Membrane electrode, preparation method thereof and fuel cell

By designing an optimized membrane electrode structure in the fuel cell, using carbon-laden nanometal catalysts and hydrophilic nanoparticles, the problem of inconsistent membrane electrode humidity in the fuel cell is solved, and the power density and performance of the fuel cell are improved.

CN118899486APending Publication Date: 2024-11-05SHANGHAI ELECTRICGROUP CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410937816.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the existing fuel cell technology, external humidification equipment increases system complexity and energy loss, resulting in inconsistent humidity in front and back of the membrane electrode flow field, reducing the power density of the fuel cell.

Method used

A membrane electrode is designed, including a proton exchange membrane layer, a first anode catalytic layer and a second anode catalytic layer, which is sandwiched between the proton exchange membrane layer and the second anode catalytic layer, using carbon-supported nanometers. Metal catalysts and hydrophilic nanoparticles optimize the structure and preparation method of membrane electrodes, eliminate the interface between the catalytic layers, and improve the self-humidification ability.

Benefits of technology

The power density of the membrane electrode is improved, interface pores and large-area cracks are eliminated, more uniform hydrothermal distribution is achieved, and the performance of the fuel cell is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899486A_ABST
    Figure CN118899486A_ABST
Patent Text Reader

Abstract

The invention discloses a membrane electrode, a preparation method thereof and a fuel cell, the membrane electrode comprises a proton exchange membrane layer, an anode catalyst layer and a cathode catalyst layer, the proton exchange membrane layer has a first side and a second side which are oppositely arranged, the anode catalyst layer is arranged on the first side, and the cathode catalyst layer is arranged on the second side; the anode catalyst layer comprises a first anode catalyst layer and a second anode catalyst layer, the first anode catalyst layer is arranged on the first side, the second anode catalyst layer is arranged on the first anode catalyst layer and on the first side, and the area of the first anode catalyst layer accounts for 10-40% of the effective active area of the membrane electrode; according to the membrane electrode structure, the self-humidifying capability of the inlet part of the membrane electrode is enhanced, and the power density of the membrane electrode is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a membrane electrode and a preparation method thereof, and a fuel cell. Background Art

[0002] Proton exchange membrane (PEM) fuel cells are becoming a new energy source for automotive drive and stationary applications because of their high power density under rapidly changing loads. During the electrochemical reaction of the fuel cell, water is generated, some of which permeates to the anode side of the membrane, and some of the generated water passes through the microporous layer and gas diffusion layer (GDL). This water is easily generated at the cathode and carried away by excess air, so the proton exchange membrane cannot be guaranteed to have a good wetting state, which reduces the ionic conductivity of the membrane electrode assembly (MEA).

[0003] In current fuel cell technology, external or internal humidification is required to additionally humidify the gas before entering the cell in order to maintain the water content of the Nafion membrane and the anode catalyst layer. The additional humidification equipment thus brought about increases the complexity and energy loss of the fuel cell system, increases the cost of the fuel cell, and reduces the power density of the fuel cell. In addition, due to the gas inlet and outlet in the flow field structure design inside the fuel cell stack, the gas flow rate before and after the flow channel is different, and thus the water content of the membrane electrode is also different, so that the membrane electrode using self-humidifying carbon or catalyst layer generally has a lower power density than conventional membrane electrodes, and it is more difficult to determine and manage due to the uneven water and heat distribution inside the battery. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the defect in the prior art that the humidity of the membrane electrode before and after the membrane electrode flow field in the external humidification stack is inconsistent, resulting in a decrease in the functional density of the fuel cell, and to provide a membrane electrode and its preparation method, and a fuel cell.

[0005] The present invention solves the above technical problems through the following technical solutions:

[0006] A membrane electrode, comprising a proton exchange membrane layer, an anode catalyst layer and a cathode catalyst layer, wherein the proton exchange membrane layer has a first side and a second side arranged opposite to each other, the anode catalyst layer is arranged on the first side, and the cathode catalyst layer is arranged on the second side;

[0007] The anode catalyst layer comprises a first anode catalyst layer and a second anode catalyst layer, the first anode catalyst layer is arranged on the first side, and the second anode catalyst layer is arranged on the first anode catalyst layer and on the first side, so that the first anode catalyst layer is sandwiched between the proton exchange membrane layer and the second anode catalyst layer;

[0008] The area of ​​the first anode catalyst layer accounts for 10-40% of the effective active area of ​​the membrane electrode, the effective active area of ​​the membrane electrode refers to the overlapping portion of the first anode catalyst layer, the second anode catalyst layer and the cathode catalyst layer, and the area of ​​the first anode catalyst layer refers to the projected area of ​​the first anode catalyst layer on the effective active area of ​​the membrane electrode;

[0009] The first anode catalyst layer comprises a first resin layer, a carbon-supported nano-metal catalyst and hydrophilic nano-particles, wherein the carbon-supported nano-metal catalyst and the hydrophilic nano-particles are both arranged in the first resin layer;

[0010] The second anode catalyst layer comprises a second resin layer and a carbon-supported nano-metal catalyst, wherein the carbon-supported nano-metal catalyst is disposed in the second resin layer;

[0011] The cathode catalyst layer comprises a third resin layer and a carbon-supported nano-metal catalyst, and the carbon-supported nano-metal catalyst is arranged in the third resin layer.

[0012] In the present invention, the area of ​​the first anode catalyst layer preferably accounts for 10-25% of the effective active area of ​​the membrane electrode, more preferably 15-23%, for example 16.3%.

[0013] In the present invention, preferably, the area of ​​the second anode catalyst layer accounts for 100% of the effective active area of ​​the membrane electrode. Preferably, the area of ​​the cathode catalyst layer accounts for 100% of the effective active area of ​​the membrane electrode.

[0014] In the present invention, the thickness of the first anode catalyst layer is preferably 1 to 5 μm, more preferably 1 to 3 μm.

