Semiconductor element with porous layer

By adopting porous dielectric layer structure and barrier layer design in semiconductor components, the problem of improved performance limits of parasitic capacitance is solved, and performance improvement and reliability enhancement are achieved.

CN118899298APending Publication Date: 2024-11-05NAN YA TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410291542.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-03
Filing Date
2023-08-18
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the process of shrinking semiconductor components, there are challenges in improving performance, quality, yield and reliability, especially due to the presence of parasitic capacitors that lead to limited performance improvement.

Method used

A semiconductor element is designed with a porous dielectric layer structure, including the bottom, top and intermediate porous dielectric layers, and a porous layer structure with low dielectric constant is formed by energy processing to reduce parasitic capacitance and prevent porous through the barrier layer. Degassing the layer to improve reliability.

Benefits of technology

The parasitic capacitance of semiconductor components is effectively reduced, the performance is improved, and the degassing problem is prevented through the barrier layer, enhancing the reliability of the components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899298A_ABST
    Figure CN118899298A_ABST
Patent Text Reader

Abstract

The invention relates to a semiconductor element and a preparation method thereof. The semiconductor device includes a substrate including a mixed region and a non-mixed region; a bottom porous dielectric layer disposed on the substrate; a top porous dielectric layer disposed on the bottom porous dielectric layer; the middle porous dielectric layer is arranged above the mixing area, and is arranged between the bottom porous dielectric layer and the top porous dielectric layer; a mixed region conductive structure disposed along the top porous dielectric layer, the intermediate porous dielectric layer and the bottom porous dielectric layer and disposed on the mixed region of the substrate; and a non-mixing region conductive structure disposed along the top porous dielectric layer and the bottom porous dielectric layer and disposed on the non-mixing region of the substrate. The porosity of the top porous dielectric layer is greater than the porosity of the intermediate porous dielectric layer. The porosity of the middle porous dielectric layer is greater than that of the bottom porous dielectric layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of Chinese invention patent application No. 2023110471024, filed on August 18, 2023, with the invention name of “Semiconductor element with porous layer”. Application No. 2023110471024 claims priority and benefits of U.S. formal application No. 18 / 142,672 filed on May 3, 2023. The contents of the U.S. formal application are incorporated herein by reference in their entirety. Technical Field

[0002] The present disclosure relates to a semiconductor element, and more particularly to a semiconductor element having a porous layer. Background Art

[0003] Semiconductor components are used in a variety of electronic applications, such as personal computers, mobile phones, digital cameras, and other electronic devices. To meet the growing demand for computing power, the size of semiconductor components continues to shrink. However, various problems arise during the shrinking process, and these problems are increasing. Therefore, there are still challenges in improving the performance, quality, yield, efficiency, and reliability of semiconductor components.

[0004] The above “prior art” description is only to provide background technology, and does not admit that the above “prior art” description reveals the subject matter of the present disclosure, does not constitute the prior art of the present disclosure, and any description of the above “prior art” should not be regarded as any part of this case. Summary of the invention

[0005] One aspect of the present disclosure provides a semiconductor device, which includes a substrate, which includes a mixed region and a non-mixed region; a bottom porous dielectric layer, which is disposed on the substrate; a top porous dielectric layer, which is disposed on the bottom porous dielectric layer; an intermediate porous dielectric layer, which is disposed above the mixed region and disposed between the bottom porous dielectric layer and the top porous dielectric layer; a mixed region conductive structure, which is disposed along the top porous dielectric layer, the intermediate porous dielectric layer and the bottom porous dielectric layer, and disposed on the mixed region of the substrate; a non-mixed region conductive structure, which is disposed along the top porous dielectric layer and the bottom porous dielectric layer, and disposed on the non-mixed region of the substrate. The porosity of the top porous dielectric layer is greater than the porosity of the intermediate porous dielectric layer. The porosity of the intermediate porous dielectric layer is greater than the porosity of the bottom porous dielectric layer.

[0006] Due to the design of the semiconductor device disclosed in the present invention, the top porous dielectric layer, the middle porous dielectric layer and the bottom porous dielectric layer have low dielectric constants, so the parasitic capacitance of the semiconductor device can be reduced by using the bottom porous dielectric layer, the top porous dielectric layer and the middle porous dielectric layer. As a result, the performance of the semiconductor device will be improved.

[0007] The above has outlined the technical features and advantages of the present disclosure in a fairly broad manner, so that the detailed description of the present disclosure below can be better understood. Other technical features and advantages that constitute the subject matter of the claims of the present disclosure will be described below. It should be understood by those with ordinary knowledge in the technical field to which the present disclosure belongs that the concepts and specific embodiments disclosed below can be used to modify or design other structures or processes to achieve the same purpose as the present disclosure. It should also be understood by those with ordinary knowledge in the technical field to which the present disclosure belongs that such equivalent constructions cannot depart from the spirit and scope of the present disclosure as defined by the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] A more complete understanding of the disclosure of the present application may be obtained by referring to the embodiments and claims in conjunction with the drawings, in which the same reference numerals refer to the same elements.

[0009] Figure 1 The flowchart illustrates a method for manufacturing a semiconductor device according to an embodiment of the present disclosure.

[0010] Figures 2 to 23 is a cross-sectional view illustrating a process of manufacturing a semiconductor device in one embodiment of the present disclosure.

[0011] Figures 24 to 26 2 is a cross-sectional view illustrating semiconductor devices according to other embodiments of the present disclosure.

[0012] The reference numerals are described as follows:

[0013] 1A: Semiconductor components

[0014] 1B: Semiconductor components

[0015] 1C: Semiconductor components

[0016] 1D: Semiconductor components

[0017] 101: Base

[0018] 103: First bottom conductive layer

[0019] 105: Second bottom conductive layer

[0020] 107: Bottom dielectric layer

[0021] 109: Top dielectric layer

[0022] 200: Non-mixed area conductive structure

[0023] 201: Non-mixed zone lining

[0024] 203: Non-mixed area conductive layer

[0025] 203H: Horizontal part

[0026] 203V: Vertical section

[0027] 205: Non-blended area hard mask layer

[0028] 300: Hybrid area conductive structure

[0029] 301: Mixing zone lining

[0030] 303: Mixed zone conductive layer

[0031] 303H: Horizontal part

[0032] 303V: Vertical section

[0033] 305: Blending Area Hard Mask Layer

[0034] 401: Bottom Energy Removable Layer

[0035] 403: Top Energy Removable Layer

[0036] 411: Bottom porous dielectric layer

[0037] 413: Top porous dielectric layer

[0038] 415: Intermediate porous dielectric layer

[0039] 421: Bottom barrier layer

[0040] 423: Top barrier layer

[0041] 501: Bottom barrier material

[0042] 503: Top barrier material

[0043] 505: First liner material

[0044] 507: Secondary liner material

[0045] 509: First conductive material

[0046] 511: Second conductive material

[0047] 601: First mask layer

[0048] 603: Second mask layer

[0049] 605: The third mask layer

[0050] 607: Fourth mask layer

[0051] MA: Mixed Zone

[0052] NMA: Non-Mixed Area

[0053] R1: Concave in non-mixed area

[0054] R2: Mixing zone concave

[0055] VL1: Vertical Level

[0056] VL2: Vertical Level

[0057] S11: Steps

[0058] S13: Steps

[0059] S15: Steps

[0060] S17: Steps

[0061] Z: Direction DETAILED DESCRIPTION

[0062] The following description of the present disclosure is accompanied by the drawings which are incorporated into and constitute a part of the specification, and illustrate embodiments of the present disclosure, but the present disclosure is not limited to the embodiments. In addition, the following embodiments can be appropriately integrated to complete another embodiment.

[0063] "One embodiment", "an embodiment", "an exemplary embodiment", "another embodiment", "another embodiment", etc. mean that the embodiment described in the present disclosure may include specific features, structures or characteristics, but not every embodiment must include the specific features, structures or characteristics. Furthermore, repeated use of the phrase "in an embodiment" does not necessarily refer to the same embodiment, but it can be the same embodiment.

[0064] In order to make the present disclosure fully understood, the following description provides detailed steps and structures. Obviously, the implementation of the present disclosure will not be limited to the specific details known to those skilled in the art. In addition, the known structures and steps are no longer described in detail to avoid unnecessarily limiting the present disclosure. The preferred embodiments of the present disclosure are described in detail below. However, in addition to the detailed description, the present disclosure can also be widely implemented in other embodiments. The scope of the present disclosure is not limited to the content of the detailed description, but is defined by the claims.

