Finishing and dyeing process of knitted three-dimensional fabric
By performing the molding, shrinking, pre-designing, dyeing and post-treatment processes in the finishing and dyeing process of knitted three-dimensional fabrics, combined with appropriate temperature and leavening agents, the problem of difficult to control the shrinkage degree of three-dimensional fabrics is solved, and dimensional stability and Improvement of three-dimensional effect.
Patent Information
- Application Number
- CN202411204096.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-05
AI Technical Summary
The finishing and dyeing process of existing knitted three-dimensional fabrics is difficult to control the degree of shrinkage, resulting in large size differences between batches and cannot be applied to large-formed fabrics.
The embryo cloth is used for shaping, shrinking, pre-designing, dyeing, post-treatment and finalization processes. By controlling the temperature, vehicle speed and air volume, it is necessary to ensure that the fabric produces a three-dimensional effect within the specified shrinkage range, and add a loosening agent to the post-treatment process to Increase elasticity.
It realizes stable control of the size of the three-dimensional fabric, avoids excessive shrinkage and deformation, improves the three-dimensional effect and diversity, and ensures the elasticity and stiffness of the fabric.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of finishing and dyeing technology, and in particular to a finishing and dyeing technology for knitted three-dimensional fabrics. Background Art
[0002] Three-dimensional fabrics are very interesting and decorative, and they meet the contemporary people's pursuit of fashion. The Chinese invention patent with publication number CN107338557A discloses a weaving method for a polyester high-shrinkage single-layer concave-convex bedding fabric, which specifically discloses the use of raw materials with large heat shrinkage as weft yarns, and the concave-convex three-dimensional effect is obtained after post-finishing. However, the shrinkage degree of the three-dimensional fabric is difficult to control, there are differences between different batches, and the size of the three-dimensional pattern varies greatly. These problems make the finishing process unsuitable for three-dimensional fabrics with large patterns. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a finishing and dyeing process for knitted three-dimensional fabrics which can maintain the pattern size.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a finishing and dyeing process of a knitted three-dimensional fabric, comprising the following steps: the grey cloth is subjected to a shaping process, a shrinking process, a predetermined process, a dyeing process, a post-processing process and a finishing process in sequence.
[0005] The beneficial effect of the present invention is that the dyeing process of the present invention first shapes the grey cloth, completes pre-shrinkage, reduces the overall shrinkage of the fabric, and then performs refining to ensure that the grey cloth is within a specified shrinkage range, which can produce a three-dimensional effect due to shrinkage and avoid excessive shrinkage of the pattern size being far smaller than the required finished product size. DETAILED DESCRIPTION
[0006] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in conjunction with the implementation modes.
[0007] A finishing and dyeing process for knitted three-dimensional fabrics comprises the following steps: the grey fabric is subjected to a shaping process, a shrinking process, a presetting process, a dyeing process, a post-processing process and a finishing process in sequence.
[0008] From the above description, it can be seen that the beneficial effects of the present invention are: since there is longitudinal tension in the concentrator, if the concentrating machine is directly used without performing the shaping process, the problem of excessive shrinkage of the fabric or insufficient longitudinal shrinkage of the fabric will occur. When the fabric shrinks excessively, the fabric surface needs to be stretched during shaping, which can easily cause the fabric surface to be flat; when the fabric shrinks insufficiently in the longitudinal direction, it will cause the fabric to be unstable and the pattern to be easily deformed.
[0009] The present invention first shapes and then shrinks the grey cloth. The shaping process can complete pre-shrinkage to ensure that the grey cloth shrinks sufficiently in the longitudinal direction. The grey cloth shrinks within a specified range to produce a three-dimensional effect, and the pattern does not deform or become excessively smaller. Then, the predetermined process, dyeing process, post-processing process and finalizing process are carried out in sequence. The predetermined process and finalizing process only need to adopt flat width setting without stretching, and the three-dimensional effect of the fabric is better.