[0015] In the present invention, in the first anode catalyst layer, the metal loading of the carbon-supported nano-metal catalyst on the first anode catalyst layer is preferably 0.01 to 0.2 mg / cm 2 , more preferably 0.01 to 0.1 mg / cm 2 , for example 0.02 mg / cm 2 The loading refers to the mass of metal per square centimeter on the first anode catalyst layer.

[0016] In the present invention, in the first anode catalyst layer, the loading of the hydrophilic nanoparticles on the first anode catalyst layer is preferably 3-4%, for example 3.3%, of the loading of the metal in the carbon-supported nanometal catalyst on the first anode catalyst layer. The loading refers to the mass of the hydrophilic nanoparticles per square centimeter on the first anode catalyst layer.

[0017] In the present invention, the thickness of the second anode catalyst layer is determined according to the metal loading in the carbon-supported nano-metal catalyst. In the second anode catalyst layer, the metal loading in the carbon-supported nano-metal catalyst on the second anode catalyst layer is preferably 0.03-0.07 mg / cm 2 , for example 0.03 mg / cm 2 The loading refers to the mass of metal per square centimeter on the second anode catalyst layer.

[0018] In the present invention, in the anode catalyst layer, the total loading of the metal in the carbon-supported nano-metal catalyst on the anode catalyst layer is preferably 0.05 to 0.1 mg / cm 2 , for example 0.05 mg / cm 2 .

[0019] In the present invention, the anode catalyst layer is a conventional layer of equal thickness in the art, that is, the total thickness of the anode catalyst layer in the area where the first anode catalyst layer is located is consistent with the total thickness of the anode catalyst layer in the remaining areas.

[0020] In the present invention, the hydrophilic nanoparticles are preferably sulfonated nano-titanium dioxide.

[0021] In the present invention, in the cathode catalyst layer, the metal loading of the carbon-supported nano-metal catalyst on the cathode catalyst layer is preferably 0.2-0.3 mg / cm 2 , e.g. 0.23 mg / cm 2 .

[0022] In the present invention, the carbon-supported nano-metal catalyst preferably comprises a carrier and metal particles supported on the surface of the carrier.

[0023] Wherein, the carrier is conventional in the art, preferably C.

[0024] The metal particles are preferably Pt, PtCo or PtCo(M), wherein M may be a transition metal element, preferably Fe, Ni, Mn, Ru, Rh or Pb.

[0025] The particle size of the carrier is preferably 45-55 nm. The particle size of the metal particles is preferably 2-7 nm.

[0026] In the present invention, the carbon-supported nano-metal catalyst is preferably one or more of a Pt / C catalyst, a PtCo / C catalyst and a PtCo(M) / C ternary alloy catalyst.

[0027] In the present invention, the metal content in the carbon-supported nano-metal catalyst is preferably 10-70%, more preferably 40-60%, for example 50%.

[0028] In the present invention, preferably, the resins of the first resin layer, the second resin layer and the third resin layer are all perfluorosulfonic acid ion exchange resins, such as perfluorosulfonic acid resin D2020.

[0029] In the present invention, preferably, the EW values ​​of the resins of the first resin layer, the second resin layer and the third resin layer are all 700 to 1200 g / mol, more preferably 800 to 1000 g / mol, where EW is ion exchange equivalent.

[0030] In the present invention, the proton exchange membrane is conventional in the art, preferably a reinforced perfluorosulfonic acid proton exchange membrane, such as an ePTFE reinforced perfluorosulfonic acid proton exchange membrane.

[0031] In the present invention, the membrane electrode may further include a gas diffusion layer, and the gas diffusion layer is respectively arranged on a side of the second anode catalyst layer away from the proton exchange membrane and a side of the cathode catalyst layer away from the proton exchange membrane.

[0032] The gas diffusion layer is conventional in the art, preferably carbon paper, and a microporous layer is arranged on the surface of the carbon paper. The microporous layers on both sides of the carbon paper are located on the side close to the second anode catalyst layer and the side close to the cathode catalyst layer.

[0033] The present invention also provides a method for preparing a membrane electrode, which comprises the following steps:

[0034] S1. Applying a first anode slurry on one side of a proton exchange membrane, wherein the area of ​​the first anode slurry accounts for 10 to 40% of the effective active area of ​​the membrane electrode; applying a second anode slurry on the first anode slurry and the proton exchange membrane while the first anode slurry is not dry;

[0035] The first anode slurry comprises a carbon-supported nano-metal catalyst, an ion exchange resin, hydrophilic nano-particles and a solvent;

[0036] The second anode slurry comprises a carbon-supported nano-metal catalyst, an ion exchange resin and a solvent;

[0037] S2. coating the cathode slurry on the other side of the proton exchange membrane;

[0038] The cathode slurry comprises a carbon-supported nano-metal catalyst, an ion exchange resin and a solvent;

[0039] The preparation order of step S1 and step S2 is not limited.

[0040] In the present invention, the carbon-supported nano-metal catalyst, the ion exchange resin, and the hydrophilic nano-particles are the same as described above, that is:

[0041] The carbon-supported nano-metal catalyst is preferably one or more of a Pt / C catalyst, a PtCo / C catalyst and a PtCo(M) / C ternary alloy catalyst.

[0042] The metal content in the carbon-supported nano-metal catalyst is preferably 10-70%, more preferably 40-60%, for example 50%.

[0043] The carbon-supported nano-metal catalyst preferably comprises a carrier and metal particles supported on the surface of the carrier, the particle size of the carrier is 45 to 55 nm, and the particle size of the metal particles is preferably 2 to 7 nm.

[0044] The ion exchange resin is preferably a perfluorosulfonic acid ion exchange resin, such as perfluorosulfonic acid resin D2020.

[0045] The EW value of the ion exchange resin is preferably 700 to 1200 mol / g, more preferably 800 to 1000 mol / g.

[0046] The hydrophilic nanoparticles are preferably sulfonated nano-titanium dioxide.

