive, the material is brittle, and the magnetic field required to drive the magnetostrictive strain is large, which limits the further application of this alloy material.
[0006] In 2000, Clark et al. from the U.S. Naval Laboratory discovered FeGa-based alloy magnetostrictive materials. <001> The oriented single crystal alloy has a large magnetostrictive strain (~200ppm) in low field and low raw material cost, which has attracted global attention. However, compared with oriented FeGa single crystal alloy materials, the room temperature magnetostrictive strain of its polycrystalline cast alloy is relatively small (~50ppm), and more complex processing methods such as directional rolling or directional solidification are required to obtain preferential orientation and improve its magnetostrictive strain, which also restricts the application of FeGa-based alloys in practical engineering fields.
[0007] In view of this, the present invention aims to provide a magnetic alloy with large magnetostrictive strain at room temperature and a preparation method thereof. Summary of the invention
[0008] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and provide a magnetic alloy with large magnetostrictive strain at room temperature, a preparation method and an application thereof.
[0009] The technical solution of the present invention is:
[0010] A method for preparing a magnetic alloy having large magnetostrictive strain at room temperature comprises the following steps:
[0011] S100, weighing Co, Cr, and Ga metal raw materials with a purity of 99.95% respectively according to the ratio of Co:Cr:Ga=2:1-x:1+x; wherein the range of x is: 0≤x<1;
[0012] S200, smelting method: put the weighed material into the crucible, and use a mechanical pump to pump the vacuum degree of the arc furnace chamber to 2×10 -3 Pa, then argon was introduced as protective gas, the melting current was 100A, each sample was turned over 3 times, and the melting was performed 5 times in total to ensure uniform composition;
[0013] S300, heat treatment method: the obtained button ingot material is sealed in a vacuum quartz tube, annealed at 850°C to 900°C for 72 to 120 hours for homogenization annealing, and then gradually cooled to room temperature at a cooling rate of 2°C / second to obtain a polycrystalline bulk ingot.
[0014] A method for preparing a magnetic alloy having large magnetostrictive strain at room temperature comprises the following steps:
[0015] S100, weighing Co, Cr, and Ga metal raw materials with a purity of 99.95% respectively according to the ratio of Co:Cr:Ga=2:1-x:1+x; wherein the range of x is: 0≤x<1;
[0016] S200, smelting method: put the weighed material into the crucible, and use a mechanical pump to pump the vacuum degree of the arc furnace chamber to 2×10 -3 Pa, then argon was introduced as protective gas, the melting current was 100A, each sample was turned over 3 times, and the melting was performed 5 times in total to ensure uniform composition;
[0017] S300, heat treatment method: the obtained button ingot material is sealed in a vacuum quartz tube, annealed at 850°C to 900°C for 72 to 120 hours for homogenization annealing, and then gradually cooled to room temperature at a cooling rate of 2°C / second to obtain a polycrystalline bulk ingot;
[0018] S400, put the button polycrystalline ingot into a quartz tube with a small hole at the bottom, place it in the furnace chamber of the belt spinning machine, and use a mechanical pump to evacuate the chamber to 10 -3 Pa, high-purity argon gas is introduced into the furnace chamber with a pressure of 0.05MPa. Induction heating is used to make the alloy in a molten state. Then the gas control valve is opened, and high-purity argon gas with a pressure of 0.05MPa is blown into the upper part of the quartz tube to make the molten alloy liquid spray from the small hole to the high-speed rotating copper wheel with a linear velocity of 25m / s and quickly thrown out to obtain a strip with a width of 3-4mm and a thickness of 30-50μm.
[0019] A magnetic alloy with large magnetostrictive strain at room temperature is prepared by the above-mentioned preparation method; it has the following chemical formula: Co2Cr 1-x Ga 1+x , wherein the range of x is: 0≤x<1; the magnetic alloy is a polycrystalline ingot.
[0020] A magnetic alloy with large magnetostrictive strain at room temperature is prepared by the above-mentioned preparation method; it has the following chemical formula: Co2Cr 1-x Ga 1+x , wherein the range of x is: 0≤x<1; the magnetic alloy is a polycrystalline strip.
[0021] Furthermore, Co2Cr 1-x Ga 1+x It is a cubic crystal system, the space group is Fm-3m, and the space group number is 225.