[0010] Furthermore, the temperature of the shaping process is 120-140° C., the vehicle speed is 20-25 m / min, and the air volume is 30-50%.
[0011] From the above description, it can be seen that the function of the shaping process is to control the shrinkage of the grey cloth. Adding a low-temperature shaping process before the shrinking process can reduce the overall shrinkage of the fabric and ensure the three-dimensional effect. After low-temperature shaping, the width of the pattern of the grey cloth is reduced by about 2cm and the height is reduced by about 3cm. Using a lower temperature for shaping can reduce the shrinkage of the yarn and prevent wrinkles on the fabric surface. The uneven shrinkage of the yarn can be used to achieve a concave and convex three-dimensional effect.
[0012] The air volume in the shaping process should not be too large. Air volume greater than 50% will cause the fabric to become flat.
[0013] Furthermore, the temperature of the reduction process is 60 to 80° C., and the vehicle speed is 20 to 25 m / min.
[0014] From the above description, it can be seen that the shrinking process causes the fabric to shrink for the second time, increasing the three-dimensional effect. The shrinking temperature is relatively low, which can reduce the degree of stretching of the fabric by the predetermined tension.
[0015] Furthermore, the temperature of the predetermined process is 160-190° C., the vehicle speed is 20-25 m / min, and the air volume is 50-70%.
[0016] From the above description, it can be seen that if the air volume in the predetermined process is greater than 70%, the three-dimensional degree will be reduced, and if the air volume is less than 50%, the hot wind force will be reduced, and the predetermined stability will be reduced, which will increase the shrinkage of the fabric during dyeing and the pattern size will shrink excessively. Therefore, the temperature of the predetermined process is controlled to be 160-190℃ and the air volume is 50-70%.
[0017] Furthermore, the upper overfeed of the predetermined process is 3 to 8%, and the lower overfeed is -3 to 3%.
[0018] Furthermore, the temperature of the dyeing process is 110-130° C., and the dyeing time is 30-50 min.
[0019] Furthermore, a leavening agent is added in the post-processing step.
[0020] From the above description, it can be seen that adding a bulking agent in the post-processing process can increase the elasticity of the fabric. The addition of an appropriate bulking agent can improve the stiffness of the yarn and the restoring force of the raised areas of the fabric, thereby maintaining the elasticity of the fabric.
[0021] Furthermore, the amount of bulking agent added is 0.2 to 0.6 owf of the weight of the grey cloth. 。
[0022] From the above description, it can be seen that when the bulking agent addition rate is less than 0.2owf, the effect is not obvious; when the bulking agent addition rate is greater than 0.6owf, the fabric surface will become soft, the bone feel and support of the fabric will be reduced, and the elasticity will be reduced; therefore, the amount of bulking agent added is controlled to be 0.2-0.6owf of the grey fabric mass.
[0023] Furthermore, the temperature of the post-treatment process is 60-80° C., and the treatment time is 30-40 min.
[0024] Furthermore, the temperature of the forming process is 150-160° C., and the vehicle speed is 20-25 m / min.
[0025] Furthermore, the upper overfeed of the fixed process is 2-7%, and the lower overfeed is -2-2%.
[0026] Furthermore, the grey cloth comprises a surface layer, an intermediate connecting layer and a bottom layer which are connected in sequence, the surface layer comprises a jacquard; the surface layer is woven from chemical fiber multifilament, the intermediate connecting layer is woven from chemical fiber monofilament, and the bottom layer is woven from elastic fiber.
[0027] From the above description, it can be seen that due to the different materials of the surface layer and the bottom layer, their shrinkage rates after dyeing are different. The shrinkage rate of the bottom layer is larger and the shrinkage is more obvious, while the shrinkage rate of the surface layer is smaller. After dyeing, the excess surface jacquard bulges upward to form a three-dimensional jacquard.
