Preparation method of proton-irradiation-resistant passive cooling silicon oxycarbide film
By preparing a proton-resistant carbon-nitride silicon oxide film on a copper indium gallium selenide solar cell, it uses its infrared strong emission characteristics to achieve passive cooling, and solves the increase in temperature and radiation damage of copper indium gallium selenide batteries in space environment. Problem, extends battery life and reduces production costs.
Patent Information
- Application Number
- CN202410999540.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-05
AI Technical Summary
The existing silicon solar cell cooling technology fails to effectively withstand proton radiation in the space environment, and lacks suitable low-cost, simple processes and lightweight infrared radiation cooling technology in the field of copper indium gallium selenide batteries, resulting in copper indium gallium selenide. The problem of short service life of solar cells in orbit.
A passive cooling carbon-nitride silicon oxide film preparation method that resists proton radiation, prepares a lifting solution by combining the organopolysiloxane precursor with di-n-butyl ether and magnetic stirring, coated with the impregnation puller and annealed at low temperature. The treatment is converted into a carbon-nitride silicon oxide film with a thickness of 1-10 microns, and the infrared strong emission of silicon-carbon bonds, silicon-nitrogen bonds and silicon-oxygen bonds can achieve passive cooling of the battery.
Effectively reduces the temperature of copper indium gallium selenide solar cells in the sun, delays the performance attenuation of high-energy proton irradiation, improves the orbital life of copper indium gallium selenide thin-film solar cells, and is simple in preparation process and low in cost, suitable for Mass production.
Smart Images

Figure CN118899366A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of spacecraft thermal control technology, and specifically relates to a method for preparing a proton irradiation-resistant, passively cooling carbon nitride silicon oxide film. Background Art
[0002] At present, with the development of large-area flexible deployment structures in the aerospace field, the application of lightweight, low-cost copper indium gallium selenide thin-film photovoltaic cells with good weak light performance in spacecraft is becoming more and more extensive. As an important source of power for spacecraft, photovoltaic cells are directly exposed to the space environment and convert solar energy into electricity for use by spacecraft, so they face extremely complex thermal and high-energy particle irradiation environments in space. Studies have shown that for every 1°C increase in the temperature of copper indium gallium selenide cells, the cell's photoelectric conversion efficiency decays by about 0.45%. When the copper indium gallium selenide cell is heated by solar radiation when in orbit facing the sun, the temperature of the copper indium gallium selenide cell can rise to 130-150°C, causing a sharp drop in photoelectric conversion efficiency; on the other hand, under the condition of high-energy particle irradiation in space, especially under proton irradiation, the copper indium gallium selenide layer produces irradiation defects and ionization damage and lattice reconstruction effect, causing the degradation of its photovoltaic efficiency, and the irradiation-induced degradation effect is particularly obvious when the cell is at a temperature of 130-150°C. It can be seen that keeping the copper indium gallium selenide cells at a low temperature in a sun-facing state and inhibiting damage from high-energy ion radiation in space are crucial to prolonging the on-orbit service life of the copper indium gallium selenide cells.
[0003] At present, there are several patent reports on cooling silicon solar cells, which can provide references for the development of related technologies. A series of patents such as CN202564421U, CN102544169B, and CN206281110U disclose adding auxiliary air cooling, liquid cooling, or heat pipe cooling systems to batteries to achieve cooling of silicon solar cells. On the other hand, passive cooling of solar cells by radiative cooling is a promising zero-energy technology. Its working principle is to cover the surface of the battery with a coating with high infrared emissivity to enhance the heat dissipation of silicon solar energy to achieve the ability of passive cooling of the battery. A series of patents such as CN112086522A and CN114843362A disclose technologies for sputtering multiple layers of thin films with different dielectric constants on the surface of silicon solar cells to enhance infrared radiation to achieve battery cooling; a series of patents such as CN115799372A and CN115572939A disclose technologies for constructing periodic microstructured thin films on the surface of silicon solar cells by means of chemical etching or mask evaporation to enhance infrared radiation to achieve silicon solar cell cooling.
