Electrode for lithium secondary battery and method for manufacturing same
By forming a regularly arranged hemispherical raised polymer film on the surface of the electrode of the lithium secondary battery and preparing a conductive metal layer, the problem of lithium dendrites is solved, the circulation performance and efficiency of the lithium secondary battery are improved, and the battery is enhanced stability.
Patent Information
- Application Number
- CN202410942389.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-27
- Filing Date
- 2019-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
The uneven deposition and peeling of lithium metal during the charging/discharging process of lithium secondary batteries lead to the formation of lithium dendrites, reducing the safety and efficiency of the battery.
A regularly arranged hemispherical raised polymer film is formed on the surface of the electrode of the lithium secondary battery, and a conductive metal layer and a lithium metal layer are formed thereon. The preparation is made by electroless plating technology to ensure uniform deposition and peeling of lithium metal.
Through uniform lithium metal deposition and peeling, the circulation performance and efficiency of lithium secondary batteries are improved, the uneven growth of lithium dendrites is significantly suppressed, and the stability and processability of the battery are enhanced.
Smart Images

Figure CN118899446A_ABST
Abstract
Description
[0001] This application is a divisional application. The international application number of the original application is PCT / KR2019 / 008600, the application number of the Chinese national phase is 201980004922.0, the application date is July 11, 2019, and the name of the invention is "Electrodes for lithium secondary batteries and methods for manufacturing the same". Technical Field
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application is based on and claims the benefit of priority from Korean Patent Application No. 10-2018-0100361, filed on August 27, 2018, the disclosure of which is incorporated herein in its entirety by reference.
[0004] The present invention relates to an electrode for a lithium secondary battery and a method for manufacturing the same. The electrode for a lithium secondary battery is applied to a lithium secondary battery to improve the cycle performance and efficiency of the battery. Background Art
[0005] With the rapid development of the electronics, telecommunications and computer industries, the application of energy storage technology is expanding to camcorders, mobile phones, notebook computers, PCs, and even electric vehicles. Therefore, a high-performance secondary battery with light weight, long life and high reliability is being developed.
[0006] Among the secondary batteries currently in use, lithium secondary batteries developed in the early 1990s have attracted much attention due to their higher operating voltage and significantly higher energy density compared to conventional batteries using aqueous electrolyte solutions (e.g., Ni-MH, Ni-Cd, and lead sulfate batteries).
[0007] As negative electrode active materials of lithium secondary batteries, lithium metal, carbon-based materials, silicon, etc. are used. Among them, lithium metal has an advantage in that the highest energy density can be obtained, and thus research has been continuously conducted thereon.
[0008] Typically, lithium foil is attached to a planar copper or nickel foil as a current collector to make a lithium electrode using lithium metal as an active material. Alternatively, the lithium foil can be used directly as a lithium electrode without a separate current collector.
[0009] However, the problem with such lithium electrodes is that during the process of lithium metal deposition and stripping on the electrode during charging / discharging of the battery, non-uniform growth of lithium dendrites occurs on the surface. Lithium dendrites may cause damage to the separator and short circuit of the lithium secondary battery, thereby reducing the safety of the battery. Therefore, it is necessary to improve it. Summary of the invention
[0010] Technical issues
[0011] An object of the present invention is to provide an electrode for a lithium secondary battery and a method for manufacturing the same, which can improve the cycle and efficiency characteristics of a lithium secondary battery by promoting uniform deposition and stripping of lithium metal when charging / discharging the battery.
[0012] Technical Solution
[0013] In order to achieve the above object, the present invention provides an electrode for a lithium secondary battery, the electrode comprising:
[0014] A polymer film having a pattern formed on one surface thereof, in which a plurality of hemispherical protrusions having a diameter of 5 μm to 50 μm are regularly arranged;
[0015] a conductive metal layer formed on the pattern of the polymer film; and
[0016] A lithium metal layer is formed on the conductive metal layer.
[0017] The height of the hemispherical protrusions may be 3 μm to 50 μm.
[0018] Preferably, the hemispherical protrusion may have a diameter of 7 μm to 40 μm and a height of 5 μm to 40 μm.
[0019] The pitch between the hemispherical protrusions may be 2 μm to 50 μm.
[0020] The polymer film may be one or more selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polybutylene, polyphenylene sulfide, polyethylene sulfide, polyimide, and polytetrafluoroethylene.
[0021] The polymer film may have a thickness of 5 μm to 30 μm, the thickness excluding the height of the hemispherical protrusions.