[0065] In the present disclosure, a semiconductor element generally refers to a device that can function by utilizing semiconductor characteristics, and electro-optical elements, light-emitting display elements, semiconductor circuits, and electronic components all fall into the category of semiconductor elements.

[0066] It should be noted that, in the description of the present disclosure, the upper side (or up) corresponds to the direction of the arrow in the Z direction, and the lower side (or down) corresponds to the opposite direction of the arrow in the Z direction.

[0067] It should be noted that, in the description of the present disclosure, the term "formation" refers to any method of creating, establishing, patterning, implanting or depositing an element, a dopant or a material, including, but not limited to, atomic layer deposition, chemical vapor deposition, physical vapor deposition, sputtering, co-sputtering, spin coating, diffusion, deposition, crystal growth, implantation, lithography, dry etching and wet etching.

[0068] It should be noted that in the description of the present disclosure, the functions or steps mentioned herein may appear in a different order than the order marked in the drawings. For example, depending on the functions or steps involved, two consecutively displayed diagrams may actually be executed substantially simultaneously or may sometimes be executed in the opposite order.

[0069] Figure 1 1 is a flow chart illustrating a method 10 for manufacturing a semiconductor device 1A according to an embodiment of the present disclosure. Figures 2 to 23 2 is a cross-sectional view illustrating a process of manufacturing a semiconductor device 1A in one embodiment of the present disclosure.

[0070] Reference Figures 1 to 4 In step S11, a substrate 101 is provided, which includes a non-mixed area NMA and a mixed area MA, a first bottom conductive layer 103 is formed in the mixed area MA, a second bottom conductive layer 105 is formed in the non-mixed area NMA, a bottom dielectric layer 107 is formed on the substrate 101, and a bottom energy removable layer 401 is formed on the bottom dielectric layer 107.

[0071] Reference Figure 2 In some embodiments, the mixing area MA and the non-mixing area NMA may be separated from each other. In some embodiments, the mixing area MA and the non-mixing area NMA are adjacent to each other.

[0072] It should be noted that the mixing area MA may include a portion of the substrate 101 and the space above the mixing area MA. Describing an element as being disposed on the mixing area MA means that the element is disposed on the top surface of the portion of the substrate 101. Describing an element as being disposed in the mixing area MA means that the element is disposed in the portion of the substrate 101; however, the top surface of the element may be flush with the top surface of the portion of the substrate 101. Describing an element as being disposed above the mixing area MA means that the element is disposed above the top surface of the portion of the substrate 101. Accordingly, the non-mixing area NMA may include another portion of the substrate 101 and the space above and below the other portion of the substrate 101.

[0073] Reference Figure 2The substrate 101 may include a bulk semiconductor substrate composed entirely of at least one semiconductor material, a plurality of device elements (not shown for clarity), a plurality of dielectric layers (not shown for clarity), and a plurality of conductive features (not shown for clarity). The bulk semiconductor substrate may be formed of elemental semiconductors such as silicon, germanium, compound semiconductors such as silicon germanium, silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, indium antimonide, or other III-V compound semiconductors or II-VI compound semiconductors, or a combination thereof.

[0074] In some embodiments, substrate 101 includes a semiconductor-on-insulator structure, which consists of a processing substrate, an insulator layer, and a topmost semiconductor material layer from bottom to top. The processing substrate and the topmost semiconductor material layer are formed of the same material as the bulk semiconductor substrate described above. The insulator layer is a crystalline or non-crystalline dielectric material, such as an oxide and / or a nitride. For example, the insulator layer can be a dielectric oxide, such as silicon oxide. For another example, the insulator layer can be a dielectric nitride, such as silicon nitride or boron nitride. For another example, the insulator layer includes a stack of dielectric oxides and dielectric nitrides, such as silicon oxide and silicon nitride or boron nitride stacked in any order. The insulator layer has a thickness between about 10 nm and about 200 nm.

[0075] It should be noted that in the description of the present disclosure, the term "approximately" changes the amount of the ingredients, components or reactants of the present disclosure, for example, by the typical measurement and liquid handling procedures used for preparation. Changes may also arise from unintentional errors in the measurement procedures, differences in the preparation, source or purity of the ingredients used in the preparation of the composition or implementation of the method. In one aspect, the term "approximately" refers to changes within 10% of the value shown. In other aspects, the term "approximately" refers to changes within 5% of the value shown. In other aspects, the term "approximately" refers to changes within 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, or 1% of the value shown.

[0076] A plurality of device elements may be formed on the substrate 101. Some portions of the device elements may be formed in the substrate 101. The device elements may be transistors, such as complementary metal oxide semiconductor transistors, metal oxide semiconductor field effect transistors, fin field effect transistors, etc., or combinations thereof.

[0077] The dielectric layer may be formed on the substrate 101 and cover the device elements. In some embodiments, the dielectric layer may be formed of, for example, silicon oxide, borophosphosilicate glass, undoped silicate glass, fluorinated silicate glass, low-k dielectric material, or the like, or a combination thereof. The low-k dielectric material has a dielectric constant less than 3.0 or even less than 2.5. In some embodiments, the low-k dielectric material may have a dielectric constant less than 2.0. The dielectric layer may be formed by a deposition process such as chemical vapor deposition, plasma enhanced chemical vapor deposition, or the like. A planarization process is performed after the deposition process to remove excess material and provide a substantially flat surface for subsequent processing steps.

[0078] Conductive features include interconnect layers, conductive vias, and conductive pads. The interconnect layers are separated from each other and are horizontally arranged in the dielectric layer along the Z direction. In the present embodiment, the topmost interconnect layer is regarded as a conductive pad. The conductive vias connect adjacent interconnect layers, adjacent device elements and interconnect layers, and adjacent conductive pads and interconnect layers along the Z direction. In some embodiments, the conductive vias can improve heat dissipation and can provide structural support. In some embodiments, the conductive features can be formed by, for example, tungsten, cobalt, zirconium, tantalum, titanium, aluminum, ruthenium, copper, metal carbides (e.g., tantalum carbide, titanium carbide, tantalum magnesium carbide), metals forming nitrides (e.g., titanium nitride), transition metal aluminides, or combinations thereof. The conductive features can be formed during the formation of the dielectric layer.

[0079] In some embodiments, the device elements and conductive features together constitute a plurality of functional units in the semiconductor device 1A. In the description of the present disclosure, a functional unit generally refers to a functionally related circuit that is divided into different units for functional purposes. In some embodiments, the functional units of the semiconductor device 1A may include, for example, highly complex circuits such as a processor core, a memory controller, an accelerator unit, or other applicable functional circuits.

[0080] Reference Figure 2, the first bottom conductive layer 103 may be formed in the mixed area MA. The second bottom conductive layer 105 may be formed in the non-mixed area NMA. In some embodiments, the first bottom conductive layer 103 and the second bottom conductive layer 105 may be regarded as part of the conductive features of the substrate 101. In some embodiments, the first bottom conductive layer 103 and the second bottom conductive layer 105 may be formed of, for example, tungsten, cobalt, zirconium, tantalum, titanium, aluminum, ruthenium, copper, metal carbides (e.g., tantalum carbide, titanium carbide, tantalum magnesium carbide), metal nitrides (e.g., titanium nitride), transition metal aluminides, or combinations thereof. In some embodiments, the width W1 of the first bottom conductive layer 103 and the width W2 of the second bottom conductive layer 105 are substantially the same. In some embodiments, the width W1 of the first bottom conductive layer 103 and the width W2 of the second bottom conductive layer 105 may be different. The top surfaces of the substrate 101, the first bottom conductive layer 103, and the second bottom conductive layer 105 are substantially coplanar.

[0081] Reference Figure 3 , a bottom dielectric layer 107 may be formed on the substrate 101 to cover the non-mixed area NMA and the mixed area MA. In some embodiments, the bottom dielectric layer 107 may be formed of a low-porosity dielectric material. For example, the porosity of the bottom dielectric layer 107 may be less than 5%, less than 4%, less than 3%, less than 2%, less than 1%, or may be 0%. In some embodiments, the bottom dielectric layer 107 may be formed of, for example, silicon oxide. In some embodiments, the bottom dielectric layer 107 may be formed by, for example, chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, or other applicable deposition processes.