[0004] Although the above patented technologies can achieve high infrared radiation cooling of silicon solar cells, they have disadvantages such as complex preparation process, high cost, and long preparation process. In addition, the related patented technologies have not been applied in the field of copper indium gallium selenide cells. Most importantly, the high infrared radiation coatings described in the related patents are designed for radiation cooling of silicon solar cells in the atmosphere. Whether the related films can effectively withstand high-energy particle irradiation in space has not been technically verified. That is, the technologies in the above patented technologies (1) are not designed for spacecraft solar cells, (2) and the films in the above patented technologies have not been tested for proton irradiation resistance, because proton irradiation resistance tests are only technically required for spacecraft, and (3) the technologies in the above patented technologies are only for silicon solar cells and have never been used for copper indium gallium selenide thin film solar cells. Therefore, in view of the development of the application of copper indium gallium selenide solar cells in my country's aerospace field, it is crucial to develop a low-cost, simple technical process, proton irradiation-resistant, lightweight infrared radiation cooling product and technology suitable for copper indium gallium selenide solar cells to promote the development of my country's aerospace industry. Summary of the invention
[0005] The purpose of the present invention is to construct a method for preparing a proton radiation-resistant, passively cooling carbon-nitride silicon oxide film, in order to provide my country with a preparation technology suitable for the cooling and protective layer required for spacecraft solar cells, and meet the actual application needs of long-term service of spacecraft solar cells; therefore, the present invention provides a method for preparing a proton radiation-resistant, passively cooling carbon-nitride silicon oxide film.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a proton irradiation-resistant, passively cooled carbon nitride silicon oxide film, characterized by comprising the following steps;
[0008] S1: Pretreatment of the sunny side of commercial copper indium gallium selenide film;
[0009] S2: Compounding an organopolysiloxane precursor with di-n-butyl ether in a mass ratio of 1:x, stirring the mixture for 1 hour under magnetic stirring to obtain an organopolysiloxane precursor impregnation and pulling solution;
[0010] S3: using the pulling solution prepared in S2 as the pulling solution, taking the sunny side of the copper indium gallium selenide film pretreated in S1 as the coating substrate, and using an immersion pulling liquid machine to prepare an organic polysiloxane precursor film with a thickness of 1-15 μm on the sunny side of the copper indium gallium selenide film;
[0011] S4: placing the copper indium gallium selenide thin film battery covered with the organic polysiloxane precursor film prepared in S3 under a certain atmosphere and annealing at a certain temperature for 3-5 hours to thermally decompose the organic polysiloxane precursor film into a carbon nitride silicon oxide film with a thickness of 1-10 microns.
[0012] Preferably, in S2, x=any value between 0.5 and 10.
[0013] Preferably, the atmosphere in S4 is one of air, oxygen, nitrogen, argon, hydrogen and a hydrogen-argon mixture.
[0014] Preferably, the annealing temperature in S4 is any temperature in the range of 80-150°C.
[0015] Preferably, the silicon oxycarbon nitride film is composed of silicon-carbon bonds, silicon-nitrogen bonds and silicon-oxygen bonds. The silicon oxycarbon nitride film is prepared by a chemical bond breaking and recombination process of an organic polysiloxane precursor film under heating conditions, and after removing some invalid impurities such as carbon dioxide and water vapor, the silicon oxycarbon nitride film is obtained. The silicon oxycarbon nitride film achieves zero-energy passive cooling of solar cell films through the strong emission of silicon-carbon bonds, silicon-nitrogen bonds and silicon-oxygen bonds in the structure in the infrared spectrum and the proton radiation resistance of this type of chemical bonds.