[0022] The conductive metal may be one or more selected from the group consisting of Ni, Ti, Cu, Ag, Au, Pt, Fe, Co, Cr, W, Mo, Al, Mg, K, Na, Ca, Sr, Ba, Si, Ge, Sb, Pb, In and Zn.
[0023] The thickness of the conductive metal layer may be 0.5 μm to 10 μm.
[0024] The thickness of the lithium metal layer may be 5 μm to 50 μm.
[0025] Furthermore, the present invention provides a lithium secondary battery including the lithium secondary battery electrode.
[0026] In addition, the present invention provides a method for manufacturing an electrode for a lithium secondary battery, the method comprising the following steps:
[0027] preparing a polymer film having a pattern formed on one surface thereof, in which a plurality of hemispherical protrusions having a diameter of 5 μm to 50 μm are regularly arranged;
[0028] forming a conductive metal layer by chemically plating a conductive metal precursor onto the pattern of the polymer film; and
[0029] The lithium metal layer is formed by electroplating lithium metal onto the conductive metal layer.
[0030] The conductive metal precursor may be one or more selected from the group consisting of sulfates, halides, nitrates and hydroxides of Ni, Ti, Cu, Ag, Au, Pt, Fe, Co, Cr, W, Mo, Al, Mg, K, Na, Ca, Sr, Ba, Si, Ge, Sb, Pb, In or Zn.
[0031] In the electroless plating step, one or more selected from the group consisting of glycine, formaldehyde, hydrazine, and citric acid may be used as a reducing agent.
[0032] The conductive metal layer may be formed in a thickness of 0.5 μm to 10 μm.
[0033] The lithium metal layer may be formed in a thickness of 5 μm to 50 μm.
[0034] Effects of the Invention
[0035] If the lithium secondary battery electrode of the present invention is applied to a lithium secondary battery, lithium metal is uniformly deposited and stripped on the entire surface of the electrode when the battery is charged / discharged, thereby preventing uneven formation of lithium dendrites, thereby improving the cycle and efficiency characteristics of the battery.
[0036] Furthermore, the electrode for a lithium secondary battery of the present invention may exhibit significantly high flexibility compared to existing electrodes including a metal current collector and an active material layer, thereby improving processability during electrode manufacturing and battery assembly. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a cross-sectional view of an electrode for a lithium secondary battery according to one embodiment of the present invention;
[0038] Figure 2 is a cross-sectional view showing the shape of the polymer film of the present invention;
[0039] Figure 3 A method for producing an electrode for a lithium secondary battery according to one embodiment of the present invention is described. DETAILED DESCRIPTION
[0040] The terms used in this specification are only used to explain the exemplary embodiments and are not intended to limit the present invention. Unless expressed differently in the context, a singular expression may include a plural expression. It must be understood that the terms "including", "equipped with" or "having" in this specification are only used to indicate the presence of features, steps, components or combinations thereof, and do not exclude the prior existence or possible addition of one or more different features, steps, components or combinations thereof.
[0041] Although the present invention is susceptible to various modifications and alternative forms, specific embodiments will be described and described in detail as follows. However, it should be understood that this description is not intended to limit the present invention to the specific forms disclosed, but on the contrary, the present invention covers all modifications, equivalents and substitutes falling within the spirit and scope of the present invention.
[0042] Likewise, the drawings are shown to describe an exemplary embodiment of the present invention, and therefore, the present invention may be implemented in several different forms and is therefore not limited to the embodiments described herein. In order to more clearly describe the present invention, certain parts that are not relevant to the description are omitted in the drawings, and the same parts have the same reference numerals throughout the specification. Moreover, the sizes and relative sizes of the parts shown in the drawings are not related to their actual scale and may be enlarged or reduced for ease of description.
[0043] Electrode for lithium secondary battery and method for producing the same
[0044] The present invention relates to an electrode for a lithium secondary battery, the electrode comprising:
[0045] A polymer film having a pattern formed on one surface thereof, in which a plurality of hemispherical protrusions having a diameter of 5 μm to 50 μm are regularly arranged;
[0046] a conductive metal layer formed on the pattern of the polymer film; and
[0047] A lithium metal layer is formed on the conductive metal layer.
[0048] Figure 1 The structure of a lithium secondary battery electrode 100 according to one embodiment of the present invention is shown.
