Preparation method of low-elasticity regenerated colored polyester staple fiber for non-woven fabric

By precrystallization, twin screw extrusion and ring blowing treatment of low-elastic polyester fibers, coupled with DTY elastic method, the carpet is solved by forming non-woven low-elastic recycled colored polyester staple fibers with excellent curling performance and smooth surface. Laying difficulty and fiber rigidity problems achieve higher laying thickness and comfort.

CN118895590APending Publication Date: 2024-11-05YANGZHOU TIANFULONG TECH FIBER CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411232191.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing low-elastic polyester fiber cannot be effectively laid when laying large-thick carpets, and are not curled firmly, and have insufficient smooth surface, resulting in difficult carpet laying and poor fiber rigidity.

Method used

A preparation method for regenerating non-elastic non-ferrous polyester staple fibers for nonwovens is adopted. The precrystallized polyester is sliced ​​and then heated and melted in a twin screw extruder, and then cooled and solidified in a ring blowing device, and carried out by DTY elastic method. Multiple stretches and windings to form special-shaped low-elastic recycled colored polyester staple fibers with excellent three-dimensional crimping properties and smooth surfaces.

Benefits of technology

It improves the elasticity and fluffy of the fiber, enhances the laying thickness and comfortable feel of the carpet, reduces the difficulty of laying, and improves the smoothness and bundling of the fiber, and reduces the coefficient of friction.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of low-elasticity regenerated colored polyester staple fibers for non-woven, belongs to the technical field of polyester reutilization, solves the problems that a large-thickness carpet cannot be laid, curling is not firm and smoothness is poor in the prior art, and comprises the steps of pre-crystallization, solid-phase polymerization of polyester chips, extrusion melting, spinning into tows and hot cylinder stretching. DTY is subjected to elasticity enhancing to form the special-shaped low-elasticity regenerated colored polyester staple fiber. The special-shaped low-elasticity regenerated colored polyester staple fiber prepared by the invention has excellent three-dimensional crimp performance, the elastic yarn has elasticity between spandex and nylon, has common polyester breaking strength and high elastic modulus, further improves the laying thickness of a laid carpet, reduces the knitting difficulty of the carpet, and improves the production efficiency of the carpet. The regenerated colored polyester staple fibers are prepared according to the special shape, the moisture removal and air permeability of the fibers are improved by increasing the cross sectional area of the monofilament surface, and it is guaranteed that the polyester fibers have good smoothness and bundling performance after being oiled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyester recycling, and in particular relates to a method for preparing low-elasticity regenerated colored polyester staple fibers for non-woven use. Background Art

[0002] Polyester low-elastic yarn is a type of textured yarn of polyester chemical fiber. It is made of polyester chips (PET) as raw material, using high-speed spinning of polyester pre-oriented yarn (POY), and then processed by drawing and false twisting. It has the characteristics of short process, high efficiency and good quality. It is an ideal raw material for knitting (weft knitting, warp knitting) or weaving. It is suitable for making clothing fabrics (such as suits, shirts), bedding (such as quilt covers, bedspreads, mosquito nets) and decorative items (such as curtain fabrics, sofa fabrics, wall coverings, and car interior decorative fabrics). Among them, fine denier yarn, especially three-leaf special-shaped yarn, is more suitable for making imitation silk fabrics, and coarse denier yarn can be used for imitation wool fabrics. In addition to the characteristics of high breaking strength and elastic modulus, excellent heat setting, good resilience, heat resistance, light resistance, strong corrosion resistance, easy washing and quick drying, it also has the characteristics of high fluffiness, good heat insulation, comfortable hand feel, soft luster, etc. Low-elastic yarn can also be used for sewing. The difference from general sewing thread is that the overlock is made of polyester filament without twisting, while the sewing thread is made of polyester staple fiber with twisting. However, the surface of this type of polyester fiber is not smooth enough, so when it is used as a carpet laying material, it is impossible to lay thick carpets. At the same time, due to low elasticity, the fiber curling is not firm enough and the rigidity is relatively poor. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing non-woven low-elasticity regenerated colored polyester staple fibers which are easy to lay thick carpets, have firm curling and good smoothness, in view of the shortcomings of the prior art.