[0022] Furthermore, the magnetic alloy has a magnetostrictive strain of 18 to 60 ppm at room temperature of 300K and a critical magnetic field of 100 mT.
[0023] Co2Cr 1-x Ga 1+x As an application of a magnetic alloy with large magnetostrictive strain at room temperature, the range of x is: 0≤x<1; the magnetostrictive strain is between 18 and 60 ppm.
[0024] A magnetic alloy with large magnetostrictive strain at room temperature is used in magnetic drive devices.
[0025] A magnetic alloy with large magnetostrictive strain at room temperature is used in sonar systems, ultrasonic devices, precision positioning control or mechanical brakes.
[0026] The beneficial effects of this application are:
[0027] First, the basic inventive concept of the present invention is to discover for the first time that Co2Cr 1-x Ga 1+x Its Curie temperature is higher than room temperature. Compared with traditional rare earth magnetostrictive materials, this alloy has better low-field magnetostrictive performance and only requires a very low external driving magnetic field (100mT) to be used. Its room-temperature magnetostrictive strain can reach 60ppm.
[0028] Secondly, the second inventive point of the present application is that the present invention provides two preparation methods, both of which are simple and fast, have a high yield rate, and do not require complicated process flows and expensive large-scale equipment.
[0029] Fourth, the magnetic alloy provided by the present application has low-priced raw materials, abundant reserves and easy storage compared to traditional rare earth magnetostrictive materials, which significantly reduces the cost of materials. Since the alloy material has a large saturation magnetostriction coefficient at room temperature and low magnetic field, it is insensitive to chemical composition and has good performance stability. The equipment used is conventional smelting and belt-spinning equipment, and the material preparation process is simple, reliable and has good stability. Therefore, the magnetic alloy with large magnetostrictive strain at room temperature and low magnetic field provided by the present invention has excellent comprehensive performance and has potential application prospects in new sonar systems, high-power ultrasonic devices, precision positioning control, mechanical brakes and various magnetic drive devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The present invention will be further described in detail below in conjunction with the embodiments in the accompanying drawings, but this does not constitute any limitation to the present invention.
[0031] Figure 1 This is the room temperature X-ray diffraction pattern of the Co2CrGa alloy ingot sample obtained in Example 1 of the present invention.
[0032] Figure 2 Magnetic characterization structure of the Co2CrGa polycrystalline cast sample obtained in Example 1 of the present invention: (a) thermal magnetic (MT) curve; (b) room temperature magnetization (MH) curve.
[0033] Figure 3 This is the room temperature magnetostrictive strain-magnetic field curve of the Co2CrGa alloy ingot sample obtained in Example 1 of the present invention.
[0034] Figure 4 This is the room temperature magnetostrictive strain-magnetic field curve of the Co2CrGa polycrystalline strip sample obtained in Example 2 of the present invention: (a) room temperature XRD; (b) magnetostrictive curve diagram.
[0035] Figure 5 The Co2Cr obtained in Example 3 of the present invention 0.75 Ga 1.25 Room temperature magnetostrictive strain-magnetic field curve of polycrystalline sample: (a) Room temperature XRD; (b) magnetostrictive curve. DETAILED DESCRIPTION
[0036] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The materials used in the following examples are conventional materials unless otherwise specified; the experimental methods are conventional methods unless otherwise specified.
[0037] The present invention is described in detail below in conjunction with the accompanying drawings to fully describe the technical solution of the present invention.
[0038] <Example 1: Preparation method 1 of Co2CrGa and property test>
[0039] A magnetic alloy ingot with a large saturation magnetostriction coefficient at room temperature and low field of Co2CrGa is prepared. The polycrystalline sample ingot is melted in a water-cooled copper crucible under argon protection by an arc melting method. The sample is annealed in a vacuum quartz tube and then furnace-cooled to room temperature to obtain a sample with uniform composition.
[0040] Follow these specific steps:
[0041] S100, weigh Co, Cr, and Ga metal raw materials with a purity of 99.95% respectively according to the ratio of Co:Cr:Ga=2:1:1.
[0042] S200, put the weighed material into the crucible, and use a mechanical pump to pump the vacuum degree of the arc furnace chamber to 2×10 -3 Pa, and then argon was introduced as a protective gas, the melting current was 100A, each sample was turned over 3 times, and the melting was performed 5 times in total to ensure uniform composition.