[0049] The electrode for lithium secondary battery of the present invention has the following structure, wherein a conductive metal layer 20 and a lithium metal layer 30 are sequentially stacked on a polymer film 10 having a pattern formed on one surface. The polymer film 10 serves as a support for the conductive metal layer 20 and the lithium metal layer 30. The pattern formed on the polymer film has a shape in which a plurality of hemispherical protrusions 11 are regularly arranged. Since the thin conductive metal layer 20 and the lithium metal layer 30 are stacked on the pattern shape, the surface of the electrode to be manufactured finally has a plurality of hemispherical protrusions in accordance with the pattern shape of the polymer film 10. In this regard, "hemispherical protrusion" refers to a hemispherical protrusion whose outer periphery of the protrusion is curved, which does not necessarily refer to a hemispherical shape.
[0050] As mentioned above, when a pattern of hemispherical protrusions is formed on the surface of an electrode, a uniform current can be induced on the electrode surface when charging / discharging the battery, whereby lithium metal can be uniformly deposited and peeled off on the surface, which can significantly inhibit the uneven growth of lithium dendrites. Therefore, during the operation of the lithium secondary battery, the lithium secondary battery electrode of the present invention can have significantly improved stability, cycle characteristics and efficiency. At the same time, as demonstrated by the following experimental examples, when the periphery of the protrusion of the pattern is curved, the effect of inducing a uniform current can be obtained, and when the protrusion includes an angled portion such as a regular hexahedron shape, it is difficult to expect the effect of dispersing the current density. In addition, even if the periphery of the hemispherical protrusion is curved, the effect can be ensured only when the diameter of the protrusion meets the appropriate range.
[0051] In order to ensure the above effect, the diameter of the hemispherical protrusions 11 in the pattern of the polymer film 10 is preferably 5 μm or more, 7 μm or more, or 10 μm or more, and 50 μm or less, 40 μm or less, or 30 μm or less. Figure 2 As shown, the diameter d of the hemispherical protrusion refers to the longest straight line distance from one side to the other side of the lowest part of the hemispherical protrusion. If the diameter of the hemispherical protrusion is less than 5 μm, the shape of the pattern may become less obvious on the surface of the lithium metal layer of the electrode finally manufactured by stacking the conductive metal layer 20 and the lithium metal layer 30. If the diameter of the hemispherical protrusion is large enough to exceed 50 μm, it is difficult to ensure the effect of dispersing the current density by patterning. Therefore, it is preferred that the diameter meets the above range.
[0052] Meanwhile, the height h1 of the hemispherical protrusion 11 refers to the height from the bottom to the top of the hemispherical protrusion, and is preferably 3 μm or more, 5 μm or more, or 10 μm or more, and 50 μm or less, 40 μm or less, or 30 μm or less. If the height of the hemispherical protrusion 11 is less than 3 μm, the shape of the pattern may become less obvious on the electrode finally manufactured, and if the height of the hemispherical protrusion 11 exceeds 50 μm, the electrode becomes too thick, so there is a problem of reduced energy density.
[0053] In addition, if Figure 2As shown, the spacing g between the hemispherical protrusions 11 refers to the shortest straight-line distance from one side of the lowest part of one hemispherical protrusion to the other side of another hemispherical protrusion, and the spacing between the hemispherical protrusions is preferably 50 μm or less, 40 μm or less, or 30 μm or less. One hemispherical protrusion and another hemispherical protrusion may be arranged so that there is no gap between them. Therefore, there is no limit to the lower limit of the spacing between the hemispherical protrusions, but considering the thickness of the conductive metal layer and the lithium metal layer stacked on the polymer film, the spacing may be preferably 2 μm or more or 3 μm or more.
[0054] If the polymer film is too thick, the flexibility of the electrode is reduced, and conversely, if the polymer film is too thin, it cannot be used as a support, which may impair processability during electrode manufacturing and battery assembly. Therefore, excluding the height of the hemispherical protrusion, the thickness h2 of the polymer film is preferably 5 μm to 30 μm, or 8 μm to 15 μm.
[0055] At the same time, the material of the polymer film is not particularly limited, but a polymer that is flexible, not easily reacted with an organic electrolyte solution, and not easily broken due to excellent tensile strength can be appropriately used. For example, the material applicable to the polymer film of the present invention can be selected from one or more of the group consisting of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polybutene, polyphenylene sulfide, polyethylene sulfide, polyimide and polytetrafluoroethylene, but is not limited thereto. Among them, polyethylene terephthalate (PET), polyimide or polytetrafluoroethylene with excellent flexibility and strength characteristics are preferably used, more preferably PET.