[0047] In the present invention, the solvent is preferably a mixture of deionized water and lower alcohols. The lower alcohol is preferably one or more of ethanol, n-propanol, isopropanol, isobutanol and ethylene glycol, more preferably one or more of ethanol, n-propanol, isopropanol and isobutanol, such as ethanol.

[0048] In the present invention, in step S1, in the first anode slurry, the carbon-supported nano-metal catalyst preferably accounts for 7-10% by mass of the first anode slurry, more preferably 7.5-8.5%, for example 8.1%.

[0049] In the first anode slurry, the mass of the ion exchange resin preferably accounts for 14-32% of the mass of the first anode slurry, more preferably 17.5-30.6%, for example 24.3%.

[0050] In the first anode slurry, the mass of the hydrophilic nanoparticles preferably accounts for 0.08-0.2% of the mass of the first anode slurry, and more preferably 0.1-0.15%, for example 0.13%.

[0051] In the first anode slurry, the mass of the solvent preferably accounts for 53-80% of the mass of the first anode slurry, more preferably 60-70%, for example 67.4%.

[0052] When the solvent is a mixture of deionized water and lower alcohol, the mass of the lower alcohol is preferably 13-27% of the mass of the first anode slurry, more preferably 13.5-22.5%, such as 20.2%. The mass of the deionized water is preferably 40-54%, more preferably 45-51%, such as 47.2% of the mass of the first anode slurry.

[0053] In the present invention, in step S1, the method for preparing the first anode slurry preferably comprises: mixing the carbon-supported nano-metal catalyst, the ion exchange resin, the hydrophilic nano-particles and the solvent to obtain the first anode slurry.

[0054] The method for preparing the first anode slurry preferably comprises the following steps: mixing the carbon-supported nano-metal catalyst with deionized water once, adding the ion exchange resin and mixing again, adding the solvent and ball milling, and then adding the hydrophilic nanoparticles and continuing ball milling to obtain the first anode slurry.

[0055] The methods of the first mixing and the second mixing are preferably ultrasonic mixing. The time of the first mixing and the second mixing is preferably 1 to 20 minutes, more preferably 2 to 10 minutes, for example 2 minutes.

[0056] The end point of the remixing is preferably when there is no obvious agglomerate in the solution.

[0057] The ball milling time after adding the solvent is preferably 10 to 180 minutes, more preferably 20 to 120 minutes, for example 30 minutes.

[0058] The time for continuing ball milling after adding the hydrophilic nanoparticles is preferably 5 to 30 minutes, more preferably 10 to 20 minutes, for example 10 minutes.

[0059] After adding the hydrophilic nanoparticles and continuing the ball milling, a degassing step may be further included.

[0060] In the present invention, in step S1, in the second anode slurry, the mass ratio of the carbon-supported nano-metal catalyst to the second anode slurry is preferably 7-10%, more preferably 7.5-8.5%, for example 8.1%.

[0061] In the second anode slurry, the mass of the ion exchange resin preferably accounts for 14-32% of the mass of the second anode slurry, more preferably 17.5-30.6%, for example 24.3%.

[0062] In the second anode slurry, the mass of the solvent accounts for preferably 53-80% of the mass of the first anode slurry, more preferably 60-70%, for example 67.6%.

[0063] When the solvent is a mixture of deionized water and lower alcohol, the mass of the lower alcohol is preferably 13-27% of the mass of the second anode slurry, more preferably 13.5-22.5%, such as 20.3%. The mass of the deionized water is preferably 40-54%, more preferably 45-51%, such as 47.3% of the mass of the second anode slurry.

[0064] In the present invention, in step S1, the method for preparing the second anode slurry preferably comprises: mixing the carbon-supported nano-metal catalyst, the ion exchange resin and the solvent to obtain the second anode slurry.

[0065] The method for preparing the second anode slurry preferably comprises the following steps: mixing the carbon-supported nano-metal catalyst with deionized water once, adding the ion exchange resin and mixing again, adding the solvent and ball milling to obtain the second anode slurry.

[0066] The methods of the first mixing and the second mixing are preferably ultrasonic mixing. The time of the first mixing and the second mixing is preferably 1 to 10 minutes, more preferably 2 to 5 minutes, for example 2 minutes.

[0067] The end point of the remixing is preferably when there is no obvious agglomerate in the solution.

[0068] The ball milling time after adding the solvent is preferably 10 to 180 minutes, more preferably 20 to 50 minutes, for example 30 minutes.

[0069] After adding the solvent and ball milling, a degassing step may be further included.

[0070] In the present invention, in step S2, in the cathode slurry, the carbon-supported nano-metal catalyst preferably accounts for 4-12% by mass of the cathode slurry, more preferably 7-10%, for example 8.6%.

[0071] In the cathode slurry, the mass of the ion exchange resin preferably accounts for 8.5-27% of the mass of the cathode slurry, more preferably 15-22%, for example 19.4%.

[0072] In the first anode slurry, the mass of the solvent accounts for preferably 53-80% of the mass of the cathode slurry, more preferably 70-80%, for example 71.9%.

[0073] When the solvent is a mixture of deionized water and a lower alcohol, the mass of the solvent accounts for preferably 13-27% of the mass of the cathode slurry, more preferably 13.5-22.5%, such as 21.6%. The mass of the deionized water accounts for preferably 40-54% of the mass of the cathode slurry, more preferably 45-51%, such as 50.3%.

[0074] In the present invention, in step S2, the method for preparing the cathode slurry preferably comprises: mixing the carbon-supported nano-metal catalyst, ion exchange resin and solvent to obtain the cathode slurry.

[0075] The method for preparing the cathode slurry preferably comprises the following steps: mixing the carbon-supported nano-metal catalyst with deionized water once, adding the ion exchange resin and mixing again, adding the solvent and ball milling to obtain the cathode slurry.

[0076] The methods of the first mixing and the second mixing are preferably ultrasonic mixing. The time of the first mixing and the second mixing is preferably 1 to 10 minutes, more preferably 2 to 5 minutes, for example 2 minutes.

[0077] The end point of the remixing is preferably when there is no obvious agglomerate in the solution.