[0082] Reference Figure 4 , forming a bottom energy removable layer 401 on the bottom dielectric layer 107. The bottom energy removable layer 401 can completely cover the non-mixed area NMA and the mixed area MA. In some embodiments, the bottom energy removable layer 401 includes a material that is a thermally decomposable material, a photon decomposable material, an electron beam decomposable material, or a combination thereof. For example, the bottom energy removable layer 401 may include a substrate material and a decomposable porogen material that is sacrificially removed when exposed to an energy source. The substrate material includes a material based on methylsilsesquioxane. The decomposable porogen material may include a porogen organic compound that provides porosity to the substrate material of the bottom energy removable layer 401.

[0083] In some embodiments, the bottom energy removable layer 401 may include about 55% of the decomposable porogen material and about 45% of the substrate material. In some embodiments, the bottom energy removable layer 401 may include about 45% of the decomposable porogen material and about 55% of the substrate material. In some embodiments, the bottom energy removable layer 401 may include about 35% of the decomposable porogen material and about 65% of the substrate material. In some embodiments, the bottom energy removable layer 401 may include about 25% of the decomposable porogen material and about 75% of the substrate material. In some embodiments, the bottom energy removable layer 401 may include about 15% of the decomposable porogen material and about 85% of the substrate material.

[0084] Reference Figure 1 and Figures 5 to 12 In step S13 , a non-mixed region conductive structure 200 is formed on the non-mixed region NMA of the substrate 101 .

[0085] Reference Figure 5 , a layer of a bottom barrier material 501 is formed on the bottom energy removable layer 401. The layer of the bottom barrier material 501 may completely cover the non-mixed area NMA and the mixed area MA. In some embodiments, the bottom barrier material 501 may be a material having an etching selectivity to the bottom energy removable layer 401. In some embodiments, the bottom barrier material 501 may be a material having an etching selectivity to aluminum, copper, or tungsten. In some embodiments, the bottom barrier material 501 may be, for example, silicon nitride, silicon oxynitride, silicon oxynitride, or a combination thereof. In some embodiments, the layer of the bottom barrier material 501 may be formed by, for example, atomic layer deposition, chemical vapor deposition, plasma enhanced chemical vapor deposition, or other applicable deposition processes.

[0086] It should be noted that in the description of the present disclosure, silicon oxynitride refers to a substance containing silicon, nitrogen and oxygen, wherein the proportion of oxygen is greater than the proportion of nitrogen. Silicon oxynitride refers to a substance containing silicon, oxygen and nitrogen, wherein the proportion of nitrogen is greater than the proportion of oxygen.

[0087] Reference Figure 5 , forming a first mask layer 601 on the layer of bottom barrier material 501. In some embodiments, the first mask layer 601 may be a photoresist layer and may include a pattern of the bottom barrier layer 421, which will be described later. The pattern of the first mask layer 601 may be formed by a lithography process. The unpatterned first mask layer 601 ( Figure 5 ) can be based on the mask ( Figure 5The process light (not shown) is exposed to process light (process light). The wavelength of the process light can be associated with the critical dimension of the pattern. In some embodiments, the process light can be deep ultraviolet (DUV). In some embodiments, the process light can be extreme ultraviolet (EUV), and the lithography process can be EUV lithography. After exposure to the process light, the pattern on the mask is converted to the unpatterned first mask layer 601. The unpatterned first mask layer 601 can then be etched according to the converted pattern, thereby forming a pattern on the first mask layer 601.

[0088] Reference Figure 6 , a first barrier etching process is performed using the first mask layer 601 as a mask to remove a portion of the bottom barrier material 501. In some embodiments, in the first barrier layer etching process, an etching rate ratio of the bottom barrier material 501 to the bottom energy removable layer 401 may be between about 100:1 and about 1.05:1, between about 15:1 and about 3:1, or between about 10::1 and about 5:1. After the first barrier etching process, the remaining bottom barrier material 501 may become a bottom barrier layer 421. The bottom barrier layer 421 may be formed over the non-mixed area NMA and on the bottom energy removable layer 401. In some embodiments, a width W3 of the bottom barrier layer 421 may be greater than a width W2 of the second bottom conductive layer 105. In some embodiments, a width W3 of the bottom barrier layer 421 may be substantially the same as a width W2 of the second bottom conductive layer 105. In some embodiments, the width W3 of the bottom barrier layer 421 may be smaller than the width W2 of the second bottom conductive layer 105. The first mask layer 601 may be removed after the bottom barrier layer 421 is formed.

[0089] Reference Figure 7 , a second mask layer 603 is formed on the bottom energy removable layer 401 and covers a portion of the bottom barrier layer 421. The second mask layer 603 may include a pattern of a non-mixed region concave R1, which will be described later. The pattern formation process of the second mask layer 603 is similar to that of the first mask layer 601, and will not be repeated here.

[0090] Reference Figure 8, a first recess etching process is performed to remove a portion of the bottom barrier layer 421, the bottom energy removable layer 401, and the bottom dielectric layer 107. In some embodiments, the first recess etching process can be a multi-stage etching process. For example, the first recess etching process can be a three-stage anisotropic dry etching process. The etching chemistry of each stage can be different to provide different etching selectivities. In some embodiments, during the first stage of the first recess etching process, the etching rate ratio of the bottom barrier layer 421 to the bottom energy removable layer 401 can be between about 100:1 and about 1.05:1, between about 15:1 and about 2:1, or between about 10:1 and about 2:1. In some embodiments, during the second stage of the first recess etching process, the etching rate ratio of the bottom energy removable layer 401 to the bottom dielectric layer 107 may be between about 100: 1 and about 1.05: 1, between about 15: 1 and about 2: 1, or between about 10: 1 and about 2: 1. In some embodiments, during the third stage of the first recess etching process, the etching rate ratio of the bottom dielectric layer 107 to the second bottom conductive layer 105 may be between about 100: 1 and about 1.05: 1, between about 15: 1 and about 2: 1, or between about 10: 1 and about 2: 1.

[0091] Reference Figure 8 , after the first recess etching process, a non-mixed region recess R1 may be formed along the bottom barrier layer 421, the bottom energy removable layer 401, and the bottom dielectric layer 107. The second bottom conductive layer 105 may be partially exposed through the non-mixed region recess R1. In some embodiments, a width W4 of the non-mixed region recess R1 may be smaller than a width W2 of the second bottom conductive layer 105 and a width W3 of the bottom barrier layer 421. After the non-mixed region recess R1 is formed, the second mask layer 603 will be removed.

[0092] Reference Fig. 9 , a layer of a first liner material 505 is conformally formed on the bottom energy removable layer 401, the bottom barrier layer 421, the non-mixed region recess R1, and the second bottom conductive layer 105. In some embodiments, the first liner material 505 may include, for example, titanium, titanium nitride, tantalum, tantalum nitride, or a combination thereof. In some embodiments, the first liner material 505 may be formed by, for example, chemical vapor deposition, atomic layer deposition, plasma enhanced chemical vapor deposition, or other applicable deposition processes.

[0093] For example, the layer of the first liner material 505 can be formed by chemical vapor deposition. In some embodiments, the formation of the layer of the first liner material 505 may include a source gas introducing step, a first purging step, a reactant flowing step, and a second purging step. The source gas introducing step, the first purging step, the reactant flowing step, and the second purging step can be regarded as a cycle. Multiple cycles can be performed to obtain the desired thickness of the layer of the first liner material 505.

[0094] In detail, Figure 8 The semiconductor component semi-finished product shown in can be loaded in the reaction chamber. In the source gas introduction step, the source gas containing the precursor and the reactant can be introduced into the reaction chamber containing the semiconductor component semi-finished product. The precursor and the reactant can diffuse through the boundary layer and reach the surface of the semiconductor component semi-finished product (that is, the surface of the bottom energy removable layer 401, the bottom barrier layer 421, the non-mixed area concave R1 and the second bottom conductive layer 105). The precursor and the reactant can be adsorbed on the above-mentioned surface and then migrate on the above-mentioned surface. The adsorbed precursor and the adsorbed reactant can react on the above-mentioned surface and form solid by-products. The solid by-products can form nuclei on the above-mentioned surface. The nucleus can grow into an island, and the island can merge into a continuous film on the above-mentioned surface. In the first purge step, a purge gas such as argon can be injected into the reaction chamber to purge out gaseous by-products, unreacted precursors and unreacted reactants.

[0095] In the reactant flow step, reactants may be introduced separately into the reaction chamber to turn a continuous film into a layer of first liner material 505. In the second purge step, a purge gas such as argon may be injected into the reaction chamber to purge out gaseous byproducts and unreacted reactants.