[0004] In order to achieve the above technical purpose, the technical solution adopted by the method for preparing low-elasticity regenerated colored polyester staple fibers for non-woven use of the present invention is: A method for preparing low-elasticity regenerated colored polyester staple fibers for nonwovens comprises the following steps: S1 Weigh polyester chips, mica particles and polyether silicone oil in a mass ratio of 9.1:0.3:0.6, pre-crystallize the polyester chips, and then perform solid phase polymerization to obtain polyester chips with a viscosity of 1.02 dl / g, and then add the polyester chips, mica particles and polyether silicone oil into a reactor equipped with a stirring roller and a cooling coil and stir and mix them thoroughly; S2: The mixture obtained after being fully stirred and mixed in the reactor is fed into a twin-screw extruder, and the temperature is maintained at 370-375°C before the outlet of the twin-screw extruder, and heated and melted for 18 minutes. Subsequently, the temperature is maintained at 220-224°C at the outlet of the twin-screw extruder, and heated and melted for 6-8 minutes. After being metered by a metering pump, the mixture is fed into a spinning assembly and extruded from a special-shaped spinneret to form a filament bundle. S3: The tow is passed through a hot cylinder at a temperature of 80-95°C for 6 minutes, and then cooled and solidified in a ring-blowing device with a ring-blowing temperature of 47°C and a wind pressure of 0.069Kpa, and then oiled through a nozzle, and passed through a roller drafting, a heat box, and a cooling plate in sequence to form a primary special-shaped low-elasticity recycled colored polyester staple fiber; S4 adopts DTY texturing method, through pre-network nozzle, first roller, deformation hot box, cooling plate, false twister, second roller, main network nozzle, auxiliary second roller, shaping hot box, third roller, oiling wheel, winding forming, to produce special-shaped low-elasticity recycled colored polyester staple fiber.

[0005] Preferably, the pre-crystallization temperature in step S1 is 195-199° C., and the pre-crystallization time is 7-9 min.

[0006] Preferably, the solid phase polymerization temperature in step S1 is 320-324° C., and the solid phase polymerization time is 21-23 min.

[0007] Preferably, the spinneret holes in the special-shaped spinneret in step S2 are triangular hollow or diamond hollow shapes, and the degree of special-shapedness is 0.35 to 0.5.

[0008] Preferably, in the DTY texturing process in step S4, the processing speed is 500-600 m / min, the stretching multiple is 1.65-1.8 times, the deformation temperature is 170-195° C., the heat setting temperature is 150-170° C., and the surface linear velocity of the friction disk and the speed ratio D / Y of the yarn leaving the false twister are 1.90-1.95.

[0009] Preferably, in step S4, the polyester staple fibers are wound using a traverse box. During the winding process, a small anti-convex cam is installed, and the small anti-convex cam transmits movement to the forming swing plate through a connecting rod, so that the low-elasticity regenerated colored polyester staple fibers produce a slight swing.

[0010] Compared with the prior art, the present invention has the following beneficial effects: The special-shaped low-elasticity regenerated colored polyester staple fiber prepared by the present invention has excellent three-dimensional curling performance. The elastic yarn thereof has an elasticity between spandex and nylon, has the general polyester breaking strength and high elastic modulus, and also improves the fluffiness and comfortable hand feel, further improves the laying thickness of the laid carpet, and reduces the difficulty of carpet knitting; the regenerated colored polyester staple fiber is prepared according to the special shape, and the moisture discharge and air permeability of the fiber are improved by increasing the cross-sectional area of ​​the surface of the single yarn; the fiber yarn is false-twisted to keep the fiber yarn in a curled shape and fluffiness, and after oiling, the polyester fiber is ensured to have good smoothness and bundling, and the friction coefficient of the polyester is reduced, and the appearance has smoothness. DETAILED DESCRIPTION

[0011] The invention is further described below in conjunction with specific embodiments: A method for preparing low-elasticity regenerated colored polyester staple fibers for nonwovens comprises the following steps: S1 Weigh polyester chips, mica particles and polyether silicone oil in a mass ratio of 9.1:0.3:0.6, pre-crystallize the polyester chips, and then perform solid phase polymerization to obtain polyester chips with a viscosity of 1.02 dl / g, and then add the polyester chips, mica particles and polyether silicone oil into a reactor equipped with a stirring roller and a cooling coil and stir and mix them thoroughly; S2: The mixture obtained after being fully stirred and mixed in the reactor is fed into a twin-screw extruder, and the temperature is maintained at 370-375°C before the outlet of the twin-screw extruder, and heated and melted for 18 minutes. Subsequently, the temperature is maintained at 220-224°C at the outlet of the twin-screw extruder, and heated and melted for 6-8 minutes. After being metered by a metering pump, the mixture is fed into a spinning assembly and extruded from a special-shaped spinneret to form a filament bundle. S3 The filament bundle is passed through a hot cylinder with a temperature of 80-95°C and maintained for 6 minutes, and then cooled and solidified in a ring-blowing device with a ring-blowing temperature of 47°C and a wind pressure of 0.069Kpa, and then oiled through a nozzle, and successively passed through roller drawing, a hot box, and a cooling plate to form a primary special-shaped low-elasticity recycled colored polyester staple fiber; the fiber is heat-insulated and heated by a hot cylinder, and the thermoplasticity of the fiber filament is utilized to stretch it at a certain temperature, so that the fiber deformation is more complete and the fiber shrinkage rate is increased.

