Modified nickel-zinc battery negative electrode and method
By sputtering carbon film and tin film on the surface of the zinc negative electrode to form a protective layer, the problem of zinc negative electrode corrosion is solved, the cycle stability and service life of nickel-zinc batteries are improved, and a simple and efficient preparation process and low-cost zinc negative electrode are realized. Production.
Patent Information
- Application Number
- CN202410956836.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-05
AI Technical Summary
The zinc negative electrode in existing nickel-zinc batteries is prone to corrosion, deformation and hydrogen evolution reaction, resulting in electrode failure. The existing modification strategy is complex, high cost, and uneven product surface, making it difficult to produce and apply on a large scale.
Magneto-controlled sputtering method is used to sputter the carbon film and tin film on the surface of the polished zinc sheet to form a protective layer, inhibit electrochemical corrosion and guide ion nucleation, and prepare a zinc negative electrode with excellent specific capacity and stability.
It improves the cycle stability and service life of zinc negative electrode, has simple process, controllable conditions, and is low in cost. It is suitable for nickel-zinc batteries and water-based zinc ion batteries.
Smart Images

Figure CN118899407A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrochemistry, and in particular relates to a modified nickel-zinc battery negative electrode and a method. Background Art
[0002] With the rapid development of the global economy, people's demand for energy is increasing. However, the massive consumption of non-renewable fossil fuels has brought about an energy crisis and put tremendous pressure on the ecological environment. Due to the convenience, popularity and cleanliness of electric energy, the development of secondary energy using electric energy as a carrier has become the current and future energy development trend.
[0003] At present, lead-acid batteries, nickel-metal hydride batteries, nickel-cadmium batteries, lithium-ion batteries, etc. have been industrialized, but these systems have certain defects, which restrict their further development and application; lead-acid secondary batteries are cheap, but have low mass-to-energy ratios, and fast charging performance cannot meet development needs; the cadmium element used in nickel-cadmium batteries poses a serious threat to the environment and human body, and has a significant memory effect; a large amount of rare earth elements are used in the negative electrode of nickel-metal hydride batteries, making them difficult to use widely. Lithium-ion batteries have the advantages of long cycle stability, high energy density and high energy efficiency, but the flammable organic electrolytes they use bring huge safety hazards, which can easily cause fires or even explosions, and lithium-ion batteries have high economic costs.
[0004] Unlike the embedding / de-embedding mechanism of common ion batteries, aqueous nickel-zinc batteries are alkaline batteries whose nickel hydroxide positive electrode reaction is based on the embedding / de-embedding of protons, while the zinc negative electrode exchanges electrons through reactions with hydroxide and water molecules. Compared with other aqueous batteries (mostly below 1.5 V), nickel-zinc batteries have a higher open circuit voltage (~1.75 V), can be stably cycled at higher rates, and have relatively high volumetric and mass energy densities. In summary, the performance of nickel-zinc batteries is more balanced and more conducive to application in large-scale energy storage devices.
[0005] As a thermodynamically active metal, zinc has high electrochemical activity in KOH electrolyte. Zinc electrodes often suffer from corrosion, deformation, dendrites, and hydrogen evolution reactions, which eventually lead to electrode failure. To address this series of problems, existing modification strategies mainly include doping and coating of active substances and constructing functional films on the surface of the negative electrode. Specific methods include spin coating, impregnation, sintering, atomic layer deposition, etc. However, most of these methods are complex and costly, and the product surface is relatively uneven, making it difficult to mass-produce and apply. Summary of the invention
[0006] The present invention provides a modified nickel-zinc battery negative electrode and method. The method simply and efficiently prepares a zinc negative electrode modified with a carbon film and a tin film. The prepared zinc negative electrode has excellent specific capacity and stability. The preparation process is simple to operate, the reaction conditions are mild, and the target material used is widely available and inexpensive.
[0007] In order to achieve the above purpose, the present invention adopts the following technical solutions: A method for modifying a negative electrode of a nickel-zinc battery comprises the following steps: (1) Cut the zinc sheet into a rectangular shape, polish it with metallographic sandpaper to remove the surface passivation layer, ultrasonically clean it with ethanol and acetone for 10-30 minutes, then clean it with deionized water, and then dry it at 60-100°C; (2) Place the prepared zinc sheet into a magnetron sputtering apparatus, install the Sn source target, introduce argon gas to control the pressure to 0.5-2 Pa, and DC sputter the Sn source target for 0.5-2 hours at a power of 20-100 W; (3) Install the C source target, introduce argon gas to control the pressure to 1-5 Pa, and RF sputter the C source target at a power of 50-200 W for 0.5-2 hours; (4) The sputtering sequence is then switched to Sn source target sputtering, and steps (2) and (3) are repeated for 5-20 cycles; (5) Cut the sample obtained in step (4) into a suitable size and prepare it into an electrode.