[0056] In the present invention, the conductive metal layer 20 is composed of a conductive metal that can be used as a collector, and as the conductive metal, any type commonly used in the negative electrode collector of a lithium secondary battery can be used without limitation. For example, the conductive metal can be one or more selected from the group consisting of Ni, Ti, Cu, Ag, Au, Pt, Fe, Co, Cr, W, Mo, Al, Mg, K, Na, Ca, Sr, Ba, Si, Ge, Sb, Pb, In and Zn, and in consideration of conductivity and economic efficiency, Ni, Cu or Ti may be preferred, more preferably Ni.
[0057] The thickness of the conductive metal layer 20 may be 0.5 μm to 10 μm, 1 μm to 7 μm, or 2 μm to 5 μm. If the thickness of the conductive metal layer 20 is thicker than 10 μm, the energy density may be reduced to deteriorate the performance of the battery, and the pattern formed on the polymer film 10 may become less obvious on the surface of the electrode finally manufactured, and it is difficult to ensure the effect of the present invention. On the contrary, if the thickness is thinner than 0.5 μm, a uniform conductive metal layer will not be formed, and there is a problem of difficulty in ensuring sufficient conductivity. Therefore, it is preferred that the thickness meets the above range.
[0058] The electrode for the lithium secondary battery of the present invention includes lithium metal as an active material. The lithium metal layer 30 is formed on the conductive metal layer 20, and preferably has a thickness of 5 μm or more or 10 μm or more so that the electrode can be stably charged / discharged. At the same time, if the lithium metal layer 30 is too thick, the pattern formed on the polymer film 10 may become unclear on the lithium metal layer 30, so it is difficult to achieve the effect of the present invention. Therefore, the thickness of the lithium metal layer 30 is preferably less than 50 μm or less than 40 μm.
[0059] The method for producing the electrode for lithium secondary battery of the present invention is not particularly limited. Figure 3 As shown, the method may include the following steps: preparing a polymer film having a pattern formed on one surface thereof, wherein a plurality of hemispherical protrusions having a diameter of 5 μm to 50 μm are regularly arranged; forming a conductive metal layer by chemically plating a conductive metal precursor onto the pattern of the polymer film; and forming a lithium metal layer by electroplating lithium metal onto the conductive metal layer. The method may be further indicated by the following examples.
[0060] As the polymer film, those commercially available or directly manufactured can be used. When a directly manufactured polymer film is used, its manufacturing method is not limited, and various methods known in the art, such as extrusion molding, injection molding, solution casting, etc., can be applied. The method of forming a pattern on the polymer film is not particularly limited, but a method of placing a flat polymer film on a mold and pressing and / or heating the polymer film to form a pattern can be used.
[0061] The step of forming the conductive metal layer can be performed by chemically plating a conductive metal precursor. Chemical plating can be a method in which a metal ion of a metal salt in an aqueous solution is reduced to a metal using a reducing agent, thereby precipitating the metal on the surface to be treated. Common chemical plating methods known in the art can be used without limitation.
[0062] The conductive metal precursor used in the step of chemical plating can be a sulfate, halide, nitrate or hydroxide of Ni, Ti, Cu, Ag, Au, Pt, Fe, Co, Cr, W, Mo, Al, Mg, K, Na, Ca, Sr, Ba, Si, Ge, Sb, Pb, In or Zn. The conductive metal precursor is preferably used in the range of 0.1M to 3M or 0.5M to 1.5M so that a sufficient amount of conductive metal layer can be formed on the polymer film.
[0063] As a reducing agent in the step of chemical plating, glycine, formaldehyde, hydrazine, citric acid, etc. can be used, and the reducing agent can be used in an appropriate range according to the molar number of the conductive metal precursor used. For example, when the conductive metal precursor contains monovalent metal ions, the reducing agent can be used in the range of 0.1M to 3M or 0.5M to 1.5M. When the conductive metal precursor contains divalent metal ions, the reducing agent can be used in the range of about twice the above concentration (in the range of 0.2M to 6M or 1M to 3M). When the conductive metal precursor contains trivalent metal ions, the reducing agent can be used in the range of about three times the above concentration (in the range of 0.3M to 9M or 1.5M to 4.5M).
[0064] At the same time, in the step of chemical plating, the conductive metal precursor solution and the reducing agent solution may not be a one-time but continuously fed at a constant rate into the electrolytic cell where the polymer film to be treated and water are placed. When the conductive metal precursor solution and the reducing agent solution are fed into the electrolytic cell once, uniform chemical plating may not occur on the polymer film, and uniform formation of the conductive metal layer may not occur. On the contrary, when they are fed continuously, a uniform conductive metal layer can be preferably obtained. For example, the conductive metal precursor solution and the reducing agent solution can be fed at a rate of 0.05ml / min to 1ml / min or 0.1ml / min to 0.5ml / min, and the feeding time (reaction time) can be 20 minutes to 5 hours, or 30 minutes to 3 hours.