[0078] The ball milling time after adding the solvent is preferably 10 to 180 minutes, more preferably 20 to 50 minutes, for example 30 minutes.

[0079] After adding the solvent and ball milling, a degassing step may be further included.

[0080] In the present invention, the coating interval time of the first anode slurry and the second anode slurry is preferably within 1 to 2 minutes.

[0081] In the present invention, in step S1, the coating method of the first anode slurry is preferably slit coating.

[0082] The slit gap of the slit coating is preferably 50-200 μm, more preferably 100-150 μm, for example 100 μm.

[0083] The die gap of the slot coating is preferably 50-150 μm, more preferably 60-100 μm, for example 70 μm.

[0084] The feeding speed of the slit coating is preferably 2-10 mL / min, more preferably 2-6 mL / min, for example 4 mL / min.

[0085] The substrate travel speed of the slit coating is preferably 0.3-3 m / min, more preferably 0.5-1 m / min, for example 0.8 m / min.

[0086] The drying temperature of the slit coating is preferably 40-120°C, more preferably 60-80°C, for example 80°C.

[0087] In the present invention, in step S1, the area of ​​the first anode slurry preferably accounts for 10-25% of the effective active area of ​​the membrane electrode, and more preferably 15-23%, for example 16.3%.

[0088] In the present invention, in step S1, the coating thickness of the first anode slurry is preferably 1 to 5 μm, more preferably 1 to 3 μm.

[0089] In the present invention, in step S1, when the first anode slurry is not dry, the second anode slurry is generally applied immediately after the first anode slurry is applied, so that no interface pores appear between the first anode slurry layer and the second anode slurry layer.

[0090] In the present invention, in step S1, the coating method of the second anode slurry is preferably slit coating.

[0091] The slit gap of the slit coating is preferably 50 to 200 μm, more preferably 100~150um, for example 100μm.

[0092] The die gap of the slot coating is preferably 50-150 μm, more preferably 60-100 μm, for example 70 μm.

[0093] The feeding speed of the slit coating is preferably 2 to 12 mL / min. The feeding speed of the slit coating is preferably a two-stage feeding speed, wherein the feeding speed of the first stage is 2 to 6 mL / min, the feeding area of ​​the first stage is the coating area of ​​the first anode slurry, and the feeding speed of the second stage is 8 to 12 mL / min, for example, 10 mL / min, and the feeding area of ​​the second stage is other areas except the coating area of ​​the first anode slurry.

[0094] The substrate travel speed of the slit coating is preferably 0.3-3 m / min, more preferably 0.5-1.5 m / min, for example 1 m / min.

[0095] The drying temperature of the slit coating is preferably 40-120°C, more preferably 60-80°C, for example 80°C.

[0096] In the present invention, in step S1, the coating thickness of the second anode slurry is determined according to the metal loading of the carbon-supported nano-metal catalyst in the coating area of ​​the second anode slurry. The total loading of the metal in the carbon-supported nano-metal catalyst in the coating area of ​​the second anode slurry is preferably 0.05-0.1 mg / cm 2 .

[0097] In the present invention, in step S1, the first anode slurry and the second anode slurry can be directly coated sequentially on one side of the proton exchange membrane, or the first anode slurry and the second anode slurry can be first coated sequentially on the surface of the transfer membrane, and then transferred to one side of the proton exchange membrane by hot pressing.

[0098] In the present invention, in step S2, the cathode slurry coating method preferably includes: applying the cathode slurry on the surface of the transfer membrane by slit coating, and then transferring it to the other side of the proton exchange membrane by hot pressing.

[0099] Wherein, the slit gap of the slit coating is preferably 100-250 μm, for example, 200 μm.

[0100] The die gap of the slot coating is preferably 200-300 μm, for example 250 μm.

[0101] The feeding speed of the slot coating is preferably 10-20 mL / min, for example 18 mL / min.

[0102] The substrate travel speed of the slit coating is preferably 0.3-1 m / min, for example 0.4 m / min.

[0103] The drying temperature of the slit coating is preferably 40-120°C, for example 80°C.

[0104] The coating thickness of the cathode slurry is determined according to the metal loading of the carbon-supported nano-metal catalyst in the coating area of ​​the cathode slurry. The total loading of the metal in the carbon-supported nano-metal catalyst in the coating area of ​​the cathode slurry is preferably 0.2-0.3 mg / cm 2 , for example 0.23 mg / cm 2 .

[0105] The temperature of the hot pressing method is preferably 130-180°C, more preferably 144-165°C, for example 160°C.

[0106] The heat pressing time is preferably 80 to 240 seconds, more preferably 100 to 180 seconds, such as 150 seconds.

[0107] In the present invention, in step S2, the cathode slurry can be directly coated on the other side of the proton exchange membrane.

[0108] The present invention also provides a membrane electrode prepared by the above-mentioned membrane electrode preparation method.

[0109] The present invention also provides a fuel cell, which comprises the membrane electrode, wherein the first anode catalyst layer is preferably located at the hydrogen inlet and outlet of the fuel cell stack.

[0110] The positive and progressive effects of the present invention are:

[0111] (1) The membrane electrode structure of the present invention enhances the self-humidification capability of the membrane electrode inlet portion and improves the power density of the membrane electrode.

[0112] (2) The preparation method of the present invention eliminates the interface between the first catalytic layer and the second anode catalytic layer, improves consistency, and eliminates large-area cracking that is prone to occur during double-layer coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0113] Figure 1 It is a schematic structural diagram of the membrane electrode with enhanced humidification at the gas inlet of the present invention.

[0114] Figure 2 2 are polarization curves of the embodiments and comparative examples.

[0115] Reference numerals:

[0116] Proton exchange membrane layer 1

[0117] Anode catalyst layer 2

[0118] The first anode catalyst layer 21

[0119] The second anode catalyst layer 22

[0120] Cathode catalyst layer 3 DETAILED DESCRIPTION

[0121] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. It should be noted that the "first, second" in the "first anode catalyst layer", "second anode catalyst layer", "first resin layer", "second resin layer" and "third resin" in the present invention is only for the convenience of describing the present invention, and does not indicate or imply the order of the devices or elements referred to, and therefore cannot be understood as limiting the present invention.