[0008] In the above steps, the Sn source target is a metal Sn target or a SnO2 target, and the C source target is a graphite C target; the thickness of the sample film obtained in step (4) is 100-500 nanometers, and the thickness of the film can be controlled by changing the sputtering power, pressure and time; if the coating is too thick, the interface charge transfer resistance will increase and the energy density will be compressed; if it is too thin, the protective layer effect will be weak, so it should be controlled within an appropriate range.
[0009] The method adopts a dual-target magnetron sputtering apparatus to evenly sputter a carbon target radio frequency and a tin target direct current onto the surface of the zinc negative electrode, and the thickness of the protective film is 100-300nm.
[0010] Beneficial effects: The present invention provides a modified nickel-zinc battery negative electrode and method. The present invention provides a method for enhancing the cycle stability of the zinc negative electrode in a nickel-zinc battery. The C film and the Sn film are sputtered on the surface of the polished zinc sheet by magnetron sputtering to protect the zinc negative electrode from corrosion. Sn has a high hydrogen evolution overpotential, which can effectively inhibit the generation of H2 and thus reduce electrochemical corrosion. It is non-toxic to the electrode and has low cost. The C film covers the surface of the Sn film and the zinc electrode, which can reduce the direct contact between the electrode and the electrolyte and guide ion nucleation. The zinc negative electrode prepared by the present invention has a significantly improved service life in the nickel-zinc battery, and the preparation process is simple and easy to operate, and the conditions are controllable. It has broad application prospects in the fields of nickel-zinc batteries and aqueous zinc ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 is the XRD spectrum of the modified zinc negative electrode material and the bare zinc sheet in the embodiment of the present invention; Figure 2 1 is a scanning electron microscope image of a bare zinc sheet (a) and a modified zinc negative electrode (b) in an embodiment of the present invention, and a scanning electron microscope image of a bare zinc sheet (c) and a modified zinc negative electrode (d) after being immersed in a KOH electrolyte for one week; Figure 3 This is a comparison chart of the cycle performance of a nickel-zinc battery assembled with a modified zinc negative electrode and a nickel-zinc battery assembled with a bare zinc negative electrode in an embodiment of the present invention. DETAILED DESCRIPTION
[0012] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments: Example 1
[0013] A method for modifying the negative electrode of a nickel-zinc battery, using a dual-target magnetron sputtering apparatus to evenly sputter a carbon target radio frequency and a tin target direct current onto the surface of the zinc negative electrode, comprising the following steps: The zinc sheet was cut into a rectangle, polished with metallographic sandpaper to remove the surface passivation layer, ultrasonically cleaned with ethanol and acetone for 15 minutes, then cleaned with deionized water, and then dried at 60 °C. The prepared zinc sheet was placed in a magnetron sputtering instrument, the metal Sn target was installed, and the vacuum was evacuated to a pressure of 5×10 -3 Pa, argon is introduced to control the flow rate to 50sccm, the baffle is kept closed, and the metal Sn target is pre-sputtered for 15 minutes with a DC power supply of 20W, and then the flow rate of argon is changed to make the pressure 0.8Pa, and the Sn source target is sputtered at a power of 20W for 30 minutes; then the C source target is installed, evacuated to a pressure of 5×10-3Pa, argon is introduced to control the flow rate to 50sccm, the baffle is kept closed, and the graphite C target is pre-sputtered for 15 minutes with an RF power supply of 150W, and then the argon flow rate is changed to control the pressure in the instrument to 2Pa, and the C source target is sputtered at a power of 150W for 30 minutes; then the sputtering sequence is switched to sputtering of the Sn source target, and the sputtering is repeated 3 times; the obtained sample is cut into a suitable size and prepared into an electrode.
[0014] The XRD pattern of Zn-C Sn electrode is shown in Figure 1 As shown, compared with the normal zinc diffraction peaks, there are four more peaks at 30.6°, 32°, 43.8° and 44.9°, which correspond to the (200), (101), (220) and (211) planes of Sn, respectively.
[0015] Scanning electron microscopy images Figure 2 As shown, Figure 2 (a) and Figure 2 (b) By comparison, it can be seen that carbon atoms and tin atoms are successfully deposited on the surface of the zinc sheet and are evenly distributed. After being immersed in 6M KOH electrolyte for one week, Figure 2 As shown in (c), the surface of the bare zinc sheet is severely corroded, and many deep pits and thick corrosion layers can be observed; Figure 2 As shown in (d), the protective layer on the surface of the Zn-CSn electrode has not fallen off and the morphology is relatively flat, proving that the corrosion is weakened.