[0043] S300, the obtained button ingot material is sealed in a vacuum quartz tube, annealed at 850° C. for 120 hours for homogenization annealing, and then gradually cooled to room temperature at a cooling rate of 2° C. / second to obtain a polycrystalline bulk ingot with a diameter of 1 cm;
[0044] S400, taking part of the polycrystalline ingot sample and grinding it to prepare powder, and determining the alloy crystal structure by X-ray diffraction experiment. The results show that the Co2CrGa magnetic alloy ingot sample prepared by the present invention has a cubic structure at room temperature, and its room temperature X-ray diffraction spectrum is shown in the attached Figure 1 .
[0045] S500, the polycrystalline bulk ingot is processed by an electric spark wire cutting machine to prepare a sample with a shape of 5 mm in length×3 mm in width×0.5 mm in thickness, and the magnetic and magnetostrictive properties of the Co2CrGa magnetic alloy are measured. Figure 2 As shown, the Curie temperature of the Co2CrGa alloy ingot sample prepared by the present invention is 507K, and the room temperature magnetization intensity-magnetic field curve of the sample is shown in Figure 2 ; Room temperature magnetostriction coefficient-magnetic field curve of alloy ingot sample is shown in Figure 3 ; The room temperature saturation magnetization, Curie temperature and room temperature saturation magnetostriction coefficient of the alloy ingot samples are shown in Table 1.
[0046] <Example 2: Preparation Method 2 of Co2CrGa and Property Test>
[0047] The invention discloses a magnetic alloy strip material with the components of Co2CrGa and a large saturation magnetostriction coefficient at room temperature and low field.
[0048] The arc melting method in Example 1 is used to prepare the bulk ingot. The bulk ingot is placed in a quartz tube, which is placed in the furnace chamber of a strip spinning machine. Under the protection of argon gas, induction heating is used to spray the molten alloy liquid onto a copper wheel and spin it out to obtain a strip of a certain size. The preparation method is carried out according to the following specific steps:
[0049] S100, Co, Cr, and Ga metal raw materials with a purity of 99.95% are weighed respectively according to the ratio of Co:Cr:Ga=2:1:1.
[0050] S200, the method for melting the sample is the same as that in Example 1.
[0051] S300, the method for heat treating the sample is the same as that in Example 1.
[0052] S400, put the button polycrystalline ingot of appropriate size melted by arc into a quartz tube with a small hole at the bottom, place it in the furnace chamber of the belt-spinning machine, and use a mechanical pump to evacuate the chamber to 10 -3 Pa, high-purity argon gas is introduced into the furnace chamber with a pressure of 0.05MPa. Induction heating is used to make the alloy in a molten state. Then the gas control valve is opened, and high-purity argon gas with a pressure of 0.05MPa is blown into the upper part of the quartz tube to make the molten alloy liquid spray from the small hole to the high-speed rotating copper wheel with a linear velocity of 25m / s and quickly thrown out to obtain a strip with a width of 3-4mm and a thickness of 30-50μm.
[0053] The room temperature XRD and magnetostrictive strain-magnetic field curves of the alloy ribbon sample are shown in the attached Figure 4 .
[0054] <Example 3: Co2Cr 0.75 Ga 1.25 Properties of the test>
[0055] Preparation components: Co2Cr 0.75 Ga 1.25 A magnetic alloy ingot having a large saturation magnetostriction coefficient at room temperature and low field; except that the composition ratio is Co:Cr:Ga=2:0.75:1.25, the sample annealing temperature is 900°C, and the annealing time is 72 hours, the remaining steps are the same as Example 1.
[0056] The room temperature XRD and magnetostrictive strain-magnetic field curves of the alloy sample are shown in the attached Figure 5 .
[0057] The room temperature saturation magnetization, Curie temperature and room temperature magnetostrictive strain of the alloy sample are shown in Table 1.
[0058] Table 1 Co2Cr with different compositions 1-x Ga 1+x Lattice constant, saturation magnetic moment and Curie temperature of the alloy.
[0059]
[0060] The above embodiments are preferred implementation modes of the present invention and are only used to facilitate the description of the present invention. They are not intended to limit the present invention in any form. Any person with ordinary knowledge in the relevant technical field, if they do not depart from the scope of the technical features of the present invention, can make equivalent embodiments by partial changes or modifications to the technical contents disclosed in the present invention, and they still fall within the scope of the technical features of the present invention without departing from the technical features of the present invention.
