A method for judging the acid replacement of polysilicon cleaning liquid mixed acid

By cleaning and etching the polysilicon sample block with the silicon block to be cleaned, the etching depth is measured and the data list is constructed, and the etching ability of the subsequent cleaning solution is estimated, the problem of degradation of acid mixed etching ability is solved, and efficient utilization and The effect of cost reduction.

CN118896822BActive Publication Date: 2024-11-26内蒙古大全半导体有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411378641.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-26
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

The etching capacity of existing polycrystalline silicon cleaning liquid mixed with acid has decreased, resulting in frequent replacement of cleaning liquids. The existing evaluation methods require high-priced detection instruments and high maintenance costs, making it difficult to maximize the efficiency of the cleaning liquid.

Method used

By cleaning and etching the polysilicon sample block with the silicon block to be cleaned, the etching depth is measured, the data list is constructed to estimate the etching capacity of the subsequent cleaning liquid, and the cleaning liquid is replaced regularly to reduce waste and cost.

Benefits of technology

Quantitative measurement of etching depth is realized, which maximizes the utilization efficiency of mixed acid acid solution, reduces the overall cost of the cleaning process, and avoids expensive detection instruments and high maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118896822B_ABST
    Figure CN118896822B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of polysilicon, and specifically discloses a method for judging the acid replacement of a polysilicon cleaning solution by mixed acid, which comprises preparing a sample block, cleaning and etching, measuring the etching thickness of the sample block, constructing a data list, and estimating the number of cleaning batches after the cleaning solution is subsequently replaced. The present invention constructs a data list of the etching capacity of a mixed acid solution according to the etching thickness of the sample block, and estimates and guides the batches that need to be replaced with acid in the subsequent same process according to the data list, without the need for expensive testing equipment and the transformation of a production line, thereby improving the accuracy of estimating the acid replacement batches, improving the utilization efficiency of the mixed acid solution, and greatly reducing the cost of the cleaning process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polysilicon, and in particular to a method for judging acid replacement of a polysilicon cleaning solution with mixed acid. Background Art

[0002] The content of metal impurities on the surface of polysilicon for chips is a key quality indicator in the electronics industry. Its stability is closely related to the development and progress of electronics companies. Metal impurities on the surface of polysilicon usually come from metal debris contaminated during the mechanical processing of silicon blocks. In the existing process, the mixed acid etching process is mainly used, that is, by etching away a certain thickness of the outer skin of the silicon block, to achieve the purpose of efficiently removing surface impurities. The main cleaning liquid used is a mixed acid composed of hydrofluoric acid and nitric acid. After mixing hydrofluoric acid and nitric acid based on a certain ratio, it can etch the surface of polysilicon for chips. The polysilicon for chips first reacts with nitric acid to produce silicon dioxide, and the produced silicon dioxide reacts with hydrofluoric acid to generate hexafluoride and certain nitrogen oxides. This cleaning method can effectively remove the oxide layer produced in the water washing process, and can also remove particles and metal substances attached to the oxide layer.

[0003] After the mixed acid cleaning solution has been used for a period of time, the etching ability of the acid solution decreases and cannot meet the process requirements. The cleaning solution needs to be replaced. Since the quality of nitric acid and hydrofluoric acid used in the cleaning solution in the existing process is ultra-high purity reagents of UP-S or above, the cost is relatively high. It is necessary to use up the cleaning ability of the cleaning solution as much as possible and then replace it with a new cleaning solution to spread the cost of changing the cleaning solution. Therefore, after each cleaning process is changed, various process parameters such as the concentration ratio of the mixed acid are changed, and the cleaning quality and cleaning ability of the cleaning solution need to be re-evaluated to ensure the maximum utilization of the cleaning solution. There is a technology, such as the invention patent of a method for evaluating a polysilicon cleaning solution with Chinese patent publication number CN113624704B, which provides a method for judging the concentration of nitric acid and hydrofluoric acid in the cleaning solution by comparing the absorbance of the cleaning solution with a reference value, and then calculating the etching ability of the mixed acid in the cleaning solution to judge the cleaning quality of the cleaning solution. This method requires extracting liquid from the acid tank, and the test instrument used is expensive and needs to be modified on the original equipment. In addition, the circulating pipe and detection system used are easily corroded by the mixed acid in the cleaning solution after long-term operation, and the maintenance cost is high. Summary of the invention

[0004] The purpose of the present invention is to provide a method for determining whether to replace mixed acid with acid in a polysilicon cleaning solution, so as to solve the problems existing in the prior art.