[0065] The formation of the lithium metal layer can be performed by electroplating lithium metal. The electroplating can be performed in a non-aqueous solvent in the presence of a lithium salt. The non-aqueous solvent can be one or more selected from the group consisting of the following organic solvents: 1,4-dioxane, 1,2-dimethoxyethane, tetrahydrofuran, dichloromethane, N-methylpyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethylmethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydroxyfranc, 2-methyl Tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl-1,3-dioxine, diethyl ether, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, ethyl propionate, etc.
[0066] In addition, the lithium salt may be one or more selected from the group consisting of LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiC4BO8, LiCF3CO2, LiCH3SO3, LiCF3SO3, LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiC4F9SO3, LiC(CF3SO2)3, (CF3SO2)2NLi, lithium chloroborate, lower aliphatic lithium carboxylate, lithium tetraphenylborate and lithium imide. Among them, in consideration of reactivity, one or more selected from the group consisting of LiN(SO2F)2, LiCl and LiPF6 can be more preferably used.
[0067] The process conditions of the electroplating step are not particularly limited. However, for example, the polymer film on which the conductive metal layer is formed may be placed in an electrolytic bath containing a non-aqueous solvent and a lithium salt, and then 0.1 mA / cm2 may be applied thereto at room temperature of 20° C. to 30° C. 2 Up to 10mA / cm 2 of current.
[0068] Lithium secondary battery
[0069] The present invention provides a lithium secondary battery comprising the above-mentioned lithium secondary battery electrode. The lithium secondary battery of the present invention comprises a positive electrode, a negative electrode, a separator disposed therebetween, and an electrolyte, and the lithium secondary battery electrode is preferably used as the negative electrode. As mentioned above, when the lithium electrode of the present invention is used as the negative electrode, the growth of lithium dendrites can be significantly suppressed during the charge / discharge of the lithium secondary battery of the present invention. Thus, the cycle and efficiency characteristics of the battery can be ensured, and the stability of the battery can be improved.
[0070] The configurations of the positive electrode, separator, and electrolyte of the lithium secondary battery are not particularly limited in the present invention and follow those known in the art.
[0071] (1) Positive electrode
[0072] The positive electrode includes a positive electrode active material formed on a positive electrode collector.
[0073] The positive electrode collector is not particularly limited as long as it has high conductivity and does not cause chemical changes in the corresponding battery. For example, stainless steel, aluminum, nickel, titanium, fired carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium or silver can be used. In this regard, the positive electrode collector can be in various forms, such as films, sheets, foils, nets, porous materials, foam materials, non-woven fabric materials, etc., with fine concavo-convex objects on its surface to enhance the adhesion of the positive electrode active material.
[0074] The positive electrode active material constituting the electrode layer may be any positive electrode active material that can be used in the art. Specific examples of the positive electrode active material may include: lithium metal; lithium cobalt oxide, such as LiCoO2; lithium manganese oxide, such as Li 1+x Mn 2- x O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxides, such as Li2CuO2, etc.; vanadium oxides, such as LiV3O8, LiFe3O4, V2O5, Cu2V2O7, etc.; LiNi 1-x M x Lithium nickel oxide represented by LiMn O2 (wherein M is Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x is 0.01 to 0.3); 2-x M x A lithium manganese composite oxide represented by Li2Mn3MO8 (wherein M is Co, Ni, Fe, Cr, Zn or Ta, and x is 0.01 to 0.1); a lithium manganese composite oxide represented by Li(Ni a Co b Mn c)O2 (wherein, 0<a<1, 0<b<1, 0<c<1, a+b+c=1); vanadium oxides, such as LiV3O8, LiFe3O4, V2O5, Cu2V2O7, etc.; sulfur or disulfide compounds; phosphates, such as LiFePO4, LiMnPO4, LiCoPO4, LiNiPO4, etc.; Fe2(MoO4)3, etc., but not limited to these.
[0075] In this regard, the electrode layer may contain a binder resin, a conductive material, a filler, other additives, and the like in addition to the positive electrode active material.