[0096] In some embodiments, forming the layer of first liner material 505 using chemical vapor deposition can be performed with the aid of plasma. The plasma source can be, for example, argon, hydrogen, or a combination thereof.

[0097] In some embodiments, the precursor may be titanium tetrachloride. The reactant may be ammonia. Due to the incomplete reaction between titanium tetrachloride and ammonia, titanium tetrachloride and ammonia may react on the surface and form a titanium nitride film containing high chloride contamination. The ammonia in the reactant flow step may reduce the chloride content of the titanium nitride film. After the ammonia treatment, the titanium nitride film may be considered as a layer of the first liner material 505.

[0098] For another example, the layer of the first liner material 505 can be formed by atomic layer deposition, such as light-assisted atomic layer deposition or liquid injection atomic layer deposition. In some embodiments, the formation of the layer of the first liner material 505 can include a first precursor introduction step, a first purge step, a second precursor introduction step, and a second purge step. The first precursor introduction step, the first purge step, the second precursor introduction step, and the second purge step can be regarded as one cycle. Multiple cycles can be performed to obtain the desired thickness of the layer of the first liner material 505.

[0099] In detail, Figure 8 The semiconductor element semi-finished product shown in can be loaded in the reaction chamber. In the first precursor introduction step, the first precursor can be introduced into the reaction chamber. The first precursor can diffuse through the boundary layer and reach the surface of the semiconductor element semi-finished product (i.e., the surface of the bottom energy removable layer 401, the bottom barrier layer 421, the non-mixed region concave R1 and the second bottom conductive layer 105). The first precursor can be adsorbed on the above-mentioned surface to form a monolayer at the single atomic level. In the first purge step, a purge gas such as argon can be injected into the reaction chamber to purge out the unreacted first precursor.

[0100] In the second precursor introduction step, the second precursor may be introduced into the reaction chamber. The second precursor may react with the monolayer and convert the monolayer into a layer of the first liner material 505. In the second purge step, a purge gas such as argon may be injected into the reaction chamber to purge out the unreacted second precursor and gaseous byproducts. Compared to chemical vapor deposition, since the first precursor and the second precursor are introduced separately, particle generation caused by gas phase reaction may be suppressed.

[0101] In some embodiments, the first precursor may be titanium tetrachloride. The second precursor may be ammonia. The adsorbed titanium tetrachloride may form a titanium nitride monolayer. The ammonia in the second precursor introduction step may react with the titanium nitride monolayer and convert the titanium nitride monolayer into a layer of the first liner material 505.

[0102] In some embodiments, the formation of the layer of first liner material 505 using atomic layer deposition can be performed with the help of plasma. The plasma source can be, for example, argon, hydrogen, oxygen, or a combination thereof. In some embodiments, the oxygen source can be, for example, water, oxygen, or ozone. In some embodiments, a co-reactant can be introduced into the reaction chamber. The co-reactant can be selected from hydrogen, hydrogen plasma, oxygen, air, water, ammonia, hydrazine, alkylhydrazine, borane, silane, ozone, and a combination thereof.

[0103] In some embodiments, the formation of the layer of the first liner material 505 can be performed using the following process conditions. The substrate temperature can be between about 160° C. and about 300° C. The evaporator temperature can be about 175° C. The pressure of the reaction chamber can be about 5 mbar. The solvent of the first precursor and the second precursor can be toluene.

[0104] Reference Fig.10 , a layer of a first conductive material 509 is formed on the layer of the first liner material 505 and completely fills the non-mixed region recess R1. In some embodiments, the first conductive material 509 includes aluminum, copper, tungsten, or a combination thereof. In some embodiments, the layer of the first conductive material 509 can be formed by, for example, physical vapor deposition, sputtering, electroplating, chemical plating, chemical vapor deposition, or other applicable deposition processes.

[0105] In some embodiments, a planarization process such as chemical mechanical polishing is performed on the layer of first conductive material 509 to provide a substantially planar surface for subsequent processing steps.

[0106] Reference Fig.11 , a non-mixed region hard mask layer 205 is formed on the layer of the first conductive material 509 and above the bottom barrier layer 421. In some embodiments, the width W5 of the non-mixed region hard mask layer 205 may be less than the width W3 of the bottom barrier layer 421. In some embodiments, the width W5 of the non-mixed region hard mask layer 205 may be greater than the width W2 of the second bottom conductive layer 105. In some embodiments, the width W5 of the non-mixed region hard mask layer 205 and the width W2 of the second bottom conductive layer 105 are substantially the same.

[0107] In some embodiments, the non-mixed region hard mask layer 205 may be formed of, for example, a material having an etching selectivity to the first conductive material 509, the first liner material 505, or the bottom barrier layer 421. In some embodiments, the non-mixed region hard mask layer 205 may be formed of, for example, silicon, silicon germanium, tetraethyl orthosilicate, silicon nitride, silicon oxynitride, silicon carbide, etc., or a combination thereof. In some embodiments, the non-mixed region hard mask layer 205 may be formed by a deposition process such as chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, etc. The process temperature for forming the non-mixed region hard mask layer 205 may be less than 400°C.

[0108] In some embodiments, the non-mixed region hard mask layer 205 may be formed of, for example, boron nitride, silicon boron nitride, phosphorus boron nitride, boron carbon silicon nitride, etc. In some embodiments, the non-mixed region hard mask layer 205 may be formed by a film formation process and a treatment process. In detail, in the film formation process, a first precursor may be introduced above the layer of the first conductive material 509 to form a boron-based layer, and the first precursor may be a boron-based precursor. Subsequently, in the treatment process, a second precursor may be introduced to react with the boron-based layer and turn the boron-based layer into the non-mixed region hard mask layer 205, and the second precursor may be a nitrogen-based precursor.

[0109] In some embodiments, the first precursor is an alkyl-substituted boron derivative such as diborane, borazine or borazine. In some embodiments, the second precursor can be introduced at a flow rate between about 5 sccm and about 50 slm or between about 10 sccm and about 1 slm. In some embodiments, the first precursor can be introduced by a diluent gas such as nitrogen, hydrogen, argon, or a combination thereof. The diluent gas can be introduced at a flow rate between about 5 sccm and about 50 slm or between about 1 slm and about 10 slm.

[0110] In some embodiments, the film forming process may be performed without plasma assistance. In this case, the substrate temperature of the film forming process is between about 100° C. and about 1000° C. For example, the substrate temperature of the film forming process may be between about 300° C. and about 500° C. The process pressure of the film forming process is between about 10 mTorr and about 760 Torr. For example, the process pressure of the film forming process may be between about 2 Torr and about 10 Torr.

[0111] In some embodiments, the film forming process may be performed in the presence of plasma. In this case, the substrate temperature of the film forming process may be between about 100°C and about 1000°C. For example, the substrate temperature of the film forming process may be between about 300°C and about 500°C. The process pressure of the film forming process may be between about 10mTorr and about 760Torr. For example, the process pressure of the film forming process may be between about 2Torr and about 10Torr. The plasma may be generated by an RF power between 2W and 5000W. For example, the RF power may be between 30W and 1000W.

[0112] In some embodiments, the second precursor can be, for example, ammonia or hydrazine. In some embodiments, the second precursor can be introduced at a flow rate between about 5 sccm and about 50 slm or between about 10 sccm and about 1 slm.

[0113] In some embodiments, oxygen-based precursors may be introduced during the process with the second precursor. The oxygen-based precursors may be, for example, oxygen, nitric oxide, nitrous oxide, carbon dioxide, or water.

[0114] In some embodiments, silicon-based precursors may be introduced during the process with the second precursor. The silicon-based precursors may be, for example, silane, trimethylsilylamine, trimethylsilane, or silazane (eg, hexamethylcyclotrisilazane).

[0115] In some embodiments, phosphorus-based precursors may be introduced during the process with the second precursor. The phosphorus-based precursor may be, for example, phosphine.

[0116] In some embodiments, an oxygen-based precursor, a silicon-based precursor, or a phosphorus-based precursor may be introduced during the process along with the second precursor.

[0117] In some embodiments, the treatment process may be performed with the assistance of a plasma process, a UV curing process, a thermal annealing process, or a combination thereof.