[0005] The present invention is implemented by the following technical scheme: A method for judging the acid replacement of polysilicon cleaning liquid mixed acid, comprising the following steps:

[0006] S1: Prepare the sample: Cut the polycrystalline bar into a number of cubic samples with equal side lengths. The side length of the sample is L, and the unit of the side length L of the sample is mm;

[0007] S2: cleaning and etching: the sample block in step S1 and the silicon block to be cleaned are placed in the basket at the same time, and the sample block and the silicon block to be cleaned pass through each cleaning tank for cleaning and etching, and the sample block is taken out after cleaning;

[0008] S3: Measure the etched thickness of the sample block: Measure the mass M1 before cleaning and the mass M2 after cleaning of the sample block in step S2, and calculate its etched thickness H: H = [(M2-M1) / ρ] / (L 2 ×6), where M1 and M2 are in g, and ρ is the density of the polysilicon material of the sample in g / mm 3 ;

[0009] S4: Construct a data table: The mixed acid etching capacity of the cleaning solution of the first batch of cleaning samples is 100%; the mixed acid etching capacity of the cleaning solution of each subsequent batch of cleaning samples is calculated by the following method:

[0010] The mixed acid etching capacity of the cleaning solution of the nth batch = [1-1 / (N-1) × (n-1)] × 100%, where N is the total number of cleaning batches; the etching thickness of the sample after the nth batch cleaning is H n , when 0.95H n <H k When the mixed acid etching capacity of the cleaning solution after the nth batch of cleaning is 0, H k is the minimum etching thickness required by the process; construct a data list of the etching thickness H of all batches of cleaned samples and the mixed acid etching capacity of the corresponding cleaning solution;

[0011] S5: Estimate the number of cleaning batches after the cleaning solution is replaced: After the cleaning solution is replaced, estimate the mixed acid etching capacity of the cleaning solution after the cleaning solution is replaced according to the data list obtained in step S4. When the etching capacity of the cleaning batch in the data list reaches 20%, the current cleaning batch and every 4 cleaning batches thereafter need to repeat steps S1-S3 to measure the etching thickness H of the sample block. When 0.95H<H k Replace the cleaning fluid.

[0012] Furthermore, in step S5, when the estimated etching capacity reaches 5%, the etching thickness H at this time is measured by repeating steps S1-S3 for the current batch and each subsequent batch. When 0.95H<H k Replace the cleaning fluid.

[0013] Furthermore, H k It is 0.002-0.03mm.

[0014] Furthermore, the side length L of the sample block in step S1 is the median of the size range of the cleaned polysilicon blocks.

[0015] Furthermore, the surface Ra value of the sample block is less than 0.8 μm.

[0016] Furthermore, the side length of the sample block is one of 4 mm, 15 mm, 38 mm, and 75 mm.

[0017] Furthermore, in step 2, a sample block in step S1 is placed in the middle and at both ends of the diagonal line of the basket respectively.

[0018] Furthermore, the etching thickness H of the sample block in step S4 is n is the average value of the etching thickness H of the three sample blocks.

[0019] Advantages of the present invention:

[0020] 1. By cleaning and etching the sample block together with the silicon block, the etching depth can be quantitatively measured, and then the etching capacity of the mixed acid of the cleaning liquid in subsequent production can be estimated through the data list of the etching capacity of the first batch of cleaning liquid, which can maximize the utilization efficiency of the mixed acid solution, reduce the waste of the mixed acid solution, and reduce the overall cost of the cleaning process.

[0021] 2. The sample blocks used can be used as finished products together with product silicon blocks after cleaning, which will not cause waste of polycrystalline silicon block products and does not require expensive testing instruments and equipment modifications. The testing method is simple and low-cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a flow chart of a method for judging acid replacement of polysilicon cleaning solution by mixed acid. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] In the description of the present invention, it should be noted that the terms "center", "up", "down", "front", "back", "top", "bottom", "left", "right", "vertical", "horizontal", "inside" and "outside" etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they should not be understood as limiting the present invention.