[0076] Binder resin is used for the bonding of electrode active material and conductive material and the bonding of collector. Non-limiting examples of binder resin can include polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), polyacrylic acid (PAA), polymethacrylic acid (PMA), polymethyl methacrylate (PMMA), polyacrylamide (PAM), polymethacrylamide, polyacrylonitrile (PAN), polymethacrylonitrile, polyimide (PI), alginic acid, alginate, chitosan, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, various copolymers thereof, etc.
[0077] The conductive material is used to further improve the conductivity of the electrode active material. The conductive material is not particularly limited as long as it has conductivity and does not cause chemical changes in the corresponding battery. Examples thereof may include: graphite, such as natural graphite or artificial graphite; carbon black, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, etc.; conductive fibers, such as carbon fibers, metal fibers, etc.; metal powders, such as fluorocarbons, aluminum, nickel powders, etc.; conductive whiskers, such as zinc oxide, potassium titanate, etc.; conductive metal oxides, such as titanium oxide, etc.; and polyphenylene derivatives, etc.
[0078] The filler is a component that is optionally used to suppress electrode expansion. The filler is not particularly limited as long as it is a fiber material and does not cause chemical changes in the corresponding battery. For example, olefinic polymers such as polyethylene, polypropylene, etc. and fiber materials such as glass fiber, carbon fiber, etc. can be used.
[0079] (2) Diaphragm
[0080] The separator may be composed of a porous substrate. As the porous substrate, any porous substrate may be used as long as it is generally used in electrochemical devices. For example, a polyolefin-based porous film or nonwoven fabric may be used, but is not particularly limited thereto.
[0081] The separator can be a porous substrate composed of any one selected from the group consisting of the following substances or a mixture of two or more thereof: polyethylene, polypropylene, polybutylene, polypentene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide and polyethylene naphthalate.
[0082] (3) Electrolytes
[0083] The electrolyte of the lithium secondary battery may be a non-aqueous electrolyte solution containing a lithium salt and a non-aqueous organic solvent, an organic solid electrolyte, or an inorganic solid electrolyte, but is not limited thereto.
[0084] The non-aqueous organic solvent may be, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydroxyfrank, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl-1,3-dioxine, diethyl ether, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, ethyl propionate, and the like.
[0085] Lithium salts are materials that are easily soluble in non-aqueous electrolytes and may include, for example, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiC4BO8, LiCF3CO2, LiCH3SO3, LiCF3SO3, LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiC4F9SO3, LiC(CF3SO2)3, (CF3SO2)2NLi, lithium chloroborate, lithium lower aliphatic carboxylate, lithium tetraphenylborate, lithium imide, etc.
[0086] The organic solid electrolyte may include, for example, polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, poly-agitated lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, polymers containing secondary dissociative groups, and the like.
[0087] The inorganic solid electrolyte may include, for example, a nitride, halide or sulfate of Li, such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, Li3PO4-Li2S-SiS2, etc.
[0088] In addition, the electrolyte may further include other additives to improve charge / discharge characteristics, flame retardancy, etc. Examples of the additives may include pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, fluoroethylene carbonate (FEC), propene sultone (PRS), vinylene carbonate (VC), etc.
[0089] In addition to the general winding process, the lithium secondary battery of the present invention can also be subjected to lamination (stacking) and folding processes of the separator and the electrode. In addition, the battery housing can be cylindrical, square, pouch-shaped, coin-shaped, etc.
[0090] Hereinafter, preferred embodiments are provided to better understand the present invention. However, the following embodiments are only for illustrative purposes, and it will be apparent to those skilled in the art that various changes and modifications may be made within the scope of the present invention and technical spirit, and these changes and modifications belong to the scope of the appended claims.
[0091] Example 1
[0092] <Manufacturing of electrodes for lithium secondary batteries>
[0093] A PET film (thickness excluding the height of the protrusions: 10 μm) having a pattern of hemispherical protrusions (diameter: 10 μm, height: 10 μm, spacing between protrusions: 5 μm) was immersed in a water tank containing water, and then nickel sulfate (1 M) and glycine (1 M) were introduced at a rate of 0.15 mL / min for 2 hours to perform Ni chemical plating. The manufactured Ni / PET film (thickness of the Ni layer: 2 μm) was washed with distilled water and then dried.