[0016] Preferably, after the backlight surface of the copper indium gallium selenide thin film battery is encapsulated and protected in S1, the sun-facing surface of the copper indium gallium selenide thin film battery is cleaned with methanol and acetone, and then placed on a laboratory-made battery film fixing bracket to ensure the flatness of the copper indium gallium selenide thin film battery. The sun-facing surface of the fixed copper indium gallium selenide thin film battery is then placed in an ultraviolet light cleaning machine at a power of 300 W for 10 minutes to obtain a clean surface.
[0017] Preferably, a proton irradiation-resistant, passive cooling functional carbon nitride silicon oxide film is prepared by the above method.
[0018] Preferably, a proton irradiation-resistant, passively cooling carbon nitride silicon oxide film is used in the preparation of copper indium gallium selenide thin-film solar cells for spacecraft with long service life.
[0019] Preferably, the technical features of the prepared silicon oxycarbon nitride film with the best performance are as follows:
[0020] (1) Appearance of silicon oxycarbon nitride film: transparent grayish white, evenly distributed;
[0021] (2) Silicon oxycarbon nitride film thickness: 3.2 μm;
[0022] (3) Solar spectrum transmittance of silicon oxycarbon nitride film> 0.92;
[0023] (4) The infrared radiation rate of the silicon oxycarbon nitride film is 0.72, and the cooling efficiency is 203.6W / m2 ;
[0024] (5) When facing the sun, the temperature on the back of the battery is 30°C lower than that on the side facing the sun;
[0025] (6) After simulating the proton irradiation dose of geosynchronous orbit for one year under 90keV proton irradiation conditions, the absorption rate of the solar spectrum band increased and the cooling efficiency decreased to 182.1W / m 2 ;
[0026] (7) Proton irradiation aging experiments show that the use of the carbon nitride silicon oxide film of the present invention can increase the life of the copper indium gallium selenide thin film solar cells in orbit by 35%-40%.
[0027] The present invention provides a method for preparing a proton irradiation-resistant, passively cooling carbon nitride silicon oxide film, which has the following beneficial effects:
[0028] The present invention: In order to solve the application problems that the photovoltaic efficiency of copper indium gallium selenide thin-film solar cells decreases due to the increase in temperature when serving in orbit, and the performance degradation of the cells caused by proton irradiation, the carbon nitride oxide silicon film with proton irradiation resistance and passive radiation cooling function described in the present invention can effectively reduce the temperature of the cells when facing the sun and delay the performance degradation of the cells under high-energy proton irradiation conditions, thereby improving the on-orbit life of copper indium gallium selenide thin-film solar cells; at the same time, the carbon nitride oxide silicon film of the present invention has a low thickness, that is, the effect of adding a coating on the surface of the cell on the overall quality of the photovoltaic module is low, so the thin-film cell processed by the patented technology has little effect on the spacecraft payload; finally, the preparation process of the carbon nitride oxide silicon layer described in the present invention is simple and low-cost, so it can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.
[0030] Figure 1 This is a real photo of a clean copper indium gallium selenide thin-film solar cell fixed on a bracket.
[0031] Figure 2 This is a real photo of a copper indium gallium selenide thin film solar cell loaded with carbon nitride silicon oxide film.
[0032] Figure 3 This is a cross-sectional scanning electron microscope image of a silicon carbon nitride oxide film.
[0033] Figure 4 This is the visible light reflectance spectrum of the copper indium gallium selenide thin-film solar cell before and after loading the carbon nitride silicon oxide film.
[0034] Figure 5 This is the infrared emission spectrum of a copper indium gallium selenide thin film solar cell covered with a 3.2 micron thick carbon nitride silicon oxide film.
[0035] Figure 6 This is the infrared emission spectrum of a copper indium gallium selenide thin film solar cell covered with a 1.1 micron thick carbon nitride silicon oxide film. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] 1. The embodiment of the present invention proposes a method for preparing a proton irradiation-resistant, passively cooled carbon nitride oxide silicon film, which comprises four basic process steps: preparation of a precursor solution, cleaning of a copper indium gallium selenide thin film solar cell, preparation of a precursor film by immersion and pulling, and preparation of a carbon nitride oxide silicon film by low temperature annealing of the precursor film.