[0118] When the treatment is performed with the aid of a plasma process. The plasma of the plasma process may be generated by RF power. In some embodiments, the RF power may be between about 2 W and about 5000 W at a single low frequency between about 100 kHz and about 1 MHz. In some embodiments, the RF power may be between about 30 W and about 1000 W at a single high frequency greater than about 13.6 MHz. In this case, the substrate temperature of the treatment process may be between about 20° C. and about 1000° C. The process pressure of the treatment process may be between about 10 mTorr and about 760 Torr.

[0119] When the treatment is performed with the aid of a UV curing process, in this case, the substrate temperature of the treatment process can be between about 20°C and about 1000°C. The process pressure of the treatment process can be between about 10mTorr and about 760Torr. UV curing can be provided by any UV source, such as a mercury microwave arc lamp, a pulsed xenon flash lamp, or an array of high-efficiency UV light emitting diodes. The UV source can have a wavelength between about 170nm and about 400nm. The UV source can provide a photon energy between about 0.5eV and about 10eV or a photon energy between about 1eV and about 6eV. The assistance of the UV curing process can remove hydrogen from the non-mixed area hard mask layer 205. Since hydrogen may diffuse into other areas of the semiconductor element 1A and may reduce the reliability of the semiconductor element 1A, removing hydrogen with the assistance of the UV curing process can improve the reliability of the semiconductor element 1A. In addition, the UV curing process can increase the density of the non-mixed area hard mask layer 205.

[0120] When the treatment is performed with the assistance of a thermal annealing process, in this case, the substrate temperature of the treatment process may be between about 20° C. and about 1000° C. The process pressure of the treatment process may be between about 10 mTorr and about 760 Torr.

[0121] Reference Fig.12 , a first etching process can be performed using the non-mixed region hard mask layer 205 as a mask to remove a portion of the first conductive material 509 and the first liner material 505. In some embodiments, the first etching process can be a multi-stage etching process. For example, the first etching process can be a two-stage anisotropic dry etching process. The etching chemistry of each stage can be different to provide different etching selectivities. In some embodiments, during the first stage of the first etching process, the etching rate ratio of the first conductive material 509 to the non-mixed region hard mask layer 205 can be between about 100:1 and about 1.05:1, between about 15:1 and about 5:1, or between about 10:1 and about 3:1. In some embodiments, during the first stage of the first etching process, the etching rate ratio of the first conductive material 509 to the first liner material 505 can be between about 100:1 and about 1.05:1, between about 15:1 and about 5:1, or between about 10:1 and about 3:1.

[0122] In some embodiments, during the second stage of the first etching process, the etching rate ratio of the first liner material 505 to the non-mixed region hard mask layer 205 may be between about 100:1 and about 1.05:1, between about 15:1 and about 5:1, or between about 10:1 and about 3:1. In some embodiments, during the second stage of the first etching process, the etching rate ratio of the first liner material 505 to the bottom barrier layer 421 may be between about 100:1 and about 1.05:1, between about 15:1 and about 5:1, or between about 10:1 and 3:1. In some embodiments, during the second stage of the first etching process, the etching rate ratio of the first liner material 505 to the bottom energy removable layer 401 may be between about 100:1 and about 1.05:1, between about 15:1 and about 5:1, or between about 10:1 and about 3:1.

[0123] Reference Fig.12 , after the first etching process, the remaining first conductive material 509 can be regarded as the non-mixed region conductive layer 203. The remaining first liner material 505 can be regarded as the non-mixed region liner layer 201. The non-mixed region liner layer 201, the non-mixed region conductive layer 203 and the non-mixed region hard mask layer 205 together constitute the non-mixed region conductive structure 200. The non-mixed region conductive structure 200 can be formed on the second bottom conductive layer 105 and the non-mixed region NMA.

[0124] Reference Fig.12 , the non-mixed region conductive layer 203 includes a vertical portion 203V and a horizontal portion 203H. The vertical portion 203V is disposed on the second bottom conductive layer 105 and in the non-mixed region recess R1. The top of the vertical portion 203V may protrude from the top surface 401TS of the bottom energy removable layer 401 and may be surrounded by the bottom barrier layer 421. In other words, the top surface of the vertical portion 203V may be at a vertical level VL1 higher than the top surface 401TS of the bottom energy removable layer 401. The bottom of the vertical portion 203V may be surrounded by the bottom dielectric layer 107. In some embodiments, the width W6 of the vertical portion 203V may be less than the width W5 of the non-mixed region hard mask layer 205.

[0125] Reference Fig.12 , the horizontal portion 203H is disposed on the vertical portion 203V and the bottom barrier layer 421. In some embodiments, the horizontal portion 203H may have the same width W5 as the non-mixed region hard mask layer 205. In some embodiments, the width W5 of the horizontal portion 203H may be greater than the width W6 of the vertical portion 203V. That is, the non-mixed region conductive layer 203 may have a T-shaped cross-sectional profile. In some embodiments, the width W5 of the horizontal portion 203H may be less than the width W3 of the bottom barrier layer 421.

[0126] Reference Fig.12 , the non-mixed region liner layer 201 is conformally disposed between the non-mixed region conductive layer 203 and the bottom energy removable layer 401, between the non-mixed region conductive layer 203 and the bottom barrier layer 421, between the non-mixed region conductive layer 203 and the bottom dielectric layer 107, and between the non-mixed region conductive layer 203 and the second bottom conductive layer 105. In detail, the non-mixed region liner layer 201 is conformally disposed between the horizontal portion 203H and the bottom barrier layer 421, between the vertical portion 203V and the bottom barrier layer 421, between the vertical portion 203V and the bottom energy removable layer 401, between the vertical portion 203V and the bottom dielectric layer 107, and between the vertical portion 203V and the second bottom conductive layer 105. The non-mixed region liner layer 201 can improve the adhesion between the non-mixed region conductive layer 203 and the bottom barrier layer 421, the bottom energy removable layer 401, the bottom dielectric layer 107, and the second bottom conductive layer 105. The non-mixed region liner layer 201 may also prevent metal ions from diffusing from the non-mixed region conductive layer 203 to the bottom energy removable layer 401 or the substrate 101 .

[0127] Reference Figure 1 and Figures 13 to 21 In step S15 , a mixed region conductive structure 300 is formed on the mixed region MA of the substrate 101 .

[0128] Reference Fig.13 , forming a top energy removable layer 403 on the bottom energy removable layer 401 and covering the non-mixed region conductive structure 200 and the bottom barrier layer 421. The top energy removable layer 403 can completely cover the non-mixed region NMA and the mixed region MA. In some embodiments, the top energy removable layer 403 includes a material that is a thermally decomposable material, a photon decomposable material, an electron beam decomposable material, or a combination thereof. For example, the top energy removable layer 403 can include a substrate material and a decomposable porogen material that is sacrificially removed when exposed to an energy source. The substrate material includes a methyl silsesquioxane-based material. The decomposable porogen material can include a porogen organic compound that provides porosity to the substrate material of the top energy removable layer 403.

[0129] In some embodiments, the proportion of the substrate material of the top energy removable layer 403 is less than the proportion of the substrate material of the bottom energy removable layer 401. In some embodiments, the top energy removable layer 403 includes about 55% of the decomposable porogen material and about 45% of the substrate material. In some embodiments, the top energy removable layer 403 includes about 65% of the decomposable porogen material and about 35% of the substrate material. In some embodiments, the top energy removable layer 403 includes about 75% of the decomposable porogen material and about 25% of the substrate material. In some embodiments, the top energy removable layer 403 includes about 85% of the decomposable porogen material and about 15% of the substrate material.

[0130] In some embodiments, a planarization process such as chemical mechanical polishing may be performed to provide a substantially planar surface for subsequent processing steps.

[0131] Reference Fig.14 , forming a layer of top barrier material 503 on the top energy removable layer 403. The layer of top barrier material 503 may completely cover the non-mixed area NMA and the mixed area MA. In some embodiments, the top barrier material 503 may be a material having an etching selectivity to the top energy removable layer 403. In some embodiments, the top barrier material 503 may be a material having an etching selectivity to aluminum, copper, or tungsten. In some embodiments, the top barrier material 503 may be, for example, silicon nitride, silicon oxynitride, silicon oxynitride, or a combination thereof. In some embodiments, the layer of top barrier material 503 may be formed by, for example, atomic layer deposition, chemical vapor deposition, plasma enhanced chemical vapor deposition, or other applicable deposition processes.