[0094] The fabricated Ni / PET film was placed in a 1,4-dioxane (DX):1,2-dimethoxyethane (DME) solution (1:2, v / v) in which 1 M LiFSI was dissolved, and a current of 1 mA / cm was applied at room temperature (25 °C). 2A current of 10000 was used to perform Li electroplating. In this regard, PESC05 of PNE Solution Co., Ltd. was used as an electroplating machine. Through this process, an electrode for a lithium secondary battery was obtained, which was plated with lithium metal having a thickness of 20 μm, sequentially stacked with Li / Ni / PET, and had a plurality of regular hemispherical protrusions.
[0095] <Manufacturing of Symmetrical Cells>
[0096] A polyolefin separator was placed between the manufactured electrodes for lithium secondary batteries to manufacture a symmetrical cell, and an electrolyte solution in which 1M LiPF6 was dissolved in a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 50:50 was injected to manufacture a coin-type cell.
[0097] <Manufacturing of full battery cells>
[0098] The full cell is manufactured by placing a polyolefin separator between the manufactured lithium secondary battery electrode (negative electrode) and the positive electrode made by coating one surface of the aluminum collector with a slurry at a thickness of 65 μm and then drying and rolling, wherein the slurry is prepared by adding 96% by weight of LiCoO2 as a positive electrode active material, 2% by weight of Denka black (conductive material) and 2% by weight of PVdF (polyvinylidene fluoride, binder) to NMP (N-methyl-2-pyrrolidone). Then inject an electrolyte solution in which 1M LiPF6 is dissolved in a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) with a volume ratio of 50:50 to manufacture a coin-type cell.
[0099] Example 2
[0100] An electrode for a lithium secondary battery and a coin-type battery cell including the same were manufactured in the same manner as in Example 1, except that a PET film having hemispherical projections with a diameter of 20 μm was used.
[0101] Example 3
[0102] An electrode for a lithium secondary battery and a coin-type battery cell including the same were manufactured in the same manner as in Example 1, except that a PET film having hemispherical projections with a diameter of 40 μm was used.
[0103] Example 4
[0104] An electrode for a lithium secondary battery and a coin-type battery cell including the same were manufactured in the same manner as in Example 1, except that a PET film having hemispherical protrusions with a height of 20 μm was used.
[0105] Example 5
[0106] An electrode for a lithium secondary battery and a coin-type battery cell including the same were manufactured in the same manner as in Example 1, except that a PET film having hemispherical protrusions with a pitch of 10 μm was used.
[0107] Comparative Example 1
[0108] An electrode for a lithium secondary battery and a coin-type battery cell including the electrode for a lithium secondary battery were manufactured in the same manner as in Example 1, except that a PET film having no pattern of hemispherical protrusions was used.
[0109] Comparative Example 2
[0110] A coin-type battery cell was manufactured in the same manner as in Example 1, except that an untreated lithium metal foil (20 μm) was used as an electrode for a lithium secondary battery.
[0111] Comparative Example 3
[0112] An electrode for a lithium secondary battery and a coin-type battery cell including the same were manufactured in the same manner as in Example 1, except that a PET film having no hemispherical protrusions but regular hexahedral protrusions with a single side length of 10 μm was used.
[0113] Comparative Example 4
[0114] An electrode for a lithium secondary battery and a coin-type battery cell including the same were manufactured in the same manner as in Example 1, except that a PET film having hemispherical projections with a diameter of 4 μm was used.
[0115] Comparative Example 5
[0116] An electrode for a lithium secondary battery and a coin-type battery cell including the same were manufactured in the same manner as in Example 1, except that a PET film having hemispherical projections with a diameter of 60 μm was used.
[0117] Experimental Example 1
[0118] An electrochemical charger / discharger (PNE Solution, PESC05) was used at 1 mA / cm 2 Each coin-type symmetrical battery cell manufactured in the embodiment and the comparative example was repeatedly charged / discharged for 1 hour at a current density of . The following Table 1 shows a comparison of the overvoltage at the 100th cycle with the overvoltage at the 1st cycle.
[0119] Experimental Example 2
[0120] Each coin-type full cell manufactured in the examples and comparative examples was charged / discharged using an electrochemical charger / discharger (PNE Solution, PESC05). Charging was performed until the Li / Li + The voltage is 4.4V, and the discharge is carried out to the relative Li / Li + The voltage was 3.0 V, and a current density of 0.5 C rate was applied. Comparison of the discharge capacity at the 100th cycle with the discharge capacity at the 1st cycle is shown in Table 1 below.