[0016] The prepared Zn-CSn negative electrode and nickel hydroxide positive electrode were assembled into a nickel-zinc full battery and constant current charge and discharge tests were carried out on the Xinwei system. Figure 3 As shown in the figure, at a current rate of 1C, the Zn-CSn electrode can be cycled for nearly 800 cycles, and the capacity is maintained at a high state. Compared with the full battery assembled with bare zinc electrodes, the cycle life and capacity retention rate are significantly improved. Example 2
[0017] A method for modifying the negative electrode of a nickel-zinc battery, using a dual-target magnetron sputtering apparatus to evenly sputter a carbon target radio frequency and a tin target direct current onto the surface of the zinc negative electrode, comprising the following steps: The zinc sheet was cut into a rectangle, polished with metallographic sandpaper to remove the surface passivation layer, ultrasonically cleaned with ethanol and acetone for 15 minutes, then cleaned with deionized water, and then dried at 60°C. Place the prepared zinc sheet into a magnetron sputtering instrument, install the SnO2 target, evacuate to a pressure of 5×10-3Pa, introduce argon to control the flow rate to 50sccm, keep the baffle closed, pre-sputter the SnO2 target for 15 minutes with a DC power supply of 30W, then change the flow rate of argon to make the pressure 0.8Pa, and sputter the Sn source target for 30 minutes with a power of 30W; then install the C source target, evacuate to a pressure of 5×10-3Pa, introduce argon to control the flow rate to 50sccm, keep the baffle closed, pre-sputter the graphite C target for 15 minutes with a RF power supply of 180W, then change the argon flow rate to control the pressure in the instrument to 2Pa, and sputter the C source target for 30 minutes with a power of 180W; then switch the sputtering sequence to sputtering of the Sn source target, and repeat the sputtering 3 times; cut the obtained sample into a suitable size and prepare it into an electrode. Example 3
[0018] A method for improving the stability of a negative electrode of a nickel-zinc battery, using a dual-target magnetron sputtering apparatus to evenly sputter a carbon target radio frequency and a tin target direct current onto a surface of a zinc negative electrode, comprising the following steps: The zinc sheet was cut into a rectangle, polished with metallographic sandpaper to remove the surface passivation layer, ultrasonically cleaned with ethanol and acetone for 15 minutes, then cleaned with deionized water, and then dried at 60°C. The prepared zinc sheet was placed in a magnetron sputtering instrument, and the metal Sn target was installed. The pressure was evacuated to 5×10-3Pa, and argon was introduced to control the flow rate to 50sccm. The baffle was kept closed, and the metal Sn target was pre-sputtered for 15 minutes with a DC power supply of 30W. Then, the flow rate of argon was changed to make the pressure 0.8Pa, and the Sn source target was sputtered at a power of 30W for 1 hour; then the C source target was installed, the pressure was evacuated to 5×10-3Pa, and argon was introduced to control the flow rate to 50sccm. The baffle was kept closed, and the graphite C target was pre-sputtered for 15 minutes with a RF power supply of 180W. Then, the argon flow rate was changed to control the pressure in the instrument to 2Pa, and the C source target was sputtered at a power of 180W for 1 hour; then the sputtering sequence was switched to sputtering of the Sn source target, and the sputtering was repeated 3 times; the obtained sample was cut into a suitable size and prepared into an electrode.
[0019] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principle of the present invention, and these improvements should also be regarded as within the protection scope of the present invention.
Claims
1. A modified nickel-zinc battery negative electrode, characterized in that: The surface of the negative electrode is plated with a C-Sn film.
2. The modified nickel-zinc battery negative electrode according to claim 1, characterized in that: The thickness of the film is 100-500 nanometers.
3. A method for modifying a negative electrode of a nickel-zinc battery, characterized in that: The following steps are involved: Direct-current sputtering of Sn source target on the treated zinc sheet; RF sputtering C source target; Repeat the DC sputtering Sn source and RF sputtering C source for 5-20 cycles to complete the modification of the negative electrode of the nickel-zinc battery.
4. The method for modifying the negative electrode of a nickel-zinc battery according to claim 3, characterized in that: The zinc sheet treatment process is as follows: cutting the zinc sheet into a rectangle, grinding with metallographic sandpaper to remove the surface passivation layer, ultrasonically cleaning with ethanol and acetone for 10-30 minutes, then cleaning with deionized water, and then drying at 60-100°C.
5. The method for modifying the negative electrode of a nickel-zinc battery according to claim 3, characterized in that: The Sn source target material is one or more of a metal Sn target and a SnO2 target.
6. The method for modifying the negative electrode of a nickel-zinc battery according to claim 3 or 5, characterized in that: The power of sputtering Sn source target is 20-100W, and the time is 0.5-2 hours.
7. The method for modifying the negative electrode of a nickel-zinc battery according to claim 6, characterized in that: Before sputtering the Sn source target, argon gas is introduced to control the pressure to 0.5-2Pa.
8. The method for modifying the negative electrode of a nickel-zinc battery according to claim 3, characterized in that: The C source target used is graphite C target.
9. The method for modifying the negative electrode of a nickel-zinc battery according to claim 3 or 8, characterized in that: The power of sputtering C source target is 50-200W, and the time is 0.5-2 hours.
10. The method for modifying the negative electrode of a nickel-zinc battery according to claim 9, characterized in that: Before sputtering the C source target, argon gas is introduced to control the pressure to 1-5Pa.