[0132] Reference Fig.14 , forming a third mask layer 605 on the layer of top barrier material 503. In some embodiments, the third mask layer 605 may be a photoresist layer and may include a pattern of the top barrier layer 423, which will be described later. The pattern of the third mask layer 605 may be formed by a lithography process. The unpatterned third mask layer 605 ( Fig.14 ) can be based on the mask ( Fig.14 The process light (not shown) is exposed to process light. The wavelength of the process light can be associated with the critical dimension of the pattern. In some embodiments, the process light can be deep ultraviolet (DUV). In some embodiments, the process light can be extreme ultraviolet (EUV), and the lithography process can be EUV lithography. After the process light exposure, the pattern on the mask is converted to the unpatterned third mask layer 605. The unpatterned third mask layer 605 can then be etched according to the converted pattern, thereby forming a pattern on the third mask layer 605.

[0133] Reference Fig.15, a second barrier etching process is performed using the third mask layer 605 as a mask to remove a portion of the top barrier material 503. In some embodiments, in the second barrier layer etching process, an etching rate ratio of the top barrier material 503 to the top energy removable layer 403 may be between about 100:1 and about 1.05:1, between about 15:1 and about 3:1, or between about 10:1 and about 5:1. After the second barrier etching process, the remaining top barrier material 503 may become a top barrier layer 423. The top barrier layer 423 may be formed above the mixed region MA and on the top energy removable layer 403.

[0134] In some embodiments, the width W7 of the top barrier layer 423 may be greater than the width W1 of the first bottom conductive layer 103. In some embodiments, the width W7 of the top barrier layer 423 may be substantially the same as the width W1 of the first bottom conductive layer 103. In some embodiments, the width W7 of the top barrier layer 423 may be less than the width W1 of the first bottom conductive layer 103. In some embodiments, the width W7 of the top barrier layer 423 and the width W3 of the bottom barrier layer 421 may be substantially the same. In some embodiments, the width W7 of the top barrier layer 423 and the width W3 of the bottom barrier layer 421 may be different. The third mask layer 605 may be removed after the top barrier layer 423 is formed.

[0135] Reference Fig.16 , a fourth mask layer 607 is formed on the top energy removable layer 403 and covers a portion of the top barrier layer 423. The fourth mask layer 607 may include a pattern of a mixed region concave R2, which will be described later. The pattern formation process of the fourth mask layer 607 is similar to that of the third mask layer 605, and will not be repeated here.

[0136] Reference Fig.17 , a second recess etching process is performed to remove a portion of the top barrier layer 423, the top energy removable layer 403, the bottom energy removable layer 401, and the bottom dielectric layer 107. In some embodiments, the second recess etching process can be a multi-stage etching process. For example, the second recess etching process can be a three-stage anisotropic dry etching process. The etching chemistry of each stage can be different to provide different etching selectivities.

[0137] In some embodiments, during the first stage of the second recess etching process, the etching rate ratio of the top barrier layer 423 to the top energy removable layer 403 may be between about 100:1 and about 1.05:1, between about 15:1 and about 2:1, or between about 10:1 and about 2:1. In some embodiments, during the second stage of the second recess etching process, the etching rate ratio of the top energy removable layer 403 (and the bottom energy removable layer 401) to the bottom dielectric layer 107 may be between about 100:1 and about 1.05:1, between about 15:1 and about 2:1, or between about 10:1 and about 2:1. In some embodiments, during the third stage of the second recess etching process, the etching rate ratio of the bottom dielectric layer 107 to the first bottom conductive layer 103 may be between about 100:1 and about 1.05:1, between about 15:1 and about 2:1, or between about 10:1 and about 2:1.

[0138] Reference Fig.17 After the second recess etching process, a mixed region recess R2 may be formed along the top barrier layer 423, the top energy removable layer 403, the bottom energy removable layer 401, and the bottom dielectric layer 107. The first bottom conductive layer 103 may be partially exposed through the mixed region recess R2. In some embodiments, a width W8 of the mixed region recess R2 may be smaller than a width W1 of the first bottom conductive layer 103 and a width W7 of the top barrier layer 423. After the mixed region recess R2 is formed, the fourth mask layer 607 will be removed.

[0139] Reference Fig.18 , a layer of a second liner material 507 is conformally formed on the top energy removable layer 403, the top barrier layer 423, the mixed region recess R2, and the first bottom conductive layer 103. In some embodiments, the second liner material 507 may include, for example, titanium, titanium nitride, tantalum, tantalum nitride, or a combination thereof. In some embodiments, the second liner material 507 may be formed by, for example, chemical vapor deposition, atomic layer deposition, plasma enhanced chemical vapor deposition, or other applicable deposition processes.

[0140] In some embodiments, the second liner material 507 may be the same material as the first liner material 505. The formation of the layer of the second liner material 507 may be similar to Fig. 9 The formation of the layer of the first liner material 505 shown in FIG. 5 is not described in detail here.

[0141] Reference Fig.19, a layer of a second conductive material 511 is formed on the layer of the second liner material 507 and completely fills the inner recess R2 of the mixed region. In some embodiments, the second conductive material 511 may include aluminum, copper, tungsten, or a combination thereof. In some embodiments, the layer of the second conductive material 511 may be formed by, for example, physical vapor deposition, sputtering, electroplating, chemical plating, chemical vapor deposition, or other applicable deposition processes.

[0142] In some embodiments, a planarization process such as chemical mechanical polishing may be performed on the layer of second conductive material 511 to provide a substantially planar surface for subsequent processing steps.

[0143] Reference Fig. 20 , the hybrid region hard mask layer 305 may be formed on the layer of the second conductive material 511 and formed above the top barrier layer 423. In some embodiments, the width W9 of the hybrid region hard mask layer 305 may be less than the width W7 of the top barrier layer 423. In some embodiments, the width W9 of the hybrid region hard mask layer 305 may be greater than the width W1 of the first bottom conductive layer 103. In some embodiments, the width W9 of the hybrid region hard mask layer 305 and the width W1 of the first bottom conductive layer 103 may be substantially the same. In some embodiments, the width W9 of the hybrid region hard mask layer 305 and the width W5 of the non-hybrid region hard mask layer 205 may be substantially the same. In some embodiments, the width W9 of the hybrid region hard mask layer 305 and the width W5 of the non-hybrid region hard mask layer 205 may be different.

[0144] In some embodiments, the hybrid region hard mask layer 305 may be formed of, for example, a material having an etching selectivity to the second conductive material 511, the second liner material 507, and the top barrier layer 423. In some embodiments, the hybrid region hard mask layer 305 may be formed of, for example, silicon, silicon germanium, tetraethyl orthosilicate, silicon nitride, silicon oxynitride, silicon carbide, etc., or a combination thereof. In some embodiments, the hybrid region hard mask layer 305 may be formed of, for example, boron nitride, silicon boron nitride, phosphorus boron nitride, boron carbon silicon nitride, etc. The hybrid region hard mask layer 305 may be formed of, for example, a material similar to Fig.11 The process of forming the non-mixed area hard mask layer 205 is shown and will not be described again here.

[0145] Reference Fig.21, a second etching process is performed using the mixed region hard mask layer 305 as a mask to remove a portion of the second conductive material 511 and the second liner material 507. In some embodiments, the second etching process may be a multi-stage etching process. For example, the second etching process may be a two-stage anisotropic dry etching process. The etching chemistry of each stage may be different to provide different etching selectivities. In some embodiments, during the first stage of the second etching process, the etching rate ratio of the second conductive material 511 to the mixed region hard mask layer 305 may be between about 100:1 and about 1.05:1, between about 15:1 and about 5:1, or between 10:1 and about 3:1. In some embodiments, during the first stage of the second etching process, the etching rate ratio of the second conductive material 511 to the second liner material 507 may be between about 100:1 and about 1.05:1, between about 15:1 and about 5:1, or between about 10:1 and about 3:1.

[0146] In some embodiments, during the second stage of the second etching process, the etch rate ratio of the second liner material 507 to the mixed region hard mask layer 305 may be between about 100:1 and about 1.05:1, between about 15:1 and about 5:1, or between about 10:1 and about 3:1. In some embodiments, during the second stage of the second etching process, the etch rate ratio of the second liner material 507 to the top barrier layer 423 may be between about 100:1 and about 1.05:1, between about 15:1 and about 5:1, or between about 10:1 and about 3:1. In some embodiments, during the second stage of the second etching process, the etch rate ratio of the second liner material 507 to the top energy removable layer 403 may be between about 100:1 and about 1.05:1, between about 15:1 and about 5:1, or between about 10:1 and about 3:1.