[0025] like Figure 1 As shown: A method for judging whether to replace acid with mixed acid in a polysilicon cleaning solution comprises the following steps:

[0026] S1: Prepare the sample: Cut the polycrystalline rod into several cube samples with equal side lengths. The side length of the sample is L, and the unit of the side length L is mm. The side length L of the sample is the median size of the cleaned polysilicon block. The current standard size of polycrystalline silicon products for chips is 2-6mm, 6-25mm, 25-50mm, and 50-100mm, four conventional sizes. Therefore, the side length of the sample corresponding to the size of the polycrystalline silicon product can be 4mm, 15mm, 38mm, and 75mm. The sample is selected from polycrystalline silicon rods produced with the same formula as the official product. The machine cutting (wire cutting machine pulling high-speed rotating diamond wire cutting) is used to cut the polycrystalline silicon rods. The polysilicon in the middle of the rod-shaped material, more than 20 mm away from the silicon core and more than 20 mm away from the skin, is selected. After machining, the surface Ra value of the sample is less than 0.8μm. The prepared sample has the same chemical properties as the silicon block to be cleaned. Therefore, during the cleaning and etching process, the etched thickness of the sample can represent the average level of the thickness of the silicon blocks in this batch after cleaning and etching. Since the polysilicon rods are broken into product silicon blocks that are generally irregular in shape, it is impossible to specifically measure their etched thickness. Therefore, by using mechanically processed samples with regular and measurable shapes for cleaning and etching, the etched thickness value of the silicon blocks cleaned together can be known, thereby performing accurate quantification.

[0027] S2: Cleaning and etching: The sample blocks in step S1 are placed in the material basket together with the silicon blocks to be cleaned. The sample blocks are passed through each cleaning tank for cleaning and etching together with the silicon blocks to be cleaned. The sample blocks are taken out after cleaning. During the first cleaning after changing the cleaning process, the silicon blocks cleaned by the first batch of cleaning liquid need to be made into sample blocks for synchronous cleaning to determine the etching thickness of each batch of silicon blocks under the cleaning process conditions.

[0028] S3: Measure the etched thickness of the sample block: Measure the mass M1 before cleaning and the mass M2 after cleaning of the sample block in step S2, and calculate its etched thickness H: H = [(M2-M1) / ρ] / (L 2×6), where M1 and M2 are in units of g, and ρ is the density of the polysilicon material of the sample block in g / mm³; the change of L before and after cleaning can be ignored for the result calculation. The etching thickness of the sample block in this batch can be calculated by measuring the difference before and after cleaning. The etching thickness of the sample block represents the average etching thickness of other silicon blocks in this batch.

[0029] S4: Construct a data table: The mixed acid etching capacity of the cleaning solution of the first batch of cleaning samples is 100%; the mixed acid etching capacity of the cleaning solution of each subsequent batch of cleaning samples is calculated by the following method:

[0030] The mixed acid etching capacity of the nth batch of cleaning solution = [1-1 / (N-1)×(n-1)]×100%, where N is the total number of all actual cleaning batches.

[0031] The etching thickness of the sample block after the nth batch of cleaning is H n , when 0.95Hn<H k When the mixed acid etching capacity of the cleaning solution after the nth batch of cleaning is 0, H k is the minimum etching thickness required by the process, H k It is 0.002-0.03mm, and the specific value needs to be determined according to the process requirements to determine its minimum etching thickness; based on the above data, a data list of the etching thickness H of all batches of cleaned samples and the mixed acid etching capacity of the corresponding cleaning solution is constructed.

[0032] S5: Estimate the number of cleaning batches after the cleaning solution is replaced: After the cleaning solution is replaced, estimate the mixed acid etching capacity of the cleaning solution after the cleaning solution is replaced according to the data list obtained in step S4. When the etching capacity of the cleaning batch in the data list reaches 20%, the current cleaning batch and every 4 cleaning batches thereafter need to repeat steps S1-S3 to measure the etching thickness H of the sample block. When 0.95H<H k When the cleaning liquid is replaced, that is, when the cleaning liquid mixed acid etching ability is low, the etching thickness H is measured once every 4 batches according to the method of steps S1-S3 to ensure that the etching thickness of the product meets the process requirements and prevent other factors from affecting the cleaning liquid mixed acid etching ability, resulting in a decrease in the cleaning liquid mixed acid etching ability and insufficient etching thickness of the silicon block, affecting product quality; when the estimated etching ability reaches 5%, the current batch and each subsequent batch repeat the method of steps S1-S3 to measure the etching thickness H at this time, when 0.95H<H kWhen the estimated etching capacity reaches 5%, the cleaning liquid is replaced. It is close to the etching limit of the cleaning liquid mixed acid. In order to make full use of the etching capacity of the cleaning liquid mixed acid as much as possible, reduce the waste of the mixed acid, and ensure the etching thickness that meets the process requirements, the method of steps S1-S3 is repeated in each batch to measure the etching thickness H at this time until the etching capacity of the cleaning liquid mixed acid is exhausted and then the acid is replaced. At this time, the cleaning liquid mixed acid reaches the maximum utilization efficiency, effectively spreading the cost of each cleaning; at the same time, the sample block used for the test can also be used as a product, which will not cause waste of products.