[0012] S4 adopts DTY texturing method, through pre-network nozzle, first roller, deformation hot box, cooling plate, false twister, second roller, main network nozzle, auxiliary second roller, shaping hot box, third roller, oiling wheel, winding forming, to produce special-shaped low-elasticity recycled colored polyester staple fiber.

[0013] In step S1, the pre-crystallization temperature is 195-199° C., the pre-crystallization time is 7-9 min, the solid phase polymerization temperature is 320-324° C., and the solid phase polymerization time is 21-23 min.

[0014] In the step S2, the spinneret holes in the special-shaped spinneret are triangular hollow or diamond hollow, and the degree of special-shapedness is 0.35-0.5.

[0015] In the step S4, the processing speed during the DTY texturing process is 500-600 m / min, the stretching multiple is 1.65-1.8 times, the deformation temperature is 170-195° C., the heat setting temperature is 150-170° C., wherein the surface linear velocity of the friction disk and the speed ratio D / Y of the yarn leaving the false twister are 1.90-1.95, and the polyester staple fiber is wound by a traverse box. During the winding process, a small anti-convex cam is installed, and the small anti-convex cam transmits the motion to the forming swing plate through a connecting rod, so that the low-elasticity regenerated colored polyester staple fiber produces a slight swing.

[0016] Embodiment 1 A method for preparing low-elasticity regenerated colored polyester staple fibers for nonwovens comprises the following steps: S1 Weigh polyester chips, mica particles and polyether silicone oil in a mass ratio of 9.1:0.3:0.6, pre-crystallize the polyester chips, and then perform solid phase polymerization to obtain polyester chips with a viscosity of 1.02 dl / g. The pre-crystallization temperature is 195-199°C, the pre-crystallization time is 7-9 min, the solid phase polymerization temperature is 320-324°C, and the solid phase polymerization time is 21-23 min. Then, add the polyester chips, mica particles and polyether silicone oil into a reactor equipped with a stirring roller and a cooling coil and stir and mix them thoroughly; S2: The mixture obtained after being fully stirred and mixed in the reactor is input into a twin-screw extruder, and the temperature is maintained at 373°C before the outlet of the twin-screw extruder, and heated and melted for 18 minutes, and then the temperature is maintained at 220-224°C at the outlet of the twin-screw extruder, and heated and melted for 6-8 minutes, and then fed into a spinning assembly after being metered by a metering pump to extrude from a special-shaped spinneret to form a filament bundle, wherein the spinneret holes in the special-shaped spinneret are triangular hollow and diamond hollow shapes, and the degree of special shape is 0.4; S3: The tow is passed through a hot cylinder at a temperature of 92°C for 6 minutes, and then cooled and solidified in a ring-blowing device with a ring-blowing temperature of 47°C and a wind pressure of 0.069Kpa, and then oiled through a nozzle, and passed through roller drafting, a heat box, and a cooling plate in sequence to form a primary profiled low-elasticity recycled colored polyester staple fiber; S4 adopts DTY texturing method, through pre-network nozzle, first roller, deformation hot box, cooling plate, false twister, second roller, main network nozzle, auxiliary second roller, setting hot box, third roller, oiling wheel, winding forming, the processing speed in DTY texturing process is 500-600 m / min, the stretching multiple is 1.65-1.8 times, the deformation temperature is 170-195°C, the heat setting temperature is 150-170°C, wherein the surface linear velocity of the friction disk and the speed ratio D / Y of the yarn leaving the false twister is 1.90-1.95, and the traverse box is used to wind the polyester staple fiber. During the winding process, a small anti-convex cam is installed, and the small anti-convex cam transmits the motion to the forming swing plate through the connecting rod, so that the low-elasticity recycled colored polyester staple fiber produces a slight swing, and the special-shaped low-elasticity recycled colored polyester staple fiber is obtained.