Claims
1. A method for preparing a magnetic alloy having large magnetostrictive strain at room temperature, It is characterized in that The steps include: S100, weighing Co, Cr, and Ga metal raw materials with a purity of 99.95% respectively according to the ratio of Co:Cr:Ga=2:1-x:1+x; The range of x is: 0≤x<1; S200, smelting method: put the weighed material into the crucible, and use a mechanical pump to pump the vacuum degree of the arc furnace chamber to 2×10 -3 Pa, then argon was introduced as protective gas, the melting current was 100A, each sample was turned over 3 times, and the melting was performed 5 times in total to ensure uniform composition; S300, heat treatment method: the obtained button ingot material is sealed in a vacuum quartz tube, annealed at 850°C to 900°C for 72 to 120 hours for homogenization annealing, and then gradually cooled to room temperature at a cooling rate of 2°C / second to obtain a polycrystalline bulk ingot.
2. A method for preparing a magnetic alloy having a large magnetostrictive strain at room temperature, It is characterized in that The steps include: S100, weighing Co, Cr, and Ga metal raw materials with a purity of 99.95% respectively according to the ratio of Co:Cr:Ga=2:1-x:1+x; The range of x is: 0≤x<1; S200, smelting method: put the weighed material into the crucible, and use a mechanical pump to pump the vacuum degree of the arc furnace chamber to 2×10 -3 Pa, then argon was introduced as protective gas, the melting current was 100A, each sample was turned over 3 times, and the melting was performed 5 times in total to ensure uniform composition; S300, heat treatment method: the obtained button ingot material is sealed in a vacuum quartz tube, annealed at 850°C to 900°C for 72 to 120 hours for homogenization annealing, and then gradually cooled to room temperature at a cooling rate of 2°C / second to obtain a polycrystalline bulk ingot; S400, put the button polycrystalline ingot into a quartz tube with a small hole at the bottom, place it in the furnace chamber of the belt spinning machine, and use a mechanical pump to evacuate the chamber to 10 -3 Pa, high-purity argon gas is introduced into the furnace chamber with a pressure of 0.05MPa. Induction heating is used to make the alloy in a molten state. Then the gas control valve is opened, and high-purity argon gas with a pressure of 0.05MPa is blown into the upper part of the quartz tube to make the molten alloy liquid spray from the small hole to the high-speed rotating copper wheel with a linear velocity of 25m / s and quickly thrown out to obtain a strip with a width of 3-4mm and a thickness of 30-50μm.
3. A magnetic alloy with large magnetostrictive strain at room temperature, It is characterized in that It is prepared by the preparation method described in claim 1; it has the following chemical formula: Co 2 Cr 1-x Ga 1+x , wherein the range of x is: 0≤x<1; the magnetic alloy is a polycrystalline ingot.
4. A magnetic alloy having large magnetostrictive strain at room temperature, It is characterized in that It is prepared by the preparation method described in claim 2; it has the following chemical formula: Co 2 Cr 1-x Ga 1+x , wherein the range of x is: 0≤x<1; the magnetic alloy is a polycrystalline strip.
5. The magnetic alloy having large magnetostrictive strain at room temperature according to claim 3 or 4, It is characterized in that Co 2 Cr 1-x Ga 1+x It is a cubic crystal system, the space group is Fm-3m, and the space group number is 225.
6. The magnetic alloy having large magnetostrictive strain at room temperature according to claim 3 or 4, It is characterized in that The magnetic alloy has a magnetostrictive strain of 18 to 60 ppm at a room temperature of 300 K and a critical magnetic field of 100 mT. 7.Co 2 Cr 1-x Ga 1+x As a magnetic alloy with large magnetostrictive strain at room temperature, It is characterized in that x range is: 0≤x<1; Co 2 Cr 1-x Ga 1+x The magnetostrictive strain is between 18 and 60 ppm.
8. Application of the magnetic alloy having large magnetostrictive strain at room temperature according to claim 3 or 4 in magnetic drive devices.
9. Application of the magnetic alloy having large magnetostrictive strain at room temperature according to claim 3 or 4 in sonar systems, ultrasonic devices, precision positioning control or mechanical brakes.
Citation Information
Cited By
Magnetic alloy preparation method based on four-arc pulling orientation crystal, magnetic alloy and application
CN120844185A