[0122] The carbon-supported nano-metal catalyst Pt / C in the following embodiments is commercially available, and the manufacturer and model are: umicro pt-0550.

[0123] Example 1

[0124] 1) Preparation of cathode slurry:

[0125] Take 1.2g of Pt / C catalyst (Pt content 50%), add 7g of deionized water, and mix by ultrasonic for 2min until the catalyst and deionized water are completely mixed;

[0126] Add 2.7g of perfluorosulfonic acid ion exchange resin solution D2020 and sonicate until no obvious catalyst agglomerates remain;

[0127] Add 3.0 g of ethanol and ball mill for 30 min;

[0128] The slurry after ball milling is taken out and degassed to obtain the final cathode slurry.

[0129] 2) Preparation of anode slurry 1:

[0130] Take 1.2g of Pt / C catalyst (Pt content 50%), add 7g of deionized water, and mix by ultrasonic for 2min until the catalyst and deionized water are completely mixed;

[0131] Add 3.6g of perfluorosulfonic acid ion exchange resin solution D2020 and sonicate until no obvious catalyst agglomerates are formed;

[0132] Add 3.0 g of ethanol and ball mill for 30 min;

[0133] Add 0.02 g of sulfonated nano-titanium dioxide and continue ball milling for 10 min;

[0134] The preparation method of sulfonated nano titanium dioxide is as follows: 0.5g TiO2 particles, 5ml methanol, and 10ml 2mol / L dilute sulfuric acid are added to three flasks in sequence, ultrasonically shaken for 2 hours, stirred continuously under N2 atmosphere, and heated at 80°C for 12 hours. After the reaction is completed, the solution is washed to neutrality and dried to obtain sulfonated titanium dioxide.

[0135] The slurry after ball milling is taken out and degassed to obtain the final anode slurry 1.

[0136] 3) Preparation of anode slurry 2:

[0137] Take 1.2g of Pt / C catalyst (Pt content 50%), add 7g of deionized water, and mix by ultrasonic for 2min until the catalyst and water are completely mixed;

[0138] Add 3.6g of perfluorosulfonic acid ion exchange resin solution D2020 and sonicate until no obvious catalyst agglomerates are formed;

[0139] Add 3.0 g of ethanol and ball mill for 30 min;

[0140] The slurry after ball milling is taken out and degassed to obtain the final anode slurry 2.

[0141] 4) Coating

[0142] The anode slurry was coated on one side of the ePTFE-enhanced perfluorosulfonic acid proton exchange membrane (purchased from Dongyue Company) by slit coating. The membrane was 5 cm long, 9.8 cm wide, and 1 μm thick. The average precious metal loading was 0.02 mg / cm 2 The average loading of hydrophilic nanoparticles is 3.3% of the precious metal loading. The total effective active area of ​​the proton exchange membrane is 300 cm 2 , the slit gap of slit coating is 100 μm, the die gap of slit coating is 70 μm, the feed speed of slit coating is 4 mL / min, the substrate travel speed of slit coating is 0.8 m / min, and the drying temperature of slit coating is 80°C.

[0143] Apply anode slurry 2 within 1 to 2 minutes after anode slurry 1 is applied to 300 cm 2 The total effective active area (two-stage method to control the liquid output) was finally obtained, and the anode noble metal loading of the membrane electrode was 0.05 mg / cm 2 The slit gap of the slit coating is 100 μm, the die gap of the slit coating is 70 μm, the feeding speed of the slit coating is 6 mL / min for the first 5 cm, the subsequent feeding speed is 10 mL / min, the substrate travel speed of the slit coating is 1 m / min, and the drying temperature of the slit coating is 80°C. Finally, the anode catalyst layer is obtained.

[0144] The cathode slurry was coated on the transfer film surface by slit coating, and the cathode precious metal loading was 0.23 mg / cm 2 , the cathode slurry coating area is 300cm 2 , and transferred to the other side of the proton exchange membrane by hot pressing. The hot pressing temperature during the transfer was 160°C, and the hot pressing time during the transfer was 150s to obtain a cathode catalyst layer.

[0145] Carbon paper is composited on the surface of the anode catalyst layer and the cathode catalyst layer by hot pressing to form a gas diffusion layer, wherein the surface of the carbon paper is coated with a microporous layer, and the microporous layer on the carbon paper on both sides is located on the side close to the second anode catalyst layer and the cathode catalyst layer.

[0146] The membrane electrode of this embodiment includes a proton exchange membrane layer 1, an anode catalyst layer 2, a cathode catalyst layer 3 and a gas diffusion layer. The proton exchange membrane layer 1 has a first side and a second side that are arranged opposite to each other. The anode catalyst layer 2 is arranged on the first side, and the cathode catalyst layer 3 is arranged on the second side. The anode catalyst layer 2 includes a first anode catalyst layer 21 and a second anode catalyst layer 22. The first anode catalyst layer 21 is arranged on the first side, and the second anode catalyst layer 22 is arranged on the first anode catalyst layer 21 and on the first side, so that the first anode catalyst layer 21 is sandwiched between the proton exchange membrane layer 1 and the second anode catalyst layer 22. Figure 1 As shown. The first anode catalyst layer 21 is 5 cm long and 9.8 cm wide, accounting for 16.3% of the effective active area of ​​the membrane electrode; the first anode catalyst layer 21 includes a first resin layer, a carbon-supported nanometal catalyst and hydrophilic nanoparticles, and the carbon-supported nanometal catalyst and the hydrophilic nanoparticles are both arranged in the first resin layer; the second anode catalyst layer 22 includes a second resin layer and a carbon-supported nanometal catalyst, and the carbon-supported nanometal catalyst is arranged in the second resin layer; the cathode catalyst layer 3 includes a third resin layer and a carbon-supported nanometal catalyst, and the carbon-supported nanometal catalyst is arranged in the third resin layer. The gas diffusion layer is a carbon paper coated with a microporous layer on the surface, and the gas diffusion layer is respectively arranged on the side of the second anode catalyst layer 22 away from the proton exchange membrane layer 1 and the side of the cathode catalyst layer 3 away from the proton exchange membrane layer 1, and the microporous layers on both sides are located on the side close to the second anode catalyst layer 22 and the cathode catalyst layer 3.