[0033] In order to avoid the impact of slightly different cleaning and etching thicknesses on the test results when the sample blocks are placed at different positions of the basket, the sample blocks are placed in the middle and at both ends of the diagonal of the basket in step S2, with one sample block placed at each of the above positions. The etching thickness of the sample blocks in step S3 is the average of the etching thicknesses of the sample blocks at three different positions.

[0034] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0035] Embodiment: After the acid solution is replaced, the mixed acid in the cleaning solution under the new process conditions is composed of a mixture of hydrofluoric acid and nitric acid. 100 kg of UPS-grade hydrofluoric acid with a content of 48.8%-49.2% and 360 kg of UPS-grade nitric acid with a content of 69%-71% are added to the acid solution tank to form an aqueous solution. The minimum etching thickness required by the process is 0.008 mm. After the polycrystalline silicon rod is crushed, the size of the product silicon block is 6-25 mm. Therefore, a 15 mm side length standard processing cube sample is selected accordingly. The sample is made according to step S1, and the pre-cleaning mass M1 of each sample is marked and recorded. The obtained sample is loaded into the cleaning agent together with the crushed silicon block according to the method shown in step S2. Cleaning and etching are carried out in the cradle, and the total mass of each batch of cleaned silicon blocks and sample blocks is 30kg. After obtaining the product, the sample blocks are taken out according to the method of step S3 to measure the mass M2 of the sample blocks after cleaning, and the etching depth of this batch is calculated, and then the next batch of silicon blocks are cleaned, and so on, until 95% of the etching thickness of the 51st batch is 0.00799mm, which is less than the minimum etching thickness of 0.008mm required by the process, indicating that the etching ability of the cleaning solution after the 51st batch of cleaning is 0, and the cleaning is stopped and the acid solution is replaced; the etching thickness of the silicon blocks cleaned in all batches is recorded to obtain Table 1. In Table 1, for the convenience of reading, the unit of the etching thickness of the silicon blocks is converted, and mm is converted into μm for listing.

[0036] Table 1

[0037]

[0038] After the cleaning liquid is replaced, the mixed acid etching capacity of the cleaning liquid after the subsequent replacement of the cleaning liquid is estimated according to the data list obtained in step S4; in the subsequent production process, according to the method of step S5, the 41st batch and the 45th batch need to repeat the method of steps S1-S3 to measure the etching thickness H of the silicon block, and verify whether 95% of the etching thickness values ​​are lower than the minimum etching thickness of 0.008 mm required by the process; when cleaning to the 49th batch, the 50th batch and the 51st batch, the etching thickness of the silicon block is measured according to the method of steps S1-S3 for each batch, and it is verified whether 95% of the etching thickness values ​​are lower than the minimum etching thickness of 0.008 mm required by the process. When any of the above batches measures that 95% of its etching thickness is lower than 0.008 mm, the acid replacement operation of replacing the cleaning liquid can be performed.

[0039] Comparative example: The same cleaning process conditions as those in the embodiment are adopted, the total amount of mixed acid in the cleaning solution and the mixing ratio are the same as those in the embodiment, the process requires a minimum etching thickness of 0.008 mm, and silicon blocks are crushed from polycrystalline silicon rods produced by the same formula as in the embodiment. The size of the silicon blocks is 6-25 mm, and the total mass of silicon blocks cleaned in each batch is 30 kg. The estimated cleaning batch = total amount of cleaning solution / amount of cleaning solution consumed for each cleaning of the silicon blocks, resulting in an estimated cleaning amount of 55 batches. In order to avoid the influence of other factors that cause the cleaning and etching thickness of the last 20% batches of silicon blocks to be lower than the minimum etching thickness required by the process, the newly replaced cleaning solution can clean a total of 55 batches - (55 × 20%), so the newly replaced cleaning solution can clean a total of 44 batches of silicon blocks.