[0147] Reference Fig.21 After the second etching process, the remaining second conductive material 511 can be regarded as the hybrid region conductive layer 303. The remaining second liner material 507 can be regarded as the hybrid region liner layer 301. The hybrid region liner layer 301, the hybrid region conductive layer 303 and the hybrid region hard mask layer 305 together constitute the hybrid region conductive structure 300. The hybrid region conductive structure 300 can be formed on the first bottom conductive layer 103 and on the hybrid region MA.

[0148] Reference Fig.21, the hybrid region conductive layer 303 may include a vertical portion 303V and a horizontal portion 303H. The vertical portion 303V may be disposed on the first bottom conductive layer 103 and in the hybrid region recess R2. The top of the vertical portion 303V may protrude from the top surface 403TS of the top energy removable layer 403 and may be surrounded by the top barrier layer 423. In other words, the top surface of the vertical portion 303V may be at a vertical level VL2 higher than the top surface 403TS of the top energy removable layer 403. The bottom of the vertical portion 303V may be surrounded by the bottom dielectric layer 107. In some embodiments, the width W10 of the vertical portion 303V may be less than the width W9 of the hybrid region hard mask layer 305. In some embodiments, the width W10 of the vertical portion 303V and the width W6 of the vertical portion 203V may be substantially the same. In some embodiments, the width W10 of the vertical portion 303V and the width W6 of the vertical portion 203V may be different.

[0149] Reference Fig.21 , the horizontal portion 303H may be disposed on the vertical portion 303V and the top barrier layer 423. In some embodiments, the horizontal portion 303H may have the same width W9 as the hybrid region hard mask layer 305. In some embodiments, the width W9 of the horizontal portion 303H may be greater than the width W10 of the vertical portion 303V. That is, the hybrid region conductive layer 303 may have a T-shaped cross-sectional profile. In some embodiments, the width W9 of the horizontal portion 303H may be less than the width W7 of the top barrier layer 423. In some embodiments, the width W9 of the horizontal portion 303H and the width W5 of the horizontal portion 203H may be substantially the same. In some embodiments, the width W9 of the horizontal portion 303H and the width W5 of the horizontal portion 203H may be different.

[0150] Reference Fig.21 The mixed zone liner layer 301 is conformally disposed between the mixed zone conductive layer 303 and the bottom energy removable layer 401, between the mixed zone conductive layer 303 and the top energy removable layer 403, between the mixed zone conductive layer 303 and the top barrier layer 423, between the mixed zone conductive layer 303 and the bottom dielectric layer 107, and between the mixed zone conductive layer 303 and the first bottom conductive layer 103.

[0151] In detail, the mixed region liner layer 301 is conformally disposed between the horizontal portion 303H and the top barrier layer 423, between the vertical portion 303V and the top barrier layer 423, between the vertical portion 303V and the top energy removable layer 403, between the vertical portion 303V and the bottom energy removable layer 401, between the vertical portion 303V and the bottom dielectric layer 107, and between the vertical portion 303V and the first bottom conductive layer 103. The mixed region liner layer 301 may improve adhesion between the mixed region conductive layer 303 and the top barrier layer 423, the top energy removable layer 403, the bottom energy removable layer 401, the bottom dielectric layer 107, and the first bottom conductive layer 103. The mixed region liner layer 301 may also prevent metal ions from diffusing from the mixed region conductive layer 303 to the bottom energy removable layer 401, the top energy removable layer 403, or the substrate 101.

[0152] Reference Figure 1 , Fig. 22 and Fig.23 In step S17, an energy treatment is performed to transform the bottom energy removable layer 401 into a bottom porous dielectric layer 411, and the top energy removable layer 403 into a top porous dielectric layer 413, and to form an intermediate porous dielectric layer 415 above the mixed area MA of the substrate 101 and between the bottom porous dielectric layer 411 and the top porous dielectric layer 413, and to form a top dielectric layer 109 on the top porous dielectric layer 413.

[0153] Reference Fig. 22 , can be Fig.21 The semi-finished semiconductor device in the embodiment of the present invention is subjected to energy treatment by applying an energy source thereto. The energy source may include heat, light, or a combination thereof. When heat is used as the energy source, the temperature of the energy treatment may be between about 800° C. and about 900° C. When light is used as the energy source, ultraviolet light may be used. The energy treatment may remove the decomposable porogen material from the bottom energy removable layer 401 and the top energy removable layer 403 to produce empty spaces (pores), while the substrate material remains in place. The empty space may be filled with air so that the dielectric constant of the layer containing the empty space may be very low.

[0154] After the energy treatment, the bottom energy removable layer 401 may become a bottom porous dielectric layer 411. The bottom porous dielectric layer 411 may be disposed on the bottom dielectric layer 107 and located above the non-mixing area NMA and the mixing area MA of the substrate 101. The top energy removable layer 403 may become a top porous dielectric layer 413. The top porous dielectric layer 413 may be disposed on the bottom porous dielectric layer 411 and located above the non-mixing area NMA and the mixing area MA of the substrate 101. In some embodiments, the porosity of the top porous dielectric layer 413 may be greater than the porosity of the bottom porous dielectric layer 411.

[0155] In some embodiments, above the mixing zone MA, since there is no barrier layer between the bottom energy removable layer 401 and the top energy removable layer 403, the bottom energy removable layer 401 and the top energy removable layer 403 may be mixed at the interface between the bottom energy removable layer 401 and the top energy removable layer 403. As a result, after the energy treatment, the intermediate porous dielectric layer 415 may be formed between the bottom porous dielectric layer 411 and the top porous dielectric layer 413 and only above the mixing zone MA. In some embodiments, the porosity of the intermediate porous dielectric layer 415 may be less than the porosity of the top porous dielectric layer 413 and may be greater than the porosity of the bottom porous dielectric layer 411. In some embodiments, the interface between the top porous dielectric layer 413 and the intermediate porous dielectric layer 415 may be fuzzy. In some embodiments, the interface between the intermediate porous dielectric layer 415 and the bottom porous dielectric layer 411 may be fuzzy.

[0156] In some embodiments, the porosity of the middle porous dielectric layer 415 may gradually decrease along the Z direction toward the substrate 101. In some embodiments, the porosity of the bottom dielectric layer 107 may be less than the porosity of the bottom porous dielectric layer 411, the porosity of the middle porous dielectric layer 415, or the porosity of the top porous dielectric layer 413.

[0157] Reference Fig.23 , a top dielectric layer 109 may be formed on the top porous dielectric layer 413 and cover the hybrid region conductive structure 300 and the top barrier layer 423. In some embodiments, the top dielectric layer 109 may be formed of, for example, silicon oxide, borophosphosilicate glass, undoped silicate glass, fluorinated silicate glass, a low dielectric constant dielectric material such as a spin-on low dielectric constant (low-k) dielectric layer or a chemical vapor deposited low dielectric constant dielectric layer, or a combination thereof. The term "low dielectric constant" as used in the present disclosure refers to a dielectric material having a dielectric constant less than that of silicon dioxide. In some embodiments, the top dielectric layer 109 may include a self-planarizing material such as spin-on glass or a self-planarizing material such as SiLK TM The use of a self-planarizing dielectric material can avoid the need to perform a subsequent planarization step. In some embodiments, the top dielectric layer 109 can be formed by a deposition process including, for example, chemical vapor deposition, plasma enhanced chemical vapor deposition, evaporation, or spin coating.

[0158] By using the bottom porous dielectric layer 411, the top porous dielectric layer 413, and the middle porous dielectric layer 415 having a low dielectric constant, the parasitic capacitance of the semiconductor element 1A can be reduced. As a result, the performance of the semiconductor element 1A will be improved. Furthermore, the bottom barrier layer 421 or the top barrier layer 423 can prevent the outgassing problem of the porous layer (i.e., the bottom porous dielectric layer 411, the top porous dielectric layer 413, and the middle porous dielectric layer 415) to avoid damage to the conductive structure (i.e., the mixed region conductive structure 300 and the non-mixed region conductive structure 200) and improve the reliability of the semiconductor element 1A. In addition, the bottom barrier layer 421 and the top barrier layer 423 can also serve as an etching stop layer in the process of forming the conductive structure to prevent the bottom energy removable layer 401 and the top energy removable layer 403 from being damaged in the process of forming the conductive structure.

[0159] Figures 24 to 26 2 are cross-sectional views illustrating semiconductor devices 1B, 1C, and 1D according to other embodiments of the present disclosure.