[0147] Comparative Example 1

[0148] In this comparative example, except that the coating length of anode slurry 1 is 0 cm and the initial feeding rate of anode slurry 2 is 6 mL / min and the coating length is 0 cm, the other raw materials, steps and process conditions are the same as those in Example 1.

[0149] Comparative Example 2

[0150] The coating length of the anode slurry is 15 cm, and the coating area is 15×9.8=147 cm 2 , accounting for 49% of the entire active area, the initial feed rate of anode slurry 2 was 6 mL / min and the coating length was 15 cm. The other raw materials, steps and process conditions were the same as those in Example 1.

[0151] Comparative Example 3

[0152] The coating length of the anode slurry is 30 cm, and the coating area is 30×9.8=294 cm 2 , accounting for 98% of the entire active area, the initial feed rate of anode slurry 2 is 6mL / min and the coating length is 30cm. The other raw materials, steps and process conditions are the same as those in Example 1.

[0153] Effect Example

[0154] Polarization curve tests were performed on the membrane electrodes of the above embodiments and comparative examples. The test conditions of this embodiment are as follows: the battery temperature is 80°C, the anode and cathode gases are hydrogen and air respectively, the anode and cathode flow rates are both controlled by excess coefficients, the coefficients are both 2, the anode and cathode humidity is 50%, and the anode and cathode pressures are 150 kPa.

[0155] Figure 2 1 and 2 are polarization curves of the membrane electrodes of Example 1 and Comparative Examples 1 to 3. Table 1 is part of the data in the polarization curves.

[0156] Table 1 Polarization curve data

[0157]

[0158] Combination Figure 2 As can be seen from Table 1, at the same current density, the voltage value of Example 1 is higher than that of Comparative Example 2 and Comparative Example 3. As the current density increases, the voltage value decrease rate of Comparative Example 2 and Comparative Example 3 increases. Although the voltages of Example 1 and Comparative Example 1 are close at high current density, they are much lower at low current density (less than 1500 mA / cm 2 The voltage value of Example 1 is obviously higher than that of Comparative Example 1. Accordingly, the power density of Example 1 is higher than that of Comparative Example.

Claims

1. A membrane electrode, It is characterized in that It comprises a proton exchange membrane layer, an anode catalyst layer and a cathode catalyst layer, wherein the proton exchange membrane layer has a first side and a second side which are arranged opposite to each other, the anode catalyst layer is arranged on the first side, and the cathode catalyst layer is arranged on the second side; The anode catalyst layer comprises a first anode catalyst layer and a second anode catalyst layer, the first anode catalyst layer is arranged on the first side, and the second anode catalyst layer is arranged on the first anode catalyst layer and on the first side, so that the first anode catalyst layer is sandwiched between the proton exchange membrane layer and the second anode catalyst layer; The area of ​​the first anode catalyst layer accounts for 10-40% of the effective active area of ​​the membrane electrode, the effective active area of ​​the membrane electrode refers to the overlapping portion of the first anode catalyst layer, the second anode catalyst layer and the cathode catalyst layer, and the area of ​​the first anode catalyst layer refers to the projected area of ​​the first anode catalyst layer on the effective active area of ​​the membrane electrode; The first anode catalyst layer comprises a first resin layer, a carbon-supported nano-metal catalyst and hydrophilic nano-particles, wherein the carbon-supported nano-metal catalyst and the hydrophilic nano-particles are both arranged in the first resin layer; The second anode catalyst layer comprises a second resin layer and a carbon-supported nano-metal catalyst, wherein the carbon-supported nano-metal catalyst is disposed in the second resin layer; The cathode catalyst layer comprises a third resin layer and a carbon-supported nano-metal catalyst, and the carbon-supported nano-metal catalyst is arranged in the third resin layer.

2. The membrane electrode according to claim 1, It is characterized in that The area of ​​the first anode catalyst layer accounts for 10-25% of the effective active area of ​​the membrane electrode, preferably 15-23%, for example 16.3%; And / or, the thickness of the first anode catalyst layer is 1 to 5 μm, preferably 1 to 3 μm; And / or, in the first anode catalyst layer, the metal loading of the carbon-supported nano-metal catalyst on the first anode catalyst layer is 0.01-0.2 mg / cm 2 , preferably 0.01 to 0.1 mg / cm 2 , for example 0.02 mg / cm 2 , the loading refers to the mass of metal on the first anode catalyst layer per square centimeter; And / or, in the first anode catalyst layer, the loading of the hydrophilic nanoparticles on the first anode catalyst layer is 3-4%, for example 3.3%, of the loading of the metal in the carbon-supported nanometal catalyst on the first anode catalyst layer, wherein the loading refers to the mass of the hydrophilic nanoparticles per square centimeter of the first anode catalyst layer; And / or, in the second anode catalyst layer, the metal loading of the carbon-supported nano-metal catalyst on the second anode catalyst layer is 0.03-0.07 mg / cm 2 , for example 0.03 mg / cm 2 , the loading refers to the mass of metal on the second anode catalyst layer per square centimeter; And / or, in the anode catalyst layer, the total loading of the metal in the carbon-supported nano-metal catalyst on the anode catalyst layer is 0.05-0.1 mg / cm 2 , for example 0.05 mg / cm 2 ; And / or, in the cathode catalyst layer, the metal in the carbon-supported nano-metal catalyst has a loading amount of 0.2 to 0.3 mg / cm 2 , e.g. 0.23 mg / cm 2 ; And / or, the hydrophilic nanoparticles are sulfonated nano-titanium dioxide; And / or, the carbon-supported nanometal catalyst is one or more of a Pt / C catalyst, a PtCo / C catalyst and a PtCo(M) / C ternary alloy catalyst, wherein M is a transition metal element, preferably Fe, Ni, Mn, Ru, Rh or Pb; And / or, the metal content in the carbon-supported nano-metal catalyst is 10-70%, preferably 40-60%, for example 50%; And / or, the carbon-supported nano-metal catalyst comprises a carrier and metal particles supported on the surface of the carrier, the carrier particle size is 45 to 55 nm, preferably, the metal particles have a particle size of 2 to 7 nm; And / or, the resins of the first resin layer, the second resin layer and the third resin layer are all perfluorosulfonic acid ion exchange resins, preferably perfluorosulfonic acid resin D2020; and / or the EW values ​​of the resins of the first resin layer, the second resin layer and the third resin layer are all 700 to 1200 g / mol, preferably 800 to 1000 g / mol; And / or, the proton exchange membrane is an enhanced perfluorosulfonic acid proton exchange membrane, such as an ePTFE enhanced perfluorosulfonic acid proton exchange membrane; And / or, the membrane electrode also includes a gas diffusion layer, which is respectively arranged on the side of the second anode catalyst layer away from the proton exchange membrane and the side of the cathode catalyst layer away from the proton exchange membrane; the gas diffusion layer is preferably carbon paper, and a microporous layer is arranged on the surface of the carbon paper, and the microporous layers on the carbon paper on both sides are located on the side close to the second anode catalyst layer and the side close to the cathode catalyst layer.