[0040] According to the comparison between the above embodiments and the comparative examples, 51 batches of silicon blocks can be cleaned by the method of the present invention, while at most 44 batches of silicon blocks can be cleaned by the method of the comparative example. The method of the present invention can maximize the utilization efficiency of the mixed acid solution and reduce the waste of the cleaning solution.

Claims

1. A method for determining whether to replace mixed acid with acid in a polysilicon cleaning solution, characterized in that: The following steps are involved: S1: Prepare the sample: Cut the polycrystalline bar into a number of cubic samples with equal side lengths. The side length of the sample is L, and the unit of the side length L of the sample is mm; S2: cleaning and etching: the sample block in step S1 and the silicon block to be cleaned are placed in the basket at the same time, and the sample block and the silicon block to be cleaned pass through each cleaning tank for cleaning and etching, and the sample block is taken out after cleaning; S3: Measure the etched thickness of the sample block: Measure the mass M1 before cleaning and the mass M2 after cleaning of the sample block in step S2, and calculate its etched thickness H: H = [(M2-M1) / ρ] / (L 2 ×6), where M1 and M2 are in g, and ρ is the density of the polysilicon material of the sample in g / mm 3 ; S4: Construct a data table: The mixed acid etching capacity of the cleaning solution of the first batch of cleaning samples is 100%; the mixed acid etching capacity of the cleaning solution of each subsequent batch of cleaning samples is calculated by the following method: The mixed acid etching capacity of the cleaning solution of the nth batch = [1-1 / (N-1) × (n-1)] × 100%, where N is the total number of all cleaning batches; The etching thickness of the sample block after the nth batch of cleaning is H n , when 0.95H n <H k When the mixed acid etching capacity of the cleaning solution after the nth batch of cleaning is 0, H k is the minimum etching thickness required by the process; construct a data list of the etching thickness H of all batches of cleaned samples and the mixed acid etching capacity of the corresponding cleaning solution; S5: Estimate the number of cleaning batches after the cleaning solution is replaced: After the cleaning solution is replaced, estimate the mixed acid etching capacity of the cleaning solution after the cleaning solution is replaced according to the data list obtained in step S4. When the etching capacity of the cleaning batch in the data list reaches 20%, the current cleaning batch and every 4 cleaning batches thereafter need to repeat steps S1-S3 to measure the etching thickness H of the sample block. When 0.95H<H k Replace the cleaning fluid.

2. A method for determining whether to replace acid with mixed acid in polysilicon cleaning solution according to claim 1, characterized in that: In step S5, when the estimated etching capacity reaches 5%, the current batch and each subsequent batch repeat the method of steps S1-S3 to measure the etching thickness H at this time. When 0.95H<H k Replace the cleaning fluid.

3. A method for determining whether to replace acid with mixed acid in polysilicon cleaning solution according to claim 2, characterized in that: Among them, H k It is 0.002-0.03mm.

4. A method for determining whether to replace acid with mixed acid in polysilicon cleaning solution according to claim 1, characterized in that: The side length L of the sample block in step S1 is the median of the size range of the cleaned polysilicon blocks.

5. A method for determining whether to replace acid with mixed acid in polysilicon cleaning solution according to claim 4, characterized in that: The surface Ra value of the sample block is less than 0.8 μm.

6. A method for determining whether to replace acid with mixed acid in polysilicon cleaning solution according to claim 4, characterized in that: The side length of the sample block is one of 4 mm, 15 mm, 38 mm, and 75 mm.

7. A method for determining acid replacement of polysilicon cleaning solution by mixed acid according to claim 1, characterized in that: In step 2, a sample block in step S1 is placed in the middle and at both ends of the diagonal line of the basket.

8. A method for determining whether to replace acid with mixed acid in polysilicon cleaning solution according to claim 7, characterized in that: The etching thickness H of the sample block in step S4 is n is the average value of the etching thickness H of the three sample blocks.

Citation Information

Cited By

  • Electronic-grade polycrystalline silicon surface metal detection method by scanning appearance

    CN121364235A

  • A method for detecting the surface metal of electronic-grade polysilicon with scanning profile

    CN121364235B