[0017] Embodiment 2 A method for preparing low-elasticity regenerated colored polyester staple fibers for nonwovens comprises the following steps: S1 Weigh polyester chips, mica particles and polyether silicone oil in a mass ratio of 9.1:0.3:0.6, pre-crystallize the polyester chips, and then perform solid phase polymerization to obtain polyester chips with a viscosity of 1.02 dl / g. The pre-crystallization temperature is 195-199°C, the pre-crystallization time is 7-9 min, the solid phase polymerization temperature is 320-324°C, and the solid phase polymerization time is 21-23 min. Then, add the polyester chips, mica particles and polyether silicone oil into a reactor equipped with a stirring roller and a cooling coil and stir and mix them thoroughly; S2: The mixture obtained after being fully stirred and mixed in the reactor is input into a twin-screw extruder, and the temperature is maintained at 370°C before the outlet of the twin-screw extruder, and heated and melted for 18 minutes, and then the temperature is maintained at 220-224°C at the outlet of the twin-screw extruder, and heated and melted for 6-8 minutes, and then fed into a spinning assembly after being metered by a metering pump and extruded from a special-shaped spinneret to form a filament bundle, wherein the spinneret hole in the special-shaped spinneret is a triangular hollow shape, and the degree of special-shapedness is 0.35; S3: The tow is passed through a hot cylinder at a temperature of 80°C for 6 minutes, and then cooled and solidified in a ring-blowing device with a ring-blowing temperature of 47°C and a wind pressure of 0.069Kpa, and then oiled through a nozzle, and passed through a roller drafting, a heat box, and a cooling plate in sequence to form a primary profiled low-elasticity recycled colored polyester staple fiber; S4 adopts DTY texturing method, through pre-network nozzle, first roller, deformation hot box, cooling plate, false twister, second roller, main network nozzle, auxiliary second roller, setting hot box, third roller, oiling wheel, winding forming, the processing speed in DTY texturing process is 500-600 m / min, the stretching multiple is 1.65-1.8 times, the deformation temperature is 170-195°C, the heat setting temperature is 150-170°C, wherein the surface linear velocity of the friction disk and the speed ratio D / Y of the yarn leaving the false twister is 1.90-1.95, and the traverse box is used to wind the polyester staple fiber. During the winding process, a small anti-convex cam is installed, and the small anti-convex cam transmits the motion to the forming swing plate through the connecting rod, so that the low-elasticity recycled colored polyester staple fiber produces a slight swing, and the special-shaped low-elasticity recycled colored polyester staple fiber is obtained.

[0018] Embodiment 3 A method for preparing low-elasticity regenerated colored polyester staple fibers for nonwovens comprises the following steps: S1 Weigh polyester chips, mica particles and polyether silicone oil in a mass ratio of 9.1:0.3:0.6, pre-crystallize the polyester chips, and then perform solid phase polymerization to obtain polyester chips with a viscosity of 1.02 dl / g. The pre-crystallization temperature is 195-199°C, the pre-crystallization time is 7-9 min, the solid phase polymerization temperature is 320-324°C, and the solid phase polymerization time is 21-23 min. Then, add the polyester chips, mica particles and polyether silicone oil into a reactor equipped with a stirring roller and a cooling coil and stir and mix them thoroughly; S2: The mixture obtained after being fully stirred and mixed in the reactor is input into a twin-screw extruder, and the temperature is maintained at 375°C before the outlet of the twin-screw extruder, and heated and melted for 18 minutes, and then the temperature is maintained at 220-224°C at the outlet of the twin-screw extruder, and heated and melted for 6-8 minutes, and then fed into a spinning assembly after being metered by a metering pump and extruded from a special-shaped spinneret to form a filament bundle, wherein the spinneret hole in the special-shaped spinneret is a diamond hollow shape, and the degree of special-shapedness is 0.5; S3: The tow is passed through a hot cylinder at a temperature of 95°C for 6 minutes, and then cooled and solidified in a ring-blowing device with a ring-blowing temperature of 47°C and a wind pressure of 0.069Kpa, and then oiled through a nozzle, and passed through a roller drafting, a heat box, and a cooling plate in sequence to form a primary profiled low-elasticity recycled colored polyester staple fiber; S4 adopts DTY texturing method, through pre-network nozzle, first roller, deformation hot box, cooling plate, false twister, second roller, main network nozzle, auxiliary second roller, setting hot box, third roller, oiling wheel, winding forming, the processing speed in DTY texturing process is 500-600 m / min, the stretching multiple is 1.65-1.8 times, the deformation temperature is 170-195°C, the heat setting temperature is 150-170°C, wherein the surface linear velocity of the friction disk and the speed ratio D / Y of the yarn leaving the false twister is 1.90-1.95, and the traverse box is used to wind the polyester staple fiber. During the winding process, a small anti-convex cam is installed, and the small anti-convex cam transmits the motion to the forming swing plate through the connecting rod, so that the low-elasticity recycled colored polyester staple fiber produces a slight swing, and the special-shaped low-elasticity recycled colored polyester staple fiber is obtained.