3. A method for preparing a membrane electrode, It is characterized in that It includes the following steps: S1. coating a first anode slurry on a first side of a proton exchange membrane, wherein the coating area of ​​the first anode slurry accounts for 10 to 40% of the effective active area of ​​the membrane electrode; coating a second anode slurry on the first anode slurry and the proton exchange membrane while the first anode slurry is not dry; The first anode slurry comprises a carbon-supported nano-metal catalyst, an ion exchange resin, hydrophilic nano-particles and a solvent; The second anode slurry comprises a carbon-supported nano-metal catalyst, an ion exchange resin and a solvent; S2. coating the cathode slurry on the second side of the proton exchange membrane; The cathode slurry comprises a carbon-supported nano-metal catalyst, an ion exchange resin and a solvent; The preparation order of step S1 and step S2 is not limited.

4. The method for preparing a membrane electrode according to claim 3, It is characterized in that The carbon-supported nanometal catalyst is one or more of a Pt / C catalyst, a PtCo / C catalyst and a PtCo(M) / C ternary alloy catalyst, wherein M is a transition metal element, and M is preferably Fe, Ni, Mn, Ru, Rh or Pb; And / or, the metal content in the carbon-supported nano-metal catalyst is 10-70%, preferably 40-60%, for example 50%; And / or, the carbon-supported nano-metal catalyst comprises a carrier and metal particles supported on the surface of the carrier, the carrier particle size is 45 to 55 nm, preferably, the metal particles have a particle size of 2 to 7 nm; And / or, the hydrophilic nanoparticles are sulfonated nano-titanium dioxide; And / or, the ion exchange resin is a perfluorosulfonic acid ion exchange resin, preferably a perfluorosulfonic acid resin D2020; and / or, the EW value of the ion exchange resin is 700 to 1200 g / mol, preferably 800 to 1000 g / mol; And / or, the proton exchange membrane is an enhanced perfluorosulfonic acid proton exchange membrane, such as an ePTFE enhanced perfluorosulfonic acid proton exchange membrane; And / or, the solvent is a mixture of deionized water and a lower alcohol, and the lower alcohol is preferably one or more of ethanol, n-propanol, isopropanol, isobutanol and ethylene glycol; And / or, in the first anode slurry, the mass ratio of the carbon-supported nano-metal catalyst to the first anode slurry is 7-10%, preferably 7.5-8.5%, for example 8.1%; And / or, in the first anode slurry, the mass ratio of the ion exchange resin to the mass ratio of the first anode slurry is 14-32%, preferably 17.5-30.6%, for example 24.3%; And / or, in the first anode slurry, the mass ratio of the hydrophilic nanoparticles to the mass ratio of the first anode slurry is 0.08-0.2%, preferably 0.1-0.15%, for example 0.13%; And / or, in the first anode slurry, the mass ratio of the solvent to the mass ratio of the first anode slurry is 53-80%, preferably 60-70%, for example 67.4%; When the solvent is a mixture of deionized water and a lower alcohol, the mass ratio of the lower alcohol to the mass ratio of the first anode slurry is 13-27%, preferably 13.5-22.5%, for example 20.2%, and the mass ratio of the deionized water to the mass ratio of the first anode slurry is 40-54%, preferably 45-51%, for example 47.2%; And / or, the coating interval time of the first anode slurry and the second anode slurry is preferably within 1 to 2 minutes; And / or, the preparation method of the first anode slurry comprises: mixing the carbon-supported nano-metal catalyst, the ion exchange resin, the hydrophilic nano-particles and the solvent to obtain the first anode slurry, preferably comprising the following steps: mixing the carbon-supported nano-metal catalyst with deionized water once, adding the ion exchange resin to mix again, adding the solvent to ball mill, and then adding the hydrophilic nano-particles to continue ball milling to obtain the first anode slurry; wherein, The methods of the first mixing and the second mixing are preferably ultrasonic mixing; The time for the first mixing and the second mixing is preferably 1 to 20 minutes, more preferably 2 to 10 minutes; The ball milling time after adding the solvent is preferably 10 to 180 minutes, more preferably 20 to 120 minutes, for example 30 minutes; The time for continuing ball milling after adding the hydrophilic nanoparticles is preferably 5 to 30 minutes, more preferably 10 to 20 minutes.