[0038] 2. The carbon nitride silicon oxide film of the present invention has excellent resistance to proton radiation and passive cooling functions. The film is composed of silicon-carbon bonds, silicon-nitrogen bonds and silicon-oxygen bonds. The high physical and chemical stability of the three silicon-containing chemical bonds is the source of the film's resistance to proton radiation. At the same time, the strong characteristic infrared absorption of the three chemical bonds in the mid- and far-infrared is the source of the physical mechanism by which the film achieves cooling through high infrared radiation.
[0039] Based on the above technical solutions and principles, the present invention provides the following specific implementation cases 1 and 2.
[0040] Embodiment 1:
[0041] This embodiment provides a method for preparing a proton irradiation-resistant, passively cooled carbon nitride silicon oxide film, and the specific preparation method comprises the following steps:
[0042] S1, after encapsulating and protecting the backlight side of the copper indium gallium selenide thin film battery, clean the sun-facing side of the copper indium gallium selenide thin film battery with methanol and acetone, and place it on the battery film fixing bracket made in the laboratory to ensure the flatness of the copper indium gallium selenide thin film battery, and then place the fixed copper indium gallium selenide thin film battery on the sun-facing side in an ultraviolet light cleaning machine at 300W power for 10 minutes to obtain a clean surface; the actual photo of the clean copper indium gallium selenide thin film battery with the battery film fixed on the bracket is referenced Figure 1 As shown;
[0043] S2, an organopolysiloxane precursor (Durazane 1800) and di-n-butyl ether are compounded in a mass ratio of 1:1, and the mixture is stirred for 1 hour under magnetic stirring to obtain an organopolysiloxane precursor impregnation and pulling solution;
[0044] S3, using the pulling solution prepared in S2 as the pulling solution, taking the sunny side of the copper indium gallium selenide thin film battery pretreated in S1 as the coating substrate, and using an immersion pulling liquid machine to prepare a 4.8 micron thick organic polysiloxane precursor film on the sunny side of the copper indium gallium selenide film;
[0045] S4, placing the copper indium gallium selenide thin film battery covered with the organic polysiloxane precursor film prepared in S3 in air and annealing at 130° C. for 4 hours, thermally decomposing the organic polysiloxane precursor film to transform it into a carbon nitride silicon oxide film with a thickness of 3.2 microns, removing the copper indium gallium selenide thin film battery from the battery film fixing bracket, and removing the copper indium gallium selenide thin film battery backlight encapsulation layer, thereby realizing the preparation of a carbon nitride silicon oxide film with proton irradiation resistance and passive radiation cooling function on the surface of the copper indium gallium selenide thin film battery;
[0046] The test results of the silicon oxycarbon nitride film prepared in this embodiment are as follows:
[0047] Reference Figure 2 The appearance of silicon oxycarbon nitride film is: transparent grayish white and evenly distributed;
[0048] Reference Figure 3 , the thickness of silicon oxycarbon nitride film: 3.2μm;
[0049] Reference Figure 4 , the solar spectrum transmittance of carbon nitride oxide silicon film is greater than 0.92, and the carbon nitride oxide silicon film coating does not change the solar irradiation characteristics of copper indium gallium selenide thin film solar cells;
[0050] Reference Figure 5 The infrared radiation rate of the carbon nitride silicon oxide film is 0.72, and the cooling efficiency is 203.6W / m 2 , the temperature of the back of the battery in the sun-facing state is 30℃ lower than that of the sun-facing side;
[0051] After simulating a proton radiation dose of one year in space under 90keV proton irradiation conditions, the cooling efficiency dropped to 182.1W / m 2 .