[0019] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the scope of implementation of the present invention. All equivalent changes and modifications in the shape, structure, characteristics and spirit of the claims of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing low-elasticity regenerated colored polyester staple fibers for non-woven fabrics, characterized in that: The following steps are involved: S1 Weigh polyester chips, mica particles and polyether silicone oil in a mass ratio of 9.1:0.3:0.6, pre-crystallize the polyester chips, and then perform solid phase polymerization to obtain polyester chips with a viscosity of 1.02 dl / g, and then add the polyester chips, mica particles and polyether silicone oil into a reactor equipped with a stirring roller and a cooling coil and stir and mix them thoroughly; S2: The mixture obtained after being fully stirred and mixed in the reactor is fed into a twin-screw extruder, and the temperature is maintained at 370-375°C before the outlet of the twin-screw extruder, and heated and melted for 18 minutes. Subsequently, the temperature is maintained at 220-224°C at the outlet of the twin-screw extruder, and heated and melted for 6-8 minutes. After being metered by a metering pump, the mixture is fed into a spinning assembly and extruded from a special-shaped spinneret to form a filament bundle. S3: The tow is passed through a hot cylinder at a temperature of 80-95°C for 6 minutes, and then cooled and solidified in a ring-blowing device with a ring-blowing temperature of 47°C and a wind pressure of 0.069Kpa, and then oiled through a nozzle, and passed through a roller drafting, a heat box, and a cooling plate in sequence to form a primary special-shaped low-elasticity recycled colored polyester staple fiber; S4 adopts DTY texturing method, through pre-network nozzle, first roller, deformation hot box, cooling plate, false twister, second roller, main network nozzle, auxiliary second roller, shaping hot box, third roller, oiling wheel, winding forming, to produce special-shaped low-elasticity recycled colored polyester staple fiber.

2. The method for preparing the low-elasticity regenerated colored polyester staple fiber for non-woven use according to claim 1, characterized in that: The pre-crystallization temperature in step S1 is 195-199° C., and the pre-crystallization time is 7-9 minutes.

3. The method for preparing the low-elasticity regenerated colored polyester staple fiber for non-woven use according to claim 1, characterized in that: The solid phase polymerization temperature in step S1 is 320-324° C., and the solid phase polymerization time is 21-23 min.

4. The method for preparing the low-elasticity regenerated colored polyester staple fiber for non-woven use according to claim 1, characterized in that: In the step S2, the spinneret holes in the special-shaped spinneret are triangular hollow or diamond hollow, and the degree of special-shapedness is 0.35-0.

5.

5. The method for preparing the low-elasticity regenerated colored polyester staple fiber for non-woven use according to claim 1, characterized in that: In the step S4, the processing speed during the DTY texturing process is 500-600 m / min, the stretching multiple is 1.65-1.8 times, the deformation temperature is 170-195° C., the heat setting temperature is 150-170° C., and the D / Y value of the surface linear velocity of the friction disk and the speed of the yarn leaving the false twister is 1.90-1.

95.

6. The method for preparing the low-elasticity regenerated colored polyester staple fiber for non-woven use according to claim 1, characterized in that: In the step S4, the polyester staple fibers are wound by a traverse box. During the winding process, a small anti-convex cam is installed. The small anti-convex cam transmits the motion to the forming swing plate through a connecting rod, so that the low-elasticity regenerated colored polyester staple fibers produce a slight swing.

Citation Information

Patent Citations

  • Cool cotton feeling polyester low-elastic yarn and processing technology thereof

    CN102383206A

  • Manufacturing method of special-shaped hollow warmth keeping polyester drawn textured yarn

    CN105908269A

  • Anti-deformation low stretch yarn and processing and preparing technology thereof

    CN112941647A

  • Elasticity enhancing method of functional polyester low-elasticity fiber

    CN116288837A