5. The method for preparing a membrane electrode according to claim 3, It is characterized in that In the second anode slurry, the mass ratio of the carbon-supported nano-metal catalyst to the second anode slurry is 7-10%, preferably 7.5-8.5%, for example 8.1%; And / or, in the second anode slurry, the mass ratio of the ion exchange resin to the mass ratio of the second anode slurry is 14-32%, preferably 17.5-30.6%, for example 24.3%; and / or, in the second anode slurry, the mass ratio of the solvent to the mass ratio of the first anode slurry is 53-80%, preferably 60-70%, for example 67.6%; When the solvent is a mixture of deionized water and a lower alcohol, the mass ratio of the lower alcohol to the mass ratio of the second anode slurry is 13-27%, preferably 13.5-22.5%, for example 20.3%; the mass ratio of the deionized water to the mass ratio of the second anode slurry is 40-54%, preferably 45-51%, for example 47.3%; And / or, the preparation method of the second anode slurry comprises: mixing the carbon-supported nano-metal catalyst, the ion exchange resin and the solvent to obtain the second anode slurry, preferably comprising the following steps: mixing the carbon-supported nano-metal catalyst with deionized water once, adding the ion exchange resin to mix again, adding the solvent to ball mill to obtain the second anode slurry, wherein, The methods of the first mixing and the second mixing are preferably ultrasonic mixing; The time for the first mixing and the second mixing is preferably 1 to 10 minutes, more preferably 2 to 5 minutes, for example 2 minutes; The ball milling time after adding the solvent is preferably 10 to 180 minutes, more preferably 20 to 50 minutes, for example 30 minutes.

6. The method for preparing a membrane electrode according to claim 3, It is characterized in that In the cathode slurry, the mass ratio of the carbon-supported nano-metal catalyst to the cathode slurry is 4-12%, preferably 7-10%, for example 8.6%; And / or, in the cathode slurry, the mass ratio of the ion exchange resin to the mass ratio of the cathode slurry is 8.5-27%, preferably 15-22%, for example 19.4%; And / or, in the first anode slurry, the mass ratio of the solvent to the mass ratio of the cathode slurry is 53-80%, preferably 70-80%, for example 71.9%; When the solvent is a mixture of deionized water and a lower alcohol, the mass ratio of the solvent to the mass ratio of the cathode slurry is 13-27%, preferably 13.5-22.5%, for example 21.6%; the mass ratio of the deionized water to the mass ratio of the cathode slurry is 40-54%, preferably 45-51%, for example 50.3%; And / or, the preparation method of the cathode slurry comprises: mixing a carbon-supported nano-metal catalyst, an ion exchange resin and a solvent to obtain a cathode slurry, preferably comprising the following steps: mixing the carbon-supported nano-metal catalyst with deionized water once, adding the ion exchange resin to mix again, adding the solvent to ball mill to obtain a cathode slurry, wherein, The methods of the first mixing and the second mixing are preferably ultrasonic mixing; The time for the first mixing and the second mixing is preferably 1 to 10 minutes, more preferably 2 to 5 minutes, for example 2 minutes; The ball milling time after adding the solvent is preferably 10 to 180 minutes, more preferably 20 to 50 minutes, for example 30 minutes.

7. The method for preparing a membrane electrode according to claim 3, It is characterized in that The coating method of the first anode slurry is slot coating, wherein: The slit gap of the slit coating is preferably 50-200 μm, more preferably 100-150 μm, for example 100 μm; The die gap of the slit coating is preferably 50-150 μm, more preferably 60-100 μm, for example 70 μm; The feeding speed of the slit coating is preferably 2 to 10 mL / min, more preferably 2 to 6 mL / min, for example 4 mL / min; The substrate speed of the slit coating is preferably 0.3-3 m / min, more preferably 0.5-1 m / min, for example 0.8 m / min; The drying temperature of the slit coating is preferably 40-120°C, more preferably 60-80°C, for example 80°C; And / or, the coating method of the second anode slurry is slit coating, wherein, The slit gap of the slit coating is preferably 50-200 μm, more preferably 100-150 μm, for example 100 μm; The die gap of the slit coating is preferably 50-150 μm, more preferably 60-100 μm, for example 70 μm; The feeding speed of the slit coating is preferably a two-stage feeding speed, wherein the feeding speed of the first stage is 2-6 mL / min, the feeding area of ​​the first stage is the coating area of ​​the first anode slurry, and the feeding speed of the second stage is 8-12 mL / min, for example, 10 mL / min, and the feeding area of ​​the second stage is other areas except the coating area of ​​the first anode slurry; The substrate speed of the slit coating is preferably 0.3-3 m / min, more preferably 0.5-1.5 m / min, for example 1 m / min; The drying temperature of the slit coating is preferably 40-120°C, more preferably 60-80°C, for example 80°C.

8. The method for preparing a membrane electrode according to claim 3, It is characterized in that The cathode slurry coating method comprises: applying the cathode slurry on the surface of the transfer membrane by slit coating, and then transferring the cathode slurry to the other side of the proton exchange membrane by hot pressing, wherein: The slit gap of the slit coating is preferably 100 to 250 μm, for example 200 μm; The die gap of the slot coating is preferably 200-300 μm, for example 250 μm; The feeding speed of the slit coating is preferably 10 to 20 mL / min, for example 18 mL / min; The substrate travel speed of the slit coating is preferably 0.3-1 m / min, for example 0.4 m / min; The drying temperature of the slit coating is preferably 40 to 120° C., for example 80° C.; The temperature of the hot pressing method is preferably 130-180°C, more preferably 144-165°C, for example 160°C; The heat pressing time is preferably 80 to 240 seconds, more preferably 100 to 180 seconds, for example 150 seconds.

9. A membrane electrode prepared by the method for preparing a membrane electrode as claimed in any one of claims 3 to 8.

10. A fuel cell, It is characterized in that It comprises the membrane electrode as claimed in any one of claims 1, 2 and 9, wherein the first anode catalyst layer is preferably located at the hydrogen inlet of the fuel cell stack.