[0121] Table 1
[0122]
[0123] As an experimental result, Examples 1 to 5 show that the rate of increase of overvoltage at the 100th cycle is significantly low relative to the 1st cycle, while the discharge capacity at the 100th cycle is significantly high, compared with Comparative Examples 1 and 2. The reason is that the electrode has a hemispherical pattern on its surface, so when the battery is charged and discharged, uniform lithium deposition and stripping occur on the entire surface of the electrode. In contrast, Comparative Examples 1 and 2, which do not have a pattern on the surface of the electrode, show a rapid increase in overvoltage and a significant decrease in discharge capacity, indicating that uneven lithium deposition and stripping occur due to the concentration of current in a specific area of the lithium metal surface.
[0124] Meanwhile, when the protrusions of the pattern were not hemispherical but in a regular hexahedral shape as in Comparative Example 3, the rate of increase of overvoltage increased and the discharge capacity decreased compared to Examples 1 to 5. This may be because the current density of the angled corners increased, which hindered uniform charging and discharging.
[0125] In addition, compared with Examples 1 to 5, Comparative Examples 4 and 5 show a high overvoltage growth rate and a low discharge capacity. This may be because the diameter of the hemispherical protrusion is too small or too large, so the effect of uniformly dispersing the current is reduced. These results show that the diameter of the hemispherical protrusion must meet the range of 5 μm to 50 μm to ensure the effect of the present invention.
[0126] Reference numerals
[0127] 10: Polymer film with a pattern on one surface
[0128] 11: Hemispherical bulge
[0129] 20: Conductive metal layer
[0130] 30: Lithium metal layer
[0131] 100: Electrodes for lithium secondary batteries
Claims
1. A lithium metal battery electrode, the electrode comprising: A polymer film having a pattern formed on one surface thereof, in which a plurality of hemispherical protrusions having a diameter of 10 μm to 40 μm are regularly arranged; a conductive metal layer formed on the pattern of the polymer film; and a lithium metal layer formed on the conductive metal layer, in, The height of the hemispherical protrusion is 3 μm to 50 μm.
2. The lithium metal battery electrode according to claim 1, wherein The height of the hemispherical protrusion is 5 μm to 40 μm.
3. The lithium metal battery electrode according to claim 1, wherein The interval between the hemispherical protrusions is 2 μm to 50 μm.
4. The lithium metal battery electrode according to claim 1, wherein The polymer film is one or more selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polybutylene, polyphenylene sulfide, polyethylene sulfide, polyimide and polytetrafluoroethylene.
5. The lithium metal battery electrode according to claim 1, wherein The polymer film has a thickness of 5 μm to 30 μm, excluding the height of the hemispherical protrusions.
6. The lithium metal battery electrode according to claim 1, wherein The conductive metal is one or more selected from the group consisting of Ni, Ti, Cu, Ag, Au, Pt, Fe, Co, Cr, W, Mo, Al, Mg, K, Na, Ca, Sr, Ba, Si, Ge, Sb, Pb, In and Zn.
7. The lithium metal battery electrode according to claim 1, wherein The thickness of the conductive metal layer is 0.5 μm to 10 μm.
8. The lithium metal battery electrode according to claim 1, wherein The lithium metal layer has a thickness of 5 μm to 50 μm. 9 . A lithium metal battery comprising the electrode for a lithium metal battery according to claim 1 .
10. A method for manufacturing an electrode for a lithium metal battery, the method comprising the following steps: preparing a polymer film having a pattern formed on one surface thereof, in which a plurality of hemispherical protrusions having a diameter of 10 μm to 40 μm are regularly arranged; forming a conductive metal layer by chemically plating a conductive metal precursor onto the pattern of the polymer film; and forming a lithium metal layer by electroplating lithium metal onto the conductive metal layer, Wherein, the height of the hemispherical protrusion is 5 μm to 40 μm.
11. The method for producing a lithium metal battery electrode according to claim 10, wherein: The conductive metal precursor is one or more selected from the group consisting of sulfates, halides, nitrates and hydroxides of Ni, Ti, Cu, Ag, Au, Pt, Fe, Co, Cr, W, Mo, Al, Mg, K, Na, Ca, Sr, Ba, Si, Ge, Sb, Pb, In or Zn.
12. The method for producing an electrode for a lithium metal battery according to claim 10, wherein: In the electroless plating step, one or more selected from the group consisting of glycine, formaldehyde, hydrazine, and citric acid are used as a reducing agent.
13. The method for producing a lithium metal battery electrode according to claim 10, wherein: The conductive metal layer is formed to a thickness of 0.5 μm to 10 μm.
14. The method for producing a lithium metal battery electrode according to claim 10, wherein: The lithium metal layer is formed to have a thickness of 5 μm to 50 μm.