[0028] Embodiment 1 of the present invention is: a finishing process for knitted three-dimensional fabrics, the steps are as follows:
[0029] S1. Woven grey cloth: The grey cloth is composed of a surface layer, an intermediate connecting layer and a bottom layer which are connected in sequence, and the surface layer includes a jacquard; the surface layer is woven from chemical fiber multifilament, the intermediate connecting layer is woven from chemical fiber monofilament, and the bottom layer is woven from elastic fiber.
[0030] S2, shaping process: temperature is 130℃, speed is 20m / min, air volume is 30%.
[0031] S3, refining process: temperature is 60°C, speed is 20m / min.
[0032] S4, scheduled process: temperature is 160℃, vehicle speed is 20m / min, air volume is 60%, upper overfeed is 5%, and lower overfeed is 1%.
[0033] S5, dyeing process: temperature is 120°C, dyeing time is 30 minutes.
[0034] S6: Post-treatment process: the temperature is 70°C, the treatment time is 30 minutes, and 7006 leavening agent is added at 0.6 owf of the grey cloth mass.
[0035] S7: Finishing process: the temperature is 150°C, the speed is 20m / min, the upper overfeed of the finishing process is 4%, and the lower overfeed is 1%.
[0036] After dyeing, the lateral shrinkage of the finished fabric is 25%, the longitudinal shrinkage is 15%, and the thickness difference between the raised and recessed parts is 5 mm.
[0037] Comparative Example 1 of the present invention is:
[0038] The difference between Comparative Example 1 and Example 1 is that the shaping process is not included.
[0039] After dyeing, the shrinkage rate of the finished fabric is 35%, the longitudinal shrinkage rate is 20%, the thickness difference between the raised and recessed parts is 7mm, and the fabric surface is wrinkled and uneven.
[0040] Comparative Example 2 of the present invention is:
[0041] The difference between Comparative Example 2 and Example 1 is that the shaping process and the refining process are not included.
[0042] After dyeing, the shrinkage rate of the finished fabric is 40%, the longitudinal shrinkage rate is 35%, and the fabric surface is severely wrinkled.
[0043] Comparative Example 3 of the present invention is:
[0044] The only difference between Comparative Example 3 and Example 1 is that 7006 leavening agent is not added in the post-treatment process.
[0045] The finished fabric after dyeing has poor elasticity and recovery of raised areas.
[0046] Embodiment 2 of the present invention is: a finishing process for knitted three-dimensional fabrics, the steps are as follows:
[0047] S1. Woven grey cloth: The grey cloth comprises a surface layer, an intermediate connecting layer and a bottom layer which are connected in sequence, and the surface layer comprises a jacquard; the surface layer is woven from chemical fiber multifilament, the intermediate connecting layer is woven from chemical fiber monofilament, and the bottom layer is woven from elastic fiber.
[0048] S2, shaping process: temperature is 120℃, speed is 25m / min, air volume is 40%.
[0049] S3, refining process: temperature is 70°C, speed is 20m / min.
[0050] S4, scheduled process: temperature is 190℃, vehicle speed is 20m / min, air volume is 50%, upper overfeed is 3%, and lower overfeed is -3%.
[0051] S5, dyeing process: temperature is 110°C, dyeing time is 35 minutes.
[0052] S6: Post-treatment process: the temperature is 70°C, the treatment time is 40 minutes, and 7006 leavening agent is added at 0.4 owf of the grey cloth mass.
[0053] S7: Finishing process: the temperature is 160°C, the speed is 20m / min, the upper overfeed of the finishing process is 7%, and the lower overfeed is 2%.
[0054] Embodiment 3 of the present invention is: a dyeing process for knitted three-dimensional fabrics, the steps are as follows:
[0055] S1. Woven grey cloth: The grey cloth comprises a surface layer, an intermediate connecting layer and a bottom layer which are connected in sequence, and the surface layer comprises a jacquard; the surface layer is woven from chemical fiber multifilament, the intermediate connecting layer is woven from chemical fiber monofilament, and the bottom layer is woven from elastic fiber.