[0052] Proton irradiation aging experiments show that the use of the carbon nitride silicon oxide film of the present invention can increase the life of the copper indium gallium selenide thin film solar cells in orbit by 35%-40%.
[0053] Embodiment 2:
[0054] This embodiment provides a method for preparing a proton irradiation-resistant, passively cooled carbon nitride silicon oxide film, and the specific preparation method comprises the following steps:
[0055] S1, after encapsulating and protecting the backlight side of the copper indium gallium selenide thin film battery, clean the sun-facing side of the copper indium gallium selenide thin film battery with methanol and acetone, and place it on a battery film fixing bracket made in the laboratory to ensure the flatness of the copper indium gallium selenide thin film battery, and then place the sun-facing side of the fixed copper indium gallium selenide thin film battery in an ultraviolet light cleaning machine at a power of 300W for 10 minutes to obtain a clean surface;
[0056] S2, an organopolysiloxane precursor (Durazane 1800) and di-n-butyl ether are compounded in a mass ratio of 1:4, and the mixture is stirred for 1 hour under magnetic stirring to obtain an organopolysiloxane precursor impregnation and pulling solution;
[0057] S3, using the pulling solution prepared in S2 as the pulling solution, taking the sunny side of the copper indium gallium selenide thin film battery pretreated in S1 as the coating substrate, and using an immersion pulling machine to prepare a 2.1 micron thick organic polysiloxane precursor film on the sunny side of the copper indium gallium selenide film;
[0058] S4, placing the copper indium gallium selenide thin film battery covered with the organic polysiloxane precursor film prepared in S3 in nitrogen and annealing at 120° C. for 4 hours, thermally decomposing the organic polysiloxane precursor film to transform it into a carbon nitride silicon oxide film with a thickness of 1.1 microns, removing the copper indium gallium selenide thin film battery from the battery film fixing bracket, and removing the copper indium gallium selenide thin film battery backlight encapsulation layer, thereby realizing the preparation of a carbon nitride silicon oxide film with proton irradiation resistance and passive radiation cooling function on the surface of the copper indium gallium selenide thin film battery;
[0059] The test results of the silicon oxycarbon nitride film prepared in this embodiment are as follows:
[0060] Appearance of silicon oxycarbon nitride film: transparent grayish white, evenly distributed;
[0061] Silicon oxycarbon nitride film thickness: 1.1μm;
[0062] Reference Figure 6 The infrared radiation rate of the carbon nitride silicon oxide film is 0.62, and the cooling efficiency is 162.2W / m 2 .
[0063] It should be understood that the embodiments of the present application are not limited to the precise structures described above and shown in the drawings, and various modifications and changes can be made without departing from the scope thereof. The scope of the embodiments of the present application is limited only by the appended claims.
[0064] The above-mentioned embodiments only express several implementation methods of the embodiments of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the embodiments of the present application, and these all belong to the protection scope of the embodiments of the present application.
Claims
1. A method for preparing a proton irradiation-resistant, passively cooled carbon nitride silicon oxide film, characterized in that: The steps include: S1: Pretreatment of the sunny side of commercial copper indium gallium selenide film; S2: Compounding an organopolysiloxane precursor with di-n-butyl ether in a mass ratio of 1:x, stirring the mixture for 1 hour under magnetic stirring to obtain an organopolysiloxane precursor impregnation and pulling solution; S3: using the pulling solution prepared in S2 as the pulling solution, taking the sunny side of the copper indium gallium selenide film pretreated in S1 as the coating substrate, and using an immersion pulling liquid machine to prepare an organic polysiloxane precursor film with a thickness of 1-15 μm on the sunny side of the copper indium gallium selenide film; S4: placing the copper indium gallium selenide thin film battery covered with the organic polysiloxane precursor film prepared in S3 under a certain atmosphere and annealing at a certain temperature for 3-5 hours to thermally decompose the organic polysiloxane precursor film into a carbon nitride silicon oxide film with a thickness of 1-10 microns.