[0160] Reference Figure 24 to Figure 26 , semiconductor elements 1B, 1C and 1D have Fig.23 A structure similar to the one shown in Figure 24 to Figure 26 Zhongyu Fig.23 The same or similar elements are marked with like reference numerals, and repeated description is omitted.

[0161] Reference Fig.24 In the semiconductor element 1B, the bottom barrier layer 421 may be disposed between the bottom porous dielectric layer 411 and the top porous dielectric layer 413 , and may completely isolate the bottom porous dielectric layer 411 and the top porous dielectric layer 413 above the non-mixed area NMA of the substrate 101 .

[0162] Reference Fig.25 In the semiconductor device 1C, the top barrier layer 423 can completely isolate the top dielectric layer 109 and the top porous dielectric layer 413 above the non-mixed area NMA and the mixed area MA of the substrate 101. That is, the top barrier layer 423 can be regarded as a capping layer or a sealing layer of the top barrier layer 423.

[0163] Reference Fig.26 In the semiconductor device 1D, the bottom barrier layer 421 may be disposed between the bottom porous dielectric layer 411 and the top porous dielectric layer 413, and may completely isolate the bottom porous dielectric layer 411 and the top porous dielectric layer 413 above the non-mixed area NMA of the substrate 101. The top barrier layer 423 may completely isolate the top dielectric layer 109 and the top porous dielectric layer 413 above the non-mixed area NMA and the mixed area MA of the substrate 101.

[0164] One aspect of the present disclosure provides a semiconductor device, which includes a substrate, which includes a mixed region and a non-mixed region; a bottom porous dielectric layer, which is disposed on the substrate; a top porous dielectric layer, which is disposed on the bottom porous dielectric layer; an intermediate porous dielectric layer, which is disposed above the mixed region and disposed between the bottom porous dielectric layer and the top porous dielectric layer; a mixed region conductive structure, which is disposed along the top porous dielectric layer, the intermediate porous dielectric layer and the bottom porous dielectric layer, and disposed on the mixed region of the substrate; a non-mixed region conductive structure, which is disposed along the top porous dielectric layer and the bottom porous dielectric layer, and disposed on the non-mixed region of the substrate. The porosity of the top porous dielectric layer is greater than the porosity of the intermediate porous dielectric layer. The porosity of the intermediate porous dielectric layer is greater than the porosity of the bottom porous dielectric layer.

[0165] Due to the design of the semiconductor element of the present disclosure, the parasitic capacitance of the semiconductor element 1A can be reduced by adopting the bottom porous dielectric layer 411, the top porous dielectric layer 413 and the middle porous dielectric layer 415 having a low dielectric constant. As a result, the performance of the semiconductor element 1A will be improved. Furthermore, the bottom barrier layer 421 or the top barrier layer 423 can prevent the outgassing problem of the porous layer (i.e., the bottom porous dielectric layer 411, the top porous dielectric layer 413 and the middle porous dielectric layer 415) to avoid damage to the conductive structure (i.e., the mixed region conductive structure 300 and the non-mixed region conductive structure 200) and improve the reliability of the semiconductor element 1A. In addition, the bottom barrier layer 421 and the top barrier layer 423 can also serve as an etching stop layer in the process of forming the conductive structure to prevent the bottom energy removable layer 401 and the top energy removable layer 403 from being damaged in the process of forming the conductive structure.

[0166] Although the present disclosure and its advantages have been described in detail, it should be understood that various changes, substitutions and replacements may be made without departing from the spirit and scope of the present disclosure as defined in the claims. For example, many of the above processes may be implemented in different ways, and other processes or combinations thereof may be used to replace many of the above processes.

[0167] Furthermore, the scope of the present application is not limited to the specific embodiments of the processes, machines, manufactures, compositions of matter, means, methods, and steps described in the specification. A person skilled in the art can understand from the disclosure of the present disclosure that existing or future developed processes, machines, manufactures, compositions of matter, means, methods, or steps that have the same functions or achieve substantially the same results as the corresponding embodiments described herein can be used according to the present disclosure. Accordingly, such processes, machines, manufactures, compositions of matter, means, methods, or steps are included in the claims of the present application.

Claims

1. A semiconductor element, comprising: A substrate including a mixed region and a non-mixed region; a bottom porous dielectric layer disposed on the substrate; a top porous dielectric layer disposed on the bottom porous dielectric layer; a middle porous dielectric layer disposed above the mixed region and between the bottom porous dielectric layer and the top porous dielectric layer; a mixed region conductive structure disposed along the top porous dielectric layer, the middle porous dielectric layer, and the bottom porous dielectric layer, and disposed on the mixed region of the substrate; and a non-mixed region conductive structure disposed along the top porous dielectric layer and the bottom porous dielectric layer and disposed on the non-mixed region of the substrate, wherein the porosity of the top porous dielectric layer is greater than the porosity of the middle porous dielectric layer, The porosity of the middle porous dielectric layer is greater than the porosity of the bottom porous dielectric layer.

2. The semiconductor device as claimed in claim 1, wherein the mixed region conductive structure comprises a mixed region conductive layer, wherein the mixed region conductive layer comprises: a vertical portion disposed along the top porous dielectric layer, the middle porous dielectric layer, and the bottom porous dielectric layer and disposed on the mixed region of the substrate; as well as a horizontal portion disposed on the vertical portion and disposed on the top porous dielectric layer, The width of the horizontal portion is greater than the width of the vertical portion. 3 . The semiconductor device as claimed in claim 2 , wherein the mixed region conductive structure comprises a top barrier layer disposed between the horizontal portion of the mixed region conductive layer and the top porous dielectric layer.

4. The semiconductor device of claim 3 , wherein the mixed region conductive structure comprises a mixed region liner layer conformally disposed between the mixed region conductive layer and the top barrier layer, between the mixed region conductive layer and the top porous dielectric layer, between the mixed region conductive layer and the middle porous dielectric layer, between the mixed region conductive layer and the bottom porous dielectric layer, and between the mixed region conductive layer and the mixed region of the substrate. 5 . The semiconductor device as claimed in claim 4 , wherein the mixed region conductive structure comprises a mixed region hard mask layer disposed on the horizontal portion of the mixed region conductive layer. 6 . The semiconductor device as claimed in claim 5 , further comprising a top dielectric layer covering the mixed region hard mask layer, the horizontal portion of the mixed region conductive layer, the top barrier layer and the top porous dielectric layer. 7 . The semiconductor device as claimed in claim 6 , further comprising a bottom dielectric layer disposed between the substrate and the bottom porous dielectric layer. 8 . The semiconductor device as claimed in claim 7 , wherein a porosity of the bottom dielectric layer is smaller than a porosity of the bottom porous dielectric layer. 9 . The semiconductor device as claimed in claim 8 , wherein the mixed region hard mask layer comprises silicon nitride, silicon nitride oxide, silicon oxynitride, or a combination thereof. 10 . The semiconductor device as claimed in claim 8 , wherein the mixed region conductive layer comprises aluminum, copper, tungsten, or a combination thereof.

11. The semiconductor device of claim 8, wherein the mixed region liner layer comprises tantalum, tantalum nitride, titanium, titanium nitride, or a combination thereof.

12. The semiconductor device as claimed in claim 8, wherein the non-mixed region conductive structure comprises a non-mixed region conductive layer, wherein the non-mixed region conductive layer comprises: a vertical portion disposed along the bottom porous dielectric layer and the middle porous dielectric layer and disposed on the unmixed region of the substrate; and a horizontal portion disposed on the vertical portion and disposed on the bottom and top porous dielectric layers, The width of the horizontal portion is greater than the width of the vertical portion.

13. The semiconductor device according to claim 12, further comprising: A bottom barrier layer is disposed between the horizontal portion of the unmixed region conductive layer and the bottom porous dielectric layer, and is disposed on the top porous dielectric layer.

14. A semiconductor device as described in claim 13, wherein the mixed region conductive structure includes a non-mixed region liner layer, which is conformally arranged between the bottom barrier layer and the horizontal portion of the non-mixed region conductive layer, between the vertical portion of the non-mixed region conductive layer and the bottom barrier layer, between the vertical portion of the non-mixed region conductive layer and the bottom porous dielectric layer, between the vertical portion of the non-mixed region conductive layer and the bottom porous dielectric layer, and between the vertical portion of the non-mixed region conductive layer and the non-mixed region of the substrate. 15 . The semiconductor device as claimed in claim 14 , wherein the non-mixed region conductive structure comprises a non-mixed region hard mask layer disposed on the horizontal portion of the non-mixed region conductive layer.