[0056] S2, shaping process: temperature is 140℃, speed is 22m / min, air volume is 50%.
[0057] S3, refining process: temperature is 80°C, speed is 25m / min.
[0058] S4, scheduled process: temperature is 170℃, vehicle speed is 25m / min, air volume is 70%, upper overfeed is 8%, and lower overfeed is 3%.
[0059] S5, dyeing process: temperature is 130°C, dyeing time is 50 minutes.
[0060] S6: Post-treatment process: the temperature is 60°C, the treatment time is 35 minutes, and 7006 leavening agent is added at 0.2 owf of the grey cloth mass.
[0061] S7: Finishing process: the temperature is 150°C, the speed is 25m / min, the upper overfeed of the finishing process is %, and the lower overfeed is -2%.
[0062] In summary, the dyeing process of the knitted three-dimensional fabric provided by the present invention has the following advantages:
[0063] 1. The present invention first shapes the grey cloth and then shrinks it, thereby avoiding the problems of excessive shrinkage and insufficient longitudinal shrinkage of the fabric caused by shrinkage, and obtaining a large-sized three-dimensional pattern.
[0064] 2. Since the grey cloth has been shrunk through the shaping and shrinking processes, the predetermined and final processes only require flat-width shaping without stretching, and the three-dimensional effect of the fabric is better.
[0065] 3. The shaping process uses a lower temperature to prevent wrinkles on the fabric.
[0066] 4. The air volume in the shaping process, the predetermined process and the final process is relatively low to avoid the fabric becoming flat and the three-dimensional effect being weakened.
[0067] 5. Adding bulking agents in the post-processing process can increase the elasticity of the fabric, which can improve the stiffness of the yarn and the restoring force of the raised areas of the fabric.
[0068] 6. Use yarns with different shrinkage rates to weave the grey cloth, and obtain three-dimensional patterns after dyeing to improve the diversity of the shape.
[0069] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the specification of the present invention, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A dyeing process for knitted three-dimensional fabrics, characterized in that: The following steps are involved: The grey cloth undergoes shaping process, shrinking process, pre-setting process, dyeing process, post-processing process and finishing process in sequence.
2. The dyeing process of the knitted three-dimensional fabric according to claim 1, characterized in that: The temperature of the shaping process is 120-140° C., and the vehicle speed is 20-25 m / min.
3. The dyeing process for knitted three-dimensional fabric according to claim 1, characterized in that: The temperature of the reduction process is 60-80° C., and the vehicle speed is 20-25 m / min.
4. The dyeing process for knitted three-dimensional fabric according to claim 1, characterized in that: The temperature of the predetermined process is 160-190° C., and the vehicle speed is 20-25 m / min.
5. The dyeing process for knitted three-dimensional fabric according to claim 1, characterized in that: The temperature of the dyeing process is 110-130° C., and the dyeing time is 30-50 minutes.
6. The dyeing process for knitted three-dimensional fabric according to claim 1, characterized in that: A leavening agent is added in the post-processing step.
7. The dyeing process for knitted three-dimensional fabric according to claim 6, characterized in that: The amount of the leavening agent added is 0.2-0.6 owf of the grey cloth mass.
8. The dyeing process for knitted three-dimensional fabric according to claim 1, characterized in that: The temperature of the post-treatment process is 60-80° C., and the treatment time is 30-40 minutes.
9. The dyeing process for knitted three-dimensional fabric according to claim 1, characterized in that: The temperature of the forming process is 150-160° C., and the vehicle speed is 20-25 m / min.
10. The dyeing process of knitted three-dimensional fabric according to claim 1, characterized in that: The grey cloth comprises a surface layer, an intermediate connecting layer and a bottom layer which are connected in sequence, the surface layer comprises a jacquard; the surface layer is woven from chemical fiber multifilaments, the intermediate connecting layer is woven from chemical fiber monofilaments, and the bottom layer is woven from elastic fibers.