2. The method for preparing a proton irradiation resistant, passive cooling carbon nitride silicon oxide film according to claim 1, characterized in that: In S2, x=any value between 0.5 and 10.
3. The method for preparing a proton irradiation resistant, passive cooling carbon nitride silicon oxide film according to claim 1, characterized in that: The atmosphere in S4 is one of air, oxygen, nitrogen, argon, hydrogen and a hydrogen-argon mixture.
4. The method for preparing a proton irradiation resistant, passive cooling carbon nitride silicon oxide film according to claim 1, characterized in that: The annealing temperature in S4 is any temperature in the range of 80-150°C.
5. The method for preparing a proton irradiation resistant, passive cooling carbon nitride silicon oxide film according to claim 1, characterized in that: The silicon oxycarbon nitride film is composed of silicon-carbon bonds, silicon-nitrogen bonds and silicon-oxygen bonds. The silicon oxycarbon nitride film is prepared by a chemical process of chemical bond breaking and recombination of an organic polysiloxane precursor film under heating conditions, and after removing some invalid impurities such as carbon dioxide and water vapor. The silicon oxycarbon nitride film achieves zero-energy passive cooling of solar cell films through the strong emission of silicon-carbon bonds, silicon-nitrogen bonds and silicon-oxygen bonds in the structure in the infrared spectrum and the proton radiation resistance of this type of chemical bonds.
6. The method for preparing a proton irradiation resistant, passive cooling carbon nitride silicon oxide film according to claim 1, characterized in that: In S1, after the backlight surface of the copper indium gallium selenide thin-film battery is encapsulated and protected, the sun-facing side of the copper indium gallium selenide thin-film battery is cleaned with methanol and acetone, and then placed on a battery film fixing bracket made in the laboratory to ensure the flatness of the copper indium gallium selenide thin-film battery. The sun-facing side of the fixed copper indium gallium selenide thin-film battery is then placed in an ultraviolet light cleaning machine at 300W power for 10 minutes to obtain a clean surface.
7. A proton irradiation-resistant, passive cooling carbon nitride silicon oxide film, characterized in that: Prepared by the method described in any one of claims 1 to 6.
8. The proton radiation resistant, passive cooling carbon nitride silicon oxide film according to claim 7, characterized in that: Application in the preparation of copper indium gallium selenide thin film solar cells for long-service-life spacecraft.
9. The proton radiation resistant, passive cooling carbon nitride silicon oxide film according to claim 8, characterized in that: The technical characteristics of the prepared silicon carbon nitride oxide film with the best performance are as follows: (1) Appearance of silicon oxycarbon nitride film: transparent grayish white, evenly distributed; (2) Silicon oxycarbon nitride film thickness: 3.2 μm; (3) Solar spectrum transmittance of silicon oxycarbon nitride film> 0.92; (4) The infrared radiation rate of the silicon oxycarbon nitride film is 0.72, and the cooling efficiency is 203.6W / m 2 ; (5) When facing the sun, the temperature on the back of the battery is 30°C lower than that on the side facing the sun; (6) After simulating the proton irradiation dose of geosynchronous orbit for one year under 90keV proton irradiation conditions, the absorption rate of the solar spectrum band increased and the cooling efficiency decreased to 182.1W / m 2 ; (7) Proton irradiation aging experiments show that the use of the carbon nitride silicon oxide film of the present invention can increase the life of the copper indium gallium selenide thin film solar cells in orbit by 35%-40%.
Citation Information
Patent Citations
Modified polysilazane, coating solution containing said modified polysilazane, and gas barrier film produced using said coating solution
CN105939959A
Front sheet for solar cell and solar cell module
JP2019064110A
Modified polysilazane, coating solution containing said modified polysilazane, and gas barrier film produced using said coating solution
